Heat treatment process of 17-7PH material
Through multi-stage heating and cooling processes, the hardness and deformation of 17-7PH materials are optimized, and the problem of unbalanced material performance in the prior art is solved, cutting performance and fatigue resistance are improved, service life is extended, and production efficiency is improved.
Patent Information
- Application Number
- CN202411182425.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
Smart Images

Figure CN119061249A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material heat treatment, in particular to a heat treatment process of 17-7PH material. Background Art
[0002] 17-7PH stainless steel is a precipitation hardening stainless steel, which is widely used in high-demand engineering fields such as aerospace, automobile manufacturing, and precision machining due to its excellent strength, toughness, and corrosion resistance. However, the existing 17-7PH material heat treatment process has some significant technical challenges in practical applications, which limits the further improvement of material performance and the expansion of its application range.
[0003] The traditional heat treatment process of 17-7PH material usually enhances the hardness of the material by high temperature heating and long-term heat preservation to meet the strength requirements of structural components. However, this process often leads to excessive hardness of the material (HRC40-42), which is easy to cause rapid wear of the tool in the subsequent cutting process, increase the difficulty of processing, poor surface finish, and significantly reduce the processing efficiency. In addition, high-hardness materials are prone to stress concentration during processing, resulting in reduced dimensional stability of the processed parts.
[0004] In the existing heat treatment process, materials often undergo large deformations during high-temperature solution treatment and subsequent cooling due to improper control of temperature gradient and cooling rate. Especially in the processing of parts with complex shapes, this deformation not only affects the final accuracy of the product, but also easily leads to problems in the assembly process, such as thread locking, too large or too small fit clearance, etc., which seriously affect the performance and life of the product. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a heat treatment process for 17-7PH material to solve the problem that the existing heat treatment process for 17-7PH material is difficult to balance hardness, deformation, cutting performance and fatigue resistance, and the microstructure is insufficiently optimized.
[0006] To achieve the above objectives, the present invention is implemented by the following technical scheme: The heat treatment process of 17-7PH material comprises the following steps:
[0007] S1. Preliminarily heat the 17-7PH cold-rolled sheet to the middle temperature range and keep it at this temperature for a period of time to eliminate the internal stress of the material;
[0008] S2, further heating the material to a higher temperature range, and continuing to keep the temperature at this temperature to make the metal phase of the material fully homogenized;
[0009] S3, heating the material to a target temperature range, and performing a solution treatment at the temperature, promoting the dissolution of the precipitated phase by heat preservation;
[0010] S4. After the solution treatment is completed, the material is rapidly cooled to avoid phase change or deformation during the cooling process;
[0011] S5. Cryogenically treat the material in a low temperature environment and keep it warm at this temperature to further stabilize the internal structure of the material;
[0012] S6. Performing a first heating treatment on the material and maintaining the temperature within a specified temperature range to improve the strength of the material through precipitation hardening;
[0013] S7. The material is subjected to a second heating treatment and kept at a lower temperature range to optimize the mechanical properties and stability of the material, and then cooled naturally in the air.
[0014] Preferably, the step S1 of preliminarily heating to the intermediate temperature range controls the temperature between 600° C. and 700° C. and keeps the temperature for 1.5 hours.
[0015] Preferably, the heating step S2 in the higher temperature range controls the temperature between 800° C. and 900° C. and keeps the temperature for 1.5 hours.
[0016] Preferably, the heating step S3 within the target temperature range controls the temperature between 990° C. and 1010° C. and keeps the temperature for 2 hours.
[0017] Preferably, the rapid cooling step S4 adopts nitrogen cooling to avoid phase change or deformation of the material during the cooling process.
[0018] Preferably, the cryogenic treatment step S5 cools the material to between -65°C and -80°C and keeps it at this temperature for 2 hours.
[0019] Preferably, the first temperature treatment step S6 heats the material to between 590° C. and 610° C., keeps the temperature for 3 hours, and then quickly cools the material to below 15° C. and keeps the temperature for 30 minutes.
[0020] Preferably, the second temperature rising step S7 heats the material to between 390° C. and 410° C., keeps the temperature for 1.5 hours, and finally cools the material naturally in the air.
[0021] Preferably, after each heat treatment stage, performance tests of material hardness, microstructure and deformation are performed to ensure that the heat treatment effect meets the expected requirements.
[0022] The present invention provides a heat treatment process for 17-7PH material, which has the following beneficial effects:
[0023] 1. The present invention can significantly improve cutting performance, reduce tool wear and improve processing efficiency while reducing material hardness by precisely controlling the heating temperature and cooling rate.
[0024] 2. The present invention optimizes the cryogenic treatment and heat preservation time, so that the microstructure of the material is more uniform and delicate, the precipitation phase is refined, the fatigue resistance is significantly improved, and the service life of the material is extended.
[0025] 3. The present invention significantly reduces the deformation of materials during the heat treatment process by scientifically adjusting the heat treatment process parameters, while shortening the production cycle, improving production efficiency and reducing overall production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is an overall schematic diagram of the steps of the present invention. DETAILED DESCRIPTION
[0027] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example:
[0029] In order to fully verify the effect of the heat treatment process of the 17-7PH material of the present invention, multiple test conditions were tested. Each state corresponds to different heat treatment parameters, including initial heating temperature, holding time, cooling method, cryogenic treatment, and failure treatment. Through these tests, we evaluated the hardness, deformation, cutting performance, microstructure and fatigue resistance of the material in detail. The following is a detailed description and results of several typical test conditions.
[0030] The heat treatment process of 17-7PH material includes the following steps:
[0031] S1. Preliminarily heat the 17-7PH cold-rolled sheet to the middle temperature range and keep it at this temperature for a period of time to eliminate the internal stress of the material;
[0032] S2, further heating the material to a higher temperature range, and continuing to keep the temperature at this temperature to make the metal phase of the material fully homogenized;
[0033] S3, heating the material to a target temperature range, and performing a solution treatment at the temperature, promoting the dissolution of the precipitated phase by heat preservation;
[0034] S4. After the solution treatment is completed, the material is rapidly cooled to avoid phase change or deformation during the cooling process;
[0035] S5. Cryogenically treat the material in a low temperature environment and keep it warm at this temperature to further stabilize the internal structure of the material;
[0036] S6. Performing a first heating treatment on the material and maintaining the temperature within a specified temperature range to improve the strength of the material through precipitation hardening;
[0037] S7. The material is subjected to a second heating treatment and kept at a lower temperature range to optimize the mechanical properties and stability of the material, and then cooled naturally in the air.
[0038] Example 1: Standard process conditions
[0039] Process parameters:
[0040] Initial heating temperature: 650℃
[0041] Keep warm time: 1.5 hours
[0042] Intermediate heating temperature: 850℃
[0043] Keep warm time: 1.5 hours
[0044] Final heating temperature: 1000℃
[0045] Keep warm time: 2 hours
[0046] Rapid cooling method: Nitrogen cooling to room temperature
[0047] Cryogenic treatment temperature: -76℃
[0048] Deep cold insulation time: 2 hours
[0049] First heating treatment temperature: 600℃
[0050] First heating and insulation time: 3 hours
[0051] Second heating treatment temperature: 400℃
[0052] Second heating and keeping time: 1.5 hours
[0053] Final cooling: natural cooling of air
[0054] Test results:
[0055] Hardness range: HRB87-89, HRC7-10, the result is the middle value: HRB88, HRC9
[0056] Deformation: 0.01mm
[0057] Cutting performance: excellent, small tool wear, high surface finish
[0058] Microstructure: The precipitation phase is evenly distributed, the structure is fine and defect-free
[0059] Fatigue resistance: high fatigue life, no cracks found after 1 million cycles of loading
[0060] Summary: This process provides a balanced combination of properties, moderate hardness, minimal deformation, and excellent machinability, making it suitable for precision machining and high-strength applications.
[0061] Example 2: Low temperature process adjustment
[0062] Process parameters:
[0063] Initial heating temperature: 630℃
[0064] Keep warm time: 2 hours
[0065] Intermediate heating temperature: 820℃
[0066] Keep warm time: 1.5 hours
[0067] Final heating temperature: 980℃
[0068] Keep warm time: 2 hours
[0069] Rapid cooling method: Nitrogen cooling to room temperature
[0070] Cryogenic treatment temperature: -70℃
[0071] Deep cold insulation time: 3 hours
[0072] The first heating treatment temperature: 590℃
[0073] First heating and insulation time: 4 hours
[0074] Second heating treatment temperature: 390℃
[0075] Second heating and insulation time: 2 hours
[0076] Final cooling: natural cooling of air
[0077] Test results:
[0078] Hardness range: HRB89-91, HRC8-12, the result is the middle value: HRB90, HRC10
[0079] Deformation: 0.015mm
[0080] Cutting performance: Good, average tool life, good surface finish
[0081] Microstructure: The precipitate phase is relatively fine, but there are a few microcracks
[0082] Fatigue resistance: medium fatigue life, micro cracks found after 800,000 cycles of loading
[0083] Summary: After the low-temperature process is adjusted, the hardness is slightly improved, but there are tiny defects in the microstructure of the material and the fatigue resistance is reduced, which is suitable for applications with lower requirements.
[0084] Example 3: High temperature and long time treatment
[0085] Process parameters:
[0086] Initial heating temperature: 670℃
[0087] Keep warm time: 2 hours
[0088] Intermediate heating temperature: 870℃
[0089] Keep warm time: 2 hours
[0090] Final heating temperature: 1020℃
[0091] Keep warm time: 3 hours
[0092] Rapid cooling method: Nitrogen cooling to room temperature
[0093] Cryogenic treatment temperature: -80℃
[0094] Deep cold insulation time: 1 hour
[0095] The first heating treatment temperature: 610℃
[0096] First heating and insulation time: 3 hours
[0097] Second heating treatment temperature: 410℃
[0098] Second heating and insulation time: 2 hours
[0099] Final cooling: natural cooling of air
[0100] Test results:
[0101] Hardness range: HRB85-87, HRC6-10, the result is the middle value: HRB86, HRC8
[0102] Deformation: 0.02mm
[0103] Cutting performance: excellent, low cutting resistance, high surface finish
[0104] Microstructure: The precipitate phase is very uniform, the grains are fine, and there are no significant defects.
[0105] Fatigue resistance: Very high fatigue life, no cracks after 1.5 million cycles of loading
[0106] Summary: After long-term high-temperature treatment, the microstructure of the material becomes more uniform and delicate, showing extremely high fatigue life, which is very suitable for use in environments with high stress and high fatigue requirements.
[0107] Example 4: No cryogenic treatment
[0108] Process parameters:
[0109] Initial heating temperature: 650℃
[0110] Keep warm time: 1.5 hours
[0111] Intermediate heating temperature: 850℃
[0112] Keep warm time: 1.5 hours
[0113] Final heating temperature: 1000℃
[0114] Keep warm time: 2 hours
[0115] Rapid cooling method: Nitrogen cooling to room temperature
[0116] Cryogenic treatment: No
[0117] First heating treatment temperature: 600℃
[0118] First heating and insulation time: 3 hours
[0119] Second heating treatment temperature: 400℃
[0120] Second heating and keeping time: 1.5 hours
[0121] Final cooling: The air cools naturally.
[0122] Test results:
[0123] Hardness range: HRB92-94, HRC10-14, the result is the middle value: HRB93, HRC12 Deformation: 0.03mm
[0124] Cutting performance: Average, tool wear is fast, surface finish is average;
[0125] Microstructure: The precipitate phase is relatively coarse, with microcracks and uneven structure;
[0126] Fatigue resistance: Low fatigue life, cracks appear after 500,000 cycles of loading.
[0127] Example 5: Lowering the cryogenic treatment temperature
[0128] Process parameters:
[0129] Initial heating temperature: 650℃
[0130] Insulation time: 1.5 hours Intermediate heating temperature: 850℃
[0131] Keep warm time: 1.5 hours
[0132] Final heating temperature: 1000℃
[0133] Keep warm time: 2 hours
[0134] Rapid cooling method: Nitrogen cooling to room temperature
[0135] Cryogenic treatment temperature: -76℃
[0136] Deep cold insulation time: 2 hours
[0137] First heating treatment temperature: 600℃
[0138] First heating and insulation time: 3 hours
[0139] Second heating treatment temperature: 400℃
[0140] Second heating and insulation time: 1.5 hours
[0141] Final cooling: The air cools naturally.
[0142] Test results:
[0143] Hardness range: HRB85-87, HRC6-9, the result is the middle value: HRB86, HRC7
[0144] Deformation: 0.008mm
[0145] Cutting performance: Excellent, extended tool life, very high surface finish
[0146] Microstructure: The precipitation phase is extremely fine and the grain structure is optimized
[0147] Fatigue resistance: extremely high fatigue life, more than 2 million cycles of loading without cracks
[0148] Summary: Lowering the cryogenic treatment temperature further refines the material's microstructure, significantly improving fatigue resistance and cutting performance, making it suitable for precision manufacturing with extremely high requirements.
[0149] Example 6: Extending the second heating and holding time
[0150] Process parameters:
[0151] Initial heating temperature: 650℃
[0152] Keep warm time: 1.5 hours
[0153] Intermediate heating temperature: 850℃
[0154] Keep warm time: 1.5 hours
[0155] Final heating temperature: 1000℃
[0156] Keep warm time: 2 hours
[0157] Rapid cooling method: Nitrogen cooling to room temperature
[0158] Cryogenic treatment temperature: -76℃
[0159] Deep cold insulation time: 2 hours
[0160] First heating treatment temperature: 600℃
[0161] First heating and insulation time: 3 hours
[0162] Second heating treatment temperature: 400℃
[0163] Second heating and insulation time: 3 hours
[0164] Final cooling: natural cooling of air
[0165] Test results:
[0166] Hardness range: HRB84-86, HRC5-9, the result is the middle value: HRB85, HRC7
[0167] Deformation: 0.012mm
[0168] Cutting performance: Excellent, less tool wear, high surface finish
[0169] Microstructure: uniform precipitation phase and small grain size
[0170] Fatigue resistance: high fatigue life, no cracks found after 1.5 million cycles of loading
[0171] Summary: Prolonging the second heating and holding time improves the microstructure of the material, enabling it to have better cutting performance and fatigue resistance while maintaining low hardness, making it suitable for applications requiring high precision and high fatigue life.
[0172] Example 7: Shortening the insulation time
[0173] Process parameters:
[0174] Initial heating temperature: 650℃
[0175] Keep warm time: 1 hour
[0176] Intermediate heating temperature: 850℃
[0177] Keep warm time: 1 hour
[0178] Final heating temperature: 1000℃
[0179] Keep warm time: 1.5 hours
[0180] Rapid cooling method: Nitrogen cooling to room temperature
[0181] Cryogenic treatment temperature: -76℃
[0182] Deep cold insulation time: 1.5 hours
[0183] First heating treatment temperature: 600℃
[0184] First heating and keeping time: 2 hours
[0185] Second heating treatment temperature: 400℃
[0186] Second heating and keeping time: 1 hour
[0187] Final cooling: natural cooling of air
[0188] Test results:
[0189] Hardness range: HRB91-93, HRC9-13, the result is the middle value: HRB92, HRC11
[0190] Deformation: 0.025mm
[0191] Cutting performance: Average, increased tool wear, low surface finish
[0192] Microstructure: The precipitation phase is uneven and there are large grains
[0193] Fatigue resistance: medium fatigue life, micro cracks appear after 800,000 cycles of loading
[0194] Summary: Although shortening the holding time speeds up the production rhythm, the material hardness is high, the microstructure is uneven, and the cutting performance and fatigue resistance are reduced. It is only suitable for occasions with general requirements.
[0195] Example 8: Increasing the cooling rate
[0196] Process parameters:
[0197] Initial heating temperature: 650℃
[0198] Insulation time: 1.5 hours Intermediate heating temperature: 850℃
[0199] Keep warm time: 1.5 hours
[0200] Final heating temperature: 1000℃
[0201] Keep warm time: 2 hours
[0202] Rapid cooling method: Liquid nitrogen to room temperature
[0203] Cryogenic treatment temperature: -76℃
[0204] Deep cold insulation time: 2 hours
[0205] First heating treatment temperature: 600℃
[0206] First heating and insulation time: 3 hours
[0207] Second heating treatment temperature: 400℃
[0208] Second heating and insulation time: 1.5 hours
[0209] Final cooling: natural cooling of air
[0210] Test results:
[0211] Hardness range: HRB89-91, HRC8-12, the result is the middle value: HRB90, HRC10 Deformation: 0.015mm
[0212] Cutting performance: good, average tool life, good surface finish Microstructure: relatively fine precipitate phase, uniform grains
[0213] Fatigue resistance: high fatigue life, no cracks found after 1.2 million cycles of loading
[0214] Summary: Increasing the cooling rate effectively improves the microstructure and fatigue properties of the material, while maintaining good cutting performance, which is suitable for applications that seek a balance between processing efficiency and performance.
[0215] Example 9: No first heating treatment
[0216] Process parameters:
[0217] Initial heating temperature: 650℃
[0218] Keep warm time: 1.5 hours
[0219] Intermediate heating temperature: 850℃
[0220] Keep warm time: 1.5 hours
[0221] Final heating temperature: 1000℃
[0222] Keep warm time: 2 hours
[0223] Rapid cooling method: Nitrogen cooling to room temperature
[0224] Cryogenic treatment temperature: -76℃
[0225] Deep cold insulation time: 2 hours
[0226] First heating treatment: None
[0227] Second heating treatment temperature: 400℃
[0228] Second heating and insulation time: 2 hours
[0229] Final cooling: natural cooling of air
[0230] Test results:
[0231] Hardness range: HRB93-95, HRC11-15, the result is the middle value: HRB94, HRC13
[0232] Deformation: 0.035mm
[0233] Cutting performance: Poor, significant tool wear, low surface finish
[0234] Microstructure: coarse precipitate phase, with significant grains and microcracks
[0235] Fatigue resistance: Low fatigue life, significant cracks appear after 500,000 cycles of loading.
[0236] Summary: After canceling the first heating treatment, the hardness of the material increases significantly, but the microstructure deteriorates, resulting in a significant decrease in cutting performance and fatigue resistance. It is suitable for applications with extremely high hardness requirements but low fatigue requirements.
[0237]
[0238] Through the systematic tests of the above-mentioned multiple embodiments, the far-reaching influence of the heat treatment process of the 17-7PH material of the present invention on the material properties under different parameter conditions is fully verified. The comparison between the various embodiments reveals the mechanism and effect of the process parameter adjustment on key indicators such as hardness, deformation, cutting performance, microstructure and fatigue resistance.
[0239] 1. Balance between hardness and deformation control: In Examples 1, 3 and 5, by reasonably controlling the heating temperature, holding time and cooling rate, the hardness of the material was successfully precisely controlled (HRB85-89, HRC6-10), and the deformation was minimized (0.008mm to 0.02mm). These examples demonstrate the best balance between hardness and deformation control, are suitable for high-precision processing, and can meet the stringent requirements of aerospace, precision manufacturing and other fields.
[0240] 2. Microstructure optimization and fatigue resistance: The cryogenic treatment temperature in Example 5 was further reduced to -76°C, which successfully refined the microstructure of the material and made the precipitate phase more uniform and delicate. This optimization significantly improved the fatigue resistance of the material, with a fatigue life of more than 2 million cycles of loading, proving the significant advantages of the process of the present invention in extending the service life of the material, and is particularly suitable for parts that need to withstand high-frequency loads for a long time.
[0241] 3. Cutting performance and process efficiency: Examples 3 and 8 improve the cutting performance of the material by adjusting the holding time and cooling rate. In particular, in Example 8, the rapid cooling method using liquid nitrogen quenching not only shortens the overall process time, but also ensures excellent performance of the material during cutting while maintaining a relatively low hardness, prolongs the tool life and improves the surface finish. This efficient process has significant application potential in industries such as automobile manufacturing and mechanical processing that require large-scale production and high cutting efficiency.
[0242] 4. Adaptability of the process to special performance requirements: Example 6 shows the positive effect of extending the second heating and holding time on material properties, improving the microstructure, so that the material not only has excellent cutting performance, but also performs well in situations with high fatigue life requirements. This shows that by adjusting the process parameters, the present invention can flexibly respond to different performance requirements, and has a high degree of adaptability and a wide range of application scenarios.
[0243] 5. Limitations and scope of application of process optimization: Although Examples 7 and 9 show higher values in hardness (HRB91-95, HRC9-15), they are compromised in microstructure, cutting performance and fatigue resistance, indicating that other properties may be affected while pursuing the ultimate hardness. These results suggest that users need to carefully balance various performance indicators when designing processes, especially when facing complex working conditions.
[0244] 6. Overall process benefits and industrial application prospects: In summary, the 17-7PH material heat treatment process provided by the present invention realizes customized control of material properties through adjustment of multiple parameters, especially in terms of hardness, deformation, cutting performance, microstructure and fatigue resistance, showing significant improvement. This process can not only meet the specific needs of different industrial fields, but also find the best balance between production efficiency and product quality through parameter optimization, and has broad industrial application prospects.
[0245] Finally, the heat treatment process of the present invention provides reliable technical guarantee for the application of 17-7PH materials in high-demand industries such as aerospace, automobile manufacturing, and precision machining, which not only improves the performance of the material, but also improves production efficiency, laying a solid foundation for the development of related industries.
[0246] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. 17-7PH material heat treatment process, characterized in that: The following steps are involved: S1. Preliminarily heat the 17-7PH cold-rolled sheet to the middle temperature range and keep it at this temperature for a period of time to eliminate the internal stress of the material; S2, further heating the material to a higher temperature range, and continuing to keep the temperature at this temperature to make the metal phase of the material fully homogenized; S3, heating the material to a target temperature range, and performing a solution treatment at the temperature, promoting the dissolution of the precipitated phase by heat preservation; S4. After the solution treatment is completed, the material is rapidly cooled to avoid phase change or deformation during the cooling process; S5. Cryogenically treat the material in a low temperature environment and keep it warm at this temperature to further stabilize the internal structure of the material; S6. Performing a first heating treatment on the material and maintaining the temperature within a specified temperature range to improve the strength of the material through precipitation hardening; S7. The material is subjected to a second heating treatment and kept at a lower temperature range to optimize the mechanical properties and stability of the material, and then cooled naturally in the air.
2. The heat treatment process of the 17-7PH material according to claim 1, characterized in that: The step S1 of preliminarily heating to the intermediate temperature range controls the temperature between 600° C. and 700° C. and keeps the temperature for 1.5 hours.
3. The heat treatment process of the 17-7PH material according to claim 1, characterized in that: The higher temperature range heating step S2 controls the temperature between 800° C. and 900° C. and keeps the temperature for 1.5 hours.
4. The heat treatment process of the 17-7PH material according to claim 1, characterized in that: The heating step S3 in the target temperature range controls the temperature between 990° C. and 1010° C. and keeps the temperature for 2 hours.
5. The heat treatment process of the 17-7PH material according to claim 1, characterized in that: The rapid cooling step S4 uses nitrogen cooling to avoid phase change or deformation of the material during the cooling process.
6. The heat treatment process of the 17-7PH material according to claim 1, characterized in that: The cryogenic treatment step S5 cools the material to between -65°C and -80°C and keeps it at this temperature for 2 hours.
7. The heat treatment process of the 17-7PH material according to claim 1, characterized in that: The first temperature treatment step S6 heats the material to between 590° C. and 610° C., and keeps the temperature for 3 hours, and then quickly cools the material to below 15° C. and keeps the temperature for 30 minutes.
8. The heat treatment process of the 17-7PH material according to claim 1, characterized in that: The second temperature rising step S7 heats the material to between 390° C. and 410° C., and keeps the temperature for 1.5 hours, and finally cools it naturally in the air.
9. The heat treatment process of the 17-7PH material according to any one of claims 1 to 8, characterized in that: After each heat treatment stage, the material hardness, microstructure and deformation performance tests are carried out to ensure that the heat treatment effect meets the expected requirements.
Citation Information
Cited By
Heat treatment method of high-temperature molten salt corrosion resistant alloy for photo-thermal power generation equipment
CN120006194A