Dry-method electrode binder as well as preparation method and application thereof

By using surface-modified polyvinylidene fluoride and carbon material coatings in the dry electrode adhesive, the problems of instability and environmental pollution of the dry electrode adhesive are solved, and the circulation of lithium-ion batteries is improved Performance and electrochemical properties.

CN119060656APending Publication Date: 2024-12-03ZHEJIANG LIWINON ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411345012.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing dry electrode binder is unstable during the preparation process, resulting in unstable electrode structure, affecting the cycle stability and battery capacity of lithium-ion batteries. In addition, the use of organic solvents in the dry process has problems with cost and environmental pollution.

Method used

Using a dry electrode adhesive including surface-modified polyvinylidene fluoride, gelatin, polytetrafluoroethylene and carbon material clad layer, the modified adhesive is treated by plasma and ball milled with carbon material. A cladding layer is formed to improve the hydrophilicity and adhesion of the adhesive.

Benefits of technology

The cycling performance of the dry-process battery and the first-time Coulomb efficiency are improved, the irreversible consumption of the binder during charging and discharging is suppressed, the problem of high impedance of the electrode sheet is reduced, and the stability and electrochemical performance of the electrode are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005060719710000071
    Figure BDA0005060719710000071
  • Figure BDA0005060719710000072
    Figure BDA0005060719710000072
  • Figure BDA0005060719710000081
    Figure BDA0005060719710000081
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium ion batteries, and particularly relates to a dry-method electrode binder and a preparation method and application thereof, and the dry-method electrode binder comprises a bonding layer and a coating layer coating the surface of the bonding layer; a bonding material used by the bonding layer comprises at least one of surface-modified polyvinylidene fluoride, gelatin and polytetrafluoroethylene, and the surface of the bonding material contains at least one of oxygen, nitrogen and hydrogen elements; the coating layer is made of a carbon material; the surface-modified polytetrafluoroethylene is easier to infiltrate by electrolyte, and the polytetrafluoroethylene coated with the carbon material can passivate the surface of the polytetrafluoroethylene, prevent irreversible decomposition of the polytetrafluoroethylene in the charging and discharging process, maintain the bonding effect and facilitate improvement of the cycle performance and the first coulombic efficiency of the battery; the polytetrafluoroethylene is easy to fibrillate when being subjected to shearing force, and the surface modified polytetrafluoroethylene weakens the adverse effect of fibrillation on the coating effect of the carbon material, so that the problem that the impedance of the pole piece is increased after the polytetrafluoroethylene is fibrillated is effectively avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion batteries, and relates to a dry electrode binder and a preparation method and application thereof. Background Art

[0002] As we all know, the preparation process of lithium-ion batteries is generally a wet process; in the wet process, organic solvents are used to prepare slurry, which is then coated and baked into electrodes. However, the baking and recycling of organic solvents incur huge costs; and the use of organic solvents can cause serious pollution to the environment; therefore, compared with wet electrodes, dry electrodes have more promising application prospects and economic benefits.

[0003] The existing dry electrode preparation process is to mix the active material, conductive agent and fiberizable binder into powder and fiberize them, roll them to form a self-supporting film and then compound them with the current collector to finally form a dry electrode. In the preparation process of dry electrode, the binder needs to go through the steps of mixing and fiberization. During the preparation process, the binder may be unstable and cause its bonding performance to deteriorate. Although the binder accounts for a very small proportion in the electrode, it plays an important role in maintaining the stability of the electrode structure. The instability of the bonding effect will seriously affect the cycle stability of the battery and reduce the battery capacity. Therefore, it is necessary to provide an improved binder so that it can better improve the performance of the battery after being applied to the battery. Summary of the invention

[0004] In view of the above problems existing in the prior art, the object of the present invention is to provide a dry electrode binder and a preparation method and application thereof.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] The present invention provides a dry electrode binder, which comprises a bonding layer and a coating layer coated on the surface of the bonding layer;

[0007] The bonding layer is a bonding material, and the bonding material includes at least one of surface-modified polyvinylidene fluoride, gelatin, and polytetrafluoroethylene, and the surface of the bonding material contains at least one of oxygen, nitrogen, and hydrogen elements;

[0008] The coating layer is made of carbon material.

[0009] In some embodiments, based on the total mass of the dry electrode binder being 100%, the content of the coating layer is 0.1% to 5%.

[0010] In some embodiments, the content of the coating layer is 2% to 5%.

[0011] In some embodiments, the bonding material is surface-modified polytetrafluoroethylene; the content of fluorine in the surface-modified polytetrafluoroethylene is recorded as F, the mass content of oxygen is recorded as O, the mass content of carbon is recorded as C, and the mass content of nitrogen is recorded as N; wherein, 1.1≤F / C≤1.6, 0.1≤(O+N) / C≤0.25.

[0012] In some embodiments, the carbon material includes at least one of conductive carbon black and graphite.

[0013] In some embodiments, the pH value of the carbon material is in the range of 3-5.

[0014] In some embodiments, the coating layer is obtained by mixing the carbon material and the bonding material and then ball milling the mixture.

[0015] The present invention also provides a method for preparing a dry electrode binder, the method comprising the following steps:

[0016] Plasma-treating the binder to obtain a surface-modified binder;

[0017] The surface-modified binder is used as a binder layer and mixed with a carbon material and ball-milled, so that the carbon material is coated on the surface of the binder layer to form a coating layer, thereby obtaining a dry electrode binder.

[0018] In some embodiments, based on the total mass of the dry electrode binder as 100%, the content of the coating layer is 2% to 5%; and the carbon material includes at least one of conductive carbon black and graphite; and the binder includes at least one of polyvinylidene fluoride, gelatin, and polytetrafluoroethylene.

[0019] In some embodiments, the step of subjecting the binder to plasma treatment to obtain a surface-modified binder comprises:

[0020] placing the binder in a plasma processing chamber;

[0021] At least one gas selected from oxygen, nitrogen and hydrogen is injected into the plasma treatment chamber to react with the surface of the binder for 1 to 5 minutes.

[0022] The present invention further provides a dry electrode sheet, comprising the above-mentioned dry electrode binder or the dry electrode binder prepared according to the preparation method of the above-mentioned dry electrode binder.

[0023] The present invention further provides a lithium ion battery comprising the above dry electrode sheet.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The dry electrode binder of the present invention comprises a bonding layer and a coating layer coated on the surface of the bonding layer. The bonding layer uses a bonding material including polyvinylidene fluoride (PVDF). At least one of polytetrafluoroethylene (PTFE), polydifluoride (PVDF), gelatin, and surface-modified polytetrafluoroethylene (PTFE); a coating layer using carbon material; wherein the hydrophilicity of PTFE can be improved and the surface tension can be increased by surface modification; the surface-modified PTFE is easier to be infiltrated by electrolyte, and the carbon material wrapping PTFE can passivate the PTFE surface, thereby preventing the irreversible consumption of Li ions by PTFE during the charge and discharge process, inhibiting the continuous decomposition of PTFE, and stably maintaining the adhesion effect of PTFE, which is beneficial to improving the cycle performance and the first coulomb efficiency of the dry-process battery; the surface-modified PTFE also improves the adhesion to the carbon material; PTFE will be subjected to huge shear force and fibrillate when preparing dry-process batteries, and the surface-modified PTFE can further improve the coating effect of carbon material on PTFE, weaken the adverse effect of fibrillation on the coating effect, and effectively avoid the problem of increased contact resistance between active particles after PTFE fibrillation, thereby causing high impedance of the electrode. DETAILED DESCRIPTION

[0026] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be further described in detail below in conjunction with specific embodiments, but the embodiments of the present invention are not limited thereto.

[0027] In the embodiment of the present invention, the dry-process negative electrode is taken as an example for description, but it is not limited thereto, and the dry-process positive electrode is also applicable to the present invention.

[0028] In the embodiment of the present invention, graphite is used as the active material in the dry-process negative electrode, but it is not limited thereto; similarly, the mass ratio of the active material can be adaptively adjusted as needed, and the present invention does not make any specific limitation thereto.

[0029] Example 1

[0030] This embodiment provides a dry electrode binder, including a bonding layer and a coating layer coated on the surface of the bonding layer; the material of the bonding layer includes surface-modified PTFE, the material of the coating layer is conductive carbon black (Super P, SP), and the pH value of SP is selected to be 4.

[0031] The preparation method of the dry electrode binder comprises the following steps:

[0032] Placing the PTFE in a plasma treatment chamber;

[0033] A mixture of nitrogen and oxygen is injected into the plasma treatment chamber to react with the PTFE surface, and the plasma treatment time is 2 minutes;

[0034] SP is mixed with plasma-treated PTFE and then ball-milled to achieve SP coating of PTFE to obtain a dry electrode binder;

[0035] Wherein, based on the total mass of the dry electrode binder being 100%, the coating amount of SP is 2%.

[0036] This embodiment also provides a dry electrode sheet, including the above-mentioned dry electrode binder.

[0037] This embodiment also provides a lithium-ion battery, including the above-mentioned dry electrode sheet.

[0038] The dry electrode binder in the present invention comprises an adhesive layer and a coating layer coated on the surface of the adhesive layer, wherein the adhesive layer comprises surface-modified PTFE, and the hydrophilicity of PTFE can be improved and the surface tension can be increased by surface modification; the surface-modified PTFE is easier to be infiltrated by electrolyte, and the surface of PTFE can be passivated by wrapping PTFE with SP, thereby preventing the irreversible consumption of Li ions by PTFE during charging and discharging, inhibiting the continuous decomposition of PTFE, and stably maintaining the bonding effect of PTFE, which is beneficial to improving the cycle performance and the first coulomb efficiency of the dry battery; the surface-modified PTFE also improves the bonding property to SP; PTFE will be subjected to huge shear force and fibrillate when preparing dry batteries, and the surface-modified PTFE can further improve the coating effect of SP on PTFE, weaken the adverse effect of fibrillation on the coating effect, and effectively avoid the problem of increased contact resistance between active particles after PTFE fibrillation, thereby causing high impedance of the pole piece.

[0039] In the preparation step of the dry electrode binder, plasma treatment causes a mixed gas of nitrogen and oxygen to generate plasma, and the plasma can remove polymer groups on the surface of PTFE and generate new functional groups on its surface, so that functional groups such as oxides and carboxyl groups appear on the surface of PTFE, which can significantly improve the hydrophilicity of the PTFE surface and the adhesion of PTFE to SP after fibrillation, thereby improving the wettability of PTFE to the electrolyte and the coating effect of SP on PTFE; the interaction time between plasma and the PTFE surface directly affects the type and number of functional groups on the PTFE surface, thereby affecting the surface modification effect of PTFE, and embodiments 2 to 5 are set, and the setting range of the plasma treatment time is further optimized by simply changing the plasma treatment time of PTFE.

[0040] In the preparation step of the dry electrode binder, after the SP is coated on PTFE, the irreversible side reaction of PTFE with other substances during the electrochemical reaction can be reduced, the decomposition of PTFE can be effectively inhibited, and the bonding failure can be prevented; and the first coulomb efficiency of the dry battery prepared by the dry electrode binder is improved, so that the electrochemical performance of the dry battery is improved; the amount of the coating layer SP directly affects the bonding effect of the PTFE surface, and embodiments 6 to 8 are set, and the setting range of the SP coating amount is further optimized by simply changing the SP coating amount.

[0041] Embodiments 2 to 5

[0042] Specifically, embodiments 2 to 5 all provide a dry electrode binder, a dry electrode sheet comprising the dry electrode binder, and a lithium ion battery comprising the dry electrode sheet;

[0043] The only difference between Example 2 and Example 1 is that the plasma treatment time of PTFE is 1 minute.

[0044] The only difference between Example 3 and Example 1 is that the plasma treatment time of PTFE is 3 minutes.

[0045] The only difference between Example 4 and Example 1 is that the plasma treatment time of PTFE is 4 minutes.

[0046] The only difference between Example 5 and Example 1 is that the plasma treatment time of PTFE is 5 minutes.

[0047] Embodiments 6 to 8

[0048] Specifically, embodiments 6 to 8 all provide a dry electrode binder, a dry electrode sheet comprising the dry electrode binder, and a lithium ion battery comprising the dry electrode sheet;

[0049] The only difference between Example 6 and Example 1 is that the coating amount of SP on PTFE is 3%.

[0050] The only difference between Example 7 and Example 1 is that the coating amount of SP on PTFE is 4%.

[0051] The only difference between Example 8 and Example 1 is that the coating amount of SP on PTFE is 5%.

[0052] Example 9

[0053] This embodiment provides a dry electrode binder, a dry electrode sheet including the dry electrode binder, and a lithium-ion battery including the dry electrode sheet; the only difference between the embodiment and the first embodiment is that the material SP of the coating layer is replaced by graphite.

[0054] Example 10

[0055] This embodiment provides a dry electrode binder, a dry electrode sheet including the dry electrode binder, and a lithium-ion battery including the dry electrode sheet; the only difference between the embodiment and the first embodiment is that the bonding material in the embodiment is surface-modified PVDF.

[0056] Comparative Example 1

[0057] This comparative example provides a binder, a dry electrode sheet including the binder, and a lithium ion battery including the dry electrode sheet; the only difference between this comparative example and Example 1 is that the binder of this comparative example is PTFE that has not been subjected to any treatment.

[0058] Comparative Example 2

[0059] This comparative example provides a binder, a dry electrode sheet including the binder, and a lithium ion battery including the dry electrode sheet; the only difference between it and Example 1 is that PTFE is directly mixed with SP and ball-milled without plasma treatment, so that the binder is obtained after SP coating PTFE; as a control experiment of Comparative Example 1, it further demonstrates the modification effect of the plasma treatment step in Example 1 on PTFE.

[0060] Comparative Example 3

[0061] This comparative example provides a binder, a dry electrode sheet including the binder, and a lithium ion battery including the dry electrode sheet; the only difference between it and Example 1 is that the surface-modified PTFE is not coated with SP; the PTFE is placed in a plasma treatment chamber, a mixed gas of nitrogen and oxygen is injected, and plasma treatment is performed for 2 minutes to obtain a binder; as a control experiment of Comparative Example 1, the modification effect of the step of forming an SP coating layer on the PTFE adhesive layer in Example 1 on the PTFE is further demonstrated.

[0062] Comparative Example 4

[0063] Specifically, Comparative Example 4 provides a binder, a dry electrode sheet comprising the binder, and a lithium ion battery comprising the dry electrode sheet;

[0064] The only difference between Comparative Example 4 and Example 1 is that the plasma treatment time of PTFE is 7 minutes.

[0065] Comparative Examples 5 to 7

[0066] Specifically, Comparative Examples 5 to 7 all provide a binder, a dry electrode sheet comprising the binder, and a lithium ion battery comprising the dry electrode sheet;

[0067] The only difference between Comparative Example 5 and Example 1 is that the coating amount of SP on PTFE is 0.1%.

[0068] The only difference between Comparative Example 6 and Example 1 is that the coating amount of SP on PTFE is 1%.

[0069] The only difference between Comparative Example 7 and Example 1 is that the coating amount of SP on PTFE is 6%.

[0070] Comparative Examples 8 to 9

[0071] Specifically, Comparative Examples 8 to 9 all provide a binder, a dry electrode sheet comprising the binder, and a lithium ion battery comprising the dry electrode sheet;

[0072] The only difference between Comparative Example 8 and Example 1 is that the pH value of SP in this comparative example is 2;

[0073] The only difference between Comparative Example 9 and Example 1 is that the pH value of SP in this comparative example is 6.

[0074] Experimental example

[0075] The PTFE obtained after the plasma treatment steps of Examples 1 to 5, Comparative Example 1 and Comparative Example 4 was left to stand for 30 minutes until it reached a stable state, and the following operations were performed: the mass percentages of elements and chemical bonds on its surface were collected; the collection results are shown in Table 1; the collection methods include but are not limited to spectroscopy and thermochemical methods.

[0076] Table 1

[0077]

[0078] The following operations were performed on the dry electrode sheets and lithium-ion batteries obtained in Examples 1 to 10 and Comparative Examples 1 to 7: testing the complete wetting time of the dry electrode sheets in the electrolyte, testing the membrane resistivity of the dry electrode sheets, testing the first coulomb cycle efficiency of the lithium-ion battery, and testing the 500cls cycle retention rate of the lithium-ion battery; the measured results are shown in Table 2.

[0079] Table 2

[0080]

[0081]

[0082] The following operations were performed on the SP, dry electrode sheet and lithium ion battery in Example 1 and Comparative Example 8 and Comparative Example 9: the ratio of oxygen-containing groups in the SP was tested, the coefficient of dispersion of the film resistance of the dry electrode sheet was tested, and the 500cls cycle retention rate of the lithium ion battery was tested; the measured results are shown in Table 1;

[0083] Table 3

[0084]

[0085] During the plasma treatment process, a mixture of nitrogen and oxygen is ionized into plasma in the plasma treatment chamber. Active particles and polar groups are generated during the initiation of the plasma. The active particles and polar groups can remove F ions on the surface of PTFE and generate free radicals, which can induce a cross-linking reaction or form an unsaturated bond on the surface of PTFE, thereby introducing N and O elements and generating new functional groups on the surface of PTFE. After the functional groups containing H and O elements such as -NH, -NCO, and -COOH are generated on the surface of PTFE, the hydrophilicity and surface tension of the PTFE surface and the adhesion of PTFE to SP after fibrillation can be significantly improved, thereby improving the wettability of PTFE to the electrolyte and the coating effect of SP on PTFE. After SP is coated with PTFE, the stability of PTFE in the electrochemical reaction process can be improved, and the side reaction or irreversible decomposition of PTFE with other substances can be inhibited, thereby overcoming the problem of PTFE adhesion failure. The electrochemical performance of the dry-process battery is improved, and the first coulomb efficiency of the dry-process battery is improved.

[0086] After PTFE is treated with plasma, the content of the elements in the stable state needs to satisfy 1.1≤F / C≤1.6 and 0.1≤(O+N) / C≤0.25 at the same time. Combining the data of Examples 1 to 5 in Tables 1 and 2, it can be seen that when 1.1≤F / C≤1.6 is satisfied, the larger the F / C value, the larger the coefficient of dispersion of the diaphragm resistance, because the increase in the F / C value indicates that the surface F elements of PTFE increase and the polar groups decrease, and the SP coating uniformity and bonding of PTFE are poor, which directly leads to the membrane The sheet resistance is unevenly distributed, resulting in a larger dispersion coefficient of the diaphragm resistance. When 0.1≤(O+N) / C≤0.25 is satisfied, the larger the value of (O+N) / C, the smaller the dispersion coefficient of the diaphragm resistance, because the increase in the value of -(O+N / C) indicates that more -CF2 bonds are broken and more functional groups containing H and O elements are generated, thereby improving the adhesion and hydrophilicity of the PTFE surface, enhancing the ball milling coating effect of PTFE and SP, and improving the uniformity of the diaphragm resistance, thereby reducing the dispersion coefficient of the diaphragm resistance.

[0087] Combining Table 1 and Table 2, it can be seen that in Comparative Example 4, F / C <1.1, (O+N) / C>0.25, when F / C <1.1 or (O+N) / C>0.25, the fiberization ability of PTFE is greatly weakened, the stability of the prepared dry electrode sheet is poor, and the cycle performance is greatly reduced; in Comparative Example 1, F / C>1.6, (O+N) / C<0.1, when F / C>1.6 or (O+N) / C<0.1, on the one hand, the surface of PTFE is coated with more F atoms, which not only enhances the hydrophobicity and oleophobicity of its surface, but also reduces the number of polar functional groups exposed on its surface. On the other hand, the high F / C content indicates that the number of polar groups in the PTFE after plasma treatment is insufficient. When the number of polar groups is insufficient, the surface energy of PTFE is small, which will lead to a decrease in the binding force between PTFE and SP and poor uniformity of ball milling coating, thereby causing problems such as uneven distribution of the resistance of the electrode sheet prepared subsequently and loss of cycle performance of the battery. For example, the dispersion coefficient of the diaphragm resistance in Comparative Example 1 is 3.43%, which is much higher than that of other embodiments.

[0088] Observing the results in Table 1, it is shown that the ratio of F / C on the PTFE surface after plasma treatment for 2 minutes in Example 1 is the lowest, and the value of -(O+N / C) is the highest; therefore, the PTFE in Example 1 has stronger surface adhesion and better electrolyte infiltration effect than other embodiments and comparative examples; it can be seen that under the condition of plasma treatment of PTFE for 2 minutes given in the present invention, the surface-modified PTFE has stronger surface adhesion and electrolyte infiltration effect.

[0089] Observe the test results of Comparative Examples 1 to 3 in Table 2. Comparative Example 2 and Comparative Example 3 are respectively used as control experiments for plasma treatment surface modification of PTFE and SP coating surface modification of PTFE; it can be seen that the electrolyte infiltration rate of the dry electrode sheet in Comparative Example 2 and Comparative Example 3 is significantly better than that in Comparative Example 1, the membrane resistivity is significantly lower than that in Comparative Example 1, and the first coulomb efficiency and capacity retention rate of the lithium ion battery in Comparative Example 2 and Comparative Example 3 after 500 cycles are significantly better than those in Comparative Example 1;

[0090] Compared with Comparative Example 2, Example 1 selects ball milling to coat the carbon material on the outside of the bonding material; when the bonding material uses surface-modified PTFE, there are fiberizable parts and non-fibrous parts on the surface of the PTFE after plasma treatment; in the process of coating the carbon material by ball milling, the fiberizable part on the surface of the PTFE can be pre-fiberized, which will further increase the fiber aspect ratio of the PTFE in the subsequent film thinning process of preparing the dry electrode pole piece, and can also increase the surface area exposed to the outside of the active substance, so as to achieve long-range connection between the active particles; at the same time, the carbon material will be evenly coated on the non-fibrous part of the PTFE containing polar groups, that is, the plasma-treated part; because the surface energy of the carbon material is relatively high, the bonding force with the non-fibrous part of the PTFE with increased surface energy after plasma treatment is also enhanced, and it can withstand large shear forces, further ensuring the uniformity and stability of the conductive network; it can be seen that coating the carbon material on the outside of the bonding material by mixed ball milling can effectively improve the fiber performance of PTFE and further improve the structural properties of the dry electrode binder.

[0091] Compared with Comparative Example 3, Example 1 chooses to first plasma treat the polytetrafluoroethylene, and then mix it with the carbon material and ball mill it for coating; if the PTFE is not plasma treated and is directly coated with the carbon material, since the surface of the PTFE is coated with F atoms, the bonding force between the PTFE and the carbon material is weak at this time, the coating effect is poor, and the coating layer is easily destroyed in the subsequent film forming and thinning process; in addition, the surface of the PTFE exposed on the surface of the electrode sheet that has not been plasma treated has hydrophobicity and oleophobicity, and it will also cause difficulty in electrolyte infiltration; in summary, after the PTFE is subjected to the two modification methods of plasma treatment and SP coating given in the present invention, the electrolyte wettability of the dry electrode binder containing PTFE and the dry electrode sheet prepared therefrom can be improved, and the first coulomb efficiency and cycle performance of the lithium ion battery prepared by the dry electrode sheet are also improved, proving the superiority of the modified dry electrode binder structure.

[0092] Secondly, it can be seen from the test results of Example 1 and Examples 6 to 8 and Comparative Examples 5 to 7 in Table 2 that, in the dry electrode binder, as the coating amount of SP on PTFE increases, the electrolyte wettability of the dry electrode sheet obtained is better and the conductivity is stronger, and the first coulomb efficiency and cycle efficiency of the lithium ion battery obtained are also higher; however, in Comparative Example 7, when the coating amount of SP exceeds 5%, the obtained battery performance test results are worse. This is because the coating layer is too thick at this time, and the polar surfaces of PTFE obtained by plasma treatment are all coated with SP, and the fiberizable part of PTFE is also greatly weakened by the shear friction due to being coated with SP, resulting in a low degree of fiberization of the obtained pole piece and a decrease in the battery cycle stability.

[0093] Furthermore, by observing the test results of Example 1 and Example 9, it can be seen that the surface modification effect of PTFE after graphite coating is not as good as the surface modification effect of SP coating; on the one hand, this is because SP has stronger conductivity, smaller particle size and more uniform coating than graphite; on the other hand, it is because the surface energy of SP and PTFE is closer, the bonding between the two is better, and the electrolyte infiltration rate of the dry electrode binder is better promoted; in the present invention, when the bonding layer uses surface-modified PTFE and the coating layer uses conductive carbon black, a better coating effect can be brought.

[0094] By observing the test results of Example 1 and Comparative Examples 8 and 9, it can be seen that the proportion of oxygen-containing groups in the SP of Comparative Examples 8 and 9 is much lower than that of Example 1, and the pH value of SP in Comparative Examples 8 and 9 is too high or too low, which will affect the diaphragm resistance dispersion coefficient and the cycle performance of the battery; in the present invention, the coating layer selects a carbon material with a pH value in the range of 3 to 5 because the number of oxygen groups in the carbon material is appropriate at this time, and the number of oxygen groups directly affects the surface energy of the carbon material, so that the carbon material and the modified PTFE surface energy are more compatible, and the carbon material at this time has a stronger bonding force with the PTFE containing a large amount of N / H after plasma treatment during ball milling coating, and the stability and uniformity of the dry electrode binder material can be steadily improved. After the electrode is prepared, the resistance dispersion coefficient of the diaphragm is also greatly reduced, which can improve the resistance consistency and improve the cycle performance of the battery cell.

[0095] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.

Claims

1. A dry electrode binder, characterized in that: The dry electrode binder comprises a bonding layer and a coating layer coated on the surface of the bonding layer; The bonding layer is a bonding material, and the bonding material includes at least one of surface-modified polyvinylidene fluoride, gelatin, and polytetrafluoroethylene, and the surface of the bonding material contains at least one of oxygen, nitrogen, and hydrogen elements; The coating layer is made of carbon material.

2. The dry electrode binder according to claim 1, characterized in that: Based on the total mass of the dry electrode binder being 100%, the content of the coating layer is 0.1% to 5%.

3. The dry electrode binder according to claim 2, characterized in that: The content of the coating layer is 2% to 5%.

4. The dry electrode binder according to claim 3, characterized in that: The bonding material is surface-modified polytetrafluoroethylene; the mass content of fluorine element in the surface-modified polytetrafluoroethylene is recorded as F, the mass content of oxygen element is recorded as O, the mass content of carbon element is recorded as C, and the mass content of nitrogen element is recorded as N; wherein 1.1≤F / C≤1.6, 0.1≤(O+N) / C≤0.

25.

5. The dry electrode binder according to claim 3 or 4, characterized in that: The carbon material includes at least one of conductive carbon black and graphite.

6. The dry electrode binder according to claim 5, characterized in that: The pH value of the carbon material is in the range of 3-5.

7. The dry electrode binder according to claim 5, characterized in that: The coating layer is obtained by mixing the carbon material and the bonding material and then ball milling the mixture.

8. A method for preparing a dry electrode binder, characterized in that: The preparation method comprises the following steps: Plasma-treating the binder to obtain a surface-modified binder; The surface-modified binder is used as a binder layer and mixed with a carbon material and ball-milled, so that the carbon material is coated on the surface of the binder layer to form a coating layer, thereby obtaining a dry electrode binder.

9. The method for preparing a dry electrode binder according to claim 8, characterized in that: Based on the total mass of the dry electrode binder being 100%, the content of the coating layer is 2% to 5%; the carbon material includes at least one of conductive carbon black and graphite; and the binder includes at least one of polyvinylidene fluoride, gelatin and polytetrafluoroethylene.

10. The method for preparing a dry electrode binder according to claim 9, characterized in that: The step of subjecting the binder to plasma treatment to obtain a surface-modified binder comprises: placing the binder in a plasma processing chamber; At least one gas selected from oxygen, nitrogen and hydrogen is injected into the plasma treatment chamber to react with the surface of the binder for 1 to 5 minutes.

11. A dry electrode sheet, characterized in that: The invention comprises the dry electrode binder according to any one of claims 1 to 7 or the dry electrode binder prepared according to the preparation method according to any one of claims 8 to 10.

12. A lithium ion battery, characterized in that: A dry-process electrode sheet comprising the dry-process electrode sheet according to claim 11.

Citation Information

Cited By

  • Fluororesin fluororubber composite material with high fracture work and preparation method thereof

    CN120098462A

  • Conductive carbon coated modified PTFE / disulfide bond composite binder, positive plate and preparation method

    CN120737762A

  • Conductive carbon-coated modified PTFE / disulfide bond composite binder, positive electrode sheet and preparation method

    CN120737762B

  • Dry-method negative electrode material as well as preparation method and application thereof

    CN121790321A