Resource recycling method for nickel-cobalt sulfide slag synergistic ternary battery black powder

Through microwave activation treatment of the collaborative leaching reaction of nickel sulfide cobalt slag and ternary battery black powder, combined with extraction and precipitation treatment, the problem of excessive use of external oxidants and reducing agents in the prior art is solved, and nickel, cobalt, manganese, The efficient recycling of lithium reduces production costs and wastewater treatment difficulty.

CN119061265AInactive Publication Date: 2024-12-03HUNAN ESSOKAI FUTURE ENERGY RES INST CO LTD

Patent Information

Application Number
CN202410775056.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, there are too many external oxidants and reducing agents used in the resource recycling process of nickel sulfide cobalt slag and ternary battery black powder, resulting in high production costs and low recycling efficiency, and it is difficult to achieve nickel, cobalt, manganese, lithium, etc. Efficient recycling of valuable metals.

Method used

Microwave activation treatment of nickel sulfide cobalt slag, destroying its crystal structure, activates the reaction site, and conducts a coordinated leaching reaction with the ternary battery black powder under acidic conditions, combining extraction and precipitation treatment to achieve the recovery of valuable metals and reduce external Use of additives.

Benefits of technology

It has achieved high recovery rates of nickel, cobalt, manganese and lithium, reduced production costs and consumption of raw and auxiliary materials, improved the economic value of resource recycling, and reduced the difficulty of subsequent debris removal and wastewater treatment.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a resource recovery method for nickel-cobalt sulfide slag synergistic ternary battery black powder. The method comprises the following steps: microwave activation treatment: carrying out microwave activation treatment on nickel-cobalt sulfide slag to generate sulfide lattice defects; leaching treatment: mixing the nickel-cobalt sulfide slag subjected to microwave activation treatment with ternary battery black powder, pulping, carrying out leaching reaction under an acidic condition, and carrying out solid-liquid separation after the reaction is completed, so as to obtain a leaching solution and leaching slag; impurity removal treatment: adding a neutralizer into the obtained leachate for impurity removal treatment, and filtering after treatment to obtain filtrate and filter residues; extraction treatment: carrying out extraction and back extraction on the obtained filtrate to obtain a solution containing nickel, cobalt and manganese and raffinate; performing heavy removal on the raffinate by a precipitator, and filtering to obtain a lithium-containing solution; and performing lithium precipitation treatment: adding a lithium precipitation agent into the lithium-containing solution to obtain a lithium salt product. According to the method, valuable metal in the nickel sulfide cobalt slag and the ternary battery black powder is recycled, the comprehensive recycling rate of nickel is larger than or equal to 98.45%, the recycling rate of cobalt is larger than or equal to 99.9%, the recycling rate of manganese is larger than or equal to 98.45%, and the recycling rate of lithium is larger than or equal to 98.64%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery recycling, and specifically to a method for recycling black powder of ternary batteries in a coordinated manner using nickel-cobalt sulfide slag. Background Art

[0002] Nickel cobalt sulfide slag is the tailings produced by sulfide impurity removal in the production process of metallurgy, battery materials, etc. Nickel cobalt sulfide slag contains a large amount of valuable metals such as nickel, cobalt, manganese and lithium. Most of the slag exists in the form of nickel sulfide, cobalt sulfide and manganese sulfide, which has important recovery value. Chinese patent No. CN114212806A discloses a method for recovering nickel cobalt manganese sulfide slag, which uses the method of adding an oxidant to oxidize the nickel cobalt manganese sulfide slag into nickel cobalt manganese sulfate with higher solubility, and then recovers it by acid leaching, but the recovery effect is not good. Chinese patent No. CN112575208A discloses a method for preparing high-purity manganese sulfate from electrolytic manganese nickel cobalt sulfide slag, which uses pyrolusite as an oxidant to mix with nickel cobalt sulfide slag, but oxygen still needs to be continuously introduced as an oxidant during the leaching process, the production cost is high, and the recovery efficiency is low.

[0003] The black mixture obtained after the waste nickel-cobalt-manganese ternary lithium battery is discharged, disassembled, crushed, sorted and separated is called ternary battery black powder. Ternary battery black powder contains a large amount of valuable metals such as nickel, cobalt, manganese and lithium. In the prior art, the valuable metals in the ternary battery black powder are usually recovered by hydrometallurgical process. The hydrometallurgical process includes an acid leaching process, that is, the battery powder reacts with water and sulfuric acid to obtain a leachate containing nickel, cobalt, manganese and lithium. However, due to the low solubility of high-priced nickel, cobalt and manganese in water, and how to fully reduce nickel, cobalt and manganese into more soluble +2-valent metal ions is the difficulty in research and development. In the prior art, the large amount of reducing agent added during the acid leaching process has a poor reduction effect and introduces impurities, affecting the purity of subsequent products.

[0004] In the prior art, there is no record of a process for fully recycling nickel-cobalt sulfide slag and ternary battery black powder. The present invention aims to develop a comprehensive recycling process for nickel-cobalt sulfide slag and ternary battery black powder to reduce the addition of external oxidants and reductants, reduce production costs and raw material consumption, while increasing the recovery rate of valuable metals such as nickel, cobalt, manganese, and lithium, and improving the economic value of resource recovery. Summary of the invention

[0005] The technical problem solved by the present invention is to provide a method for resource recovery of nickel-cobalt sulfide slag and ternary battery black powder, so as to reduce the addition of external oxidants and reductants, reduce production costs and raw material consumption, while increasing the recovery rate of valuable metals such as nickel, cobalt, manganese, and lithium, and improving the economic value of resource recovery.

[0006] The technical problem solved by the present invention is achieved by adopting the following technical solutions:

[0007] A method for recycling nickel-cobalt sulfide slag and ternary battery black powder, comprising the following steps:

[0008] Microwave activation treatment: subjecting the nickel-cobalt sulfide slag to microwave activation treatment to produce sulfide lattice defects;

[0009] Synergistic leaching treatment: The nickel-cobalt sulfide slag treated with microwave activation is mixed with the ternary battery black powder to make pulp and undergo leaching reaction under acidic conditions. After the reaction is completed, the solid-liquid separation is performed to obtain the leaching liquid and the leaching slag;

[0010] Impurity removal treatment: adding a neutralizing agent to the obtained leachate for impurity removal treatment, and filtering after treatment to obtain a filtrate and a filter residue;

[0011] Extraction treatment: extracting and stripping the obtained filtrate to obtain a nickel-cobalt-manganese solution and a raffinate; removing the weight of the raffinate with a precipitant to obtain a lithium-containing solution;

[0012] Lithium precipitation treatment: Add lithium precipitation agent to the lithium-containing solution to obtain lithium salt product.

[0013] Furthermore, the microwave activation treatment time is 0.5 to 4 hours, and the microwave power is 100 to 600W.

[0014] Furthermore, after microwave activation treatment, the obtained nickel-cobalt sulfide slag is ground to a particle size of less than 1 μm.

[0015] Furthermore, in the coordinated leaching step, the ratio of the nickel-cobalt sulfide slag to the ternary battery black powder is determined by the nickel, cobalt, and manganese contents in the ternary battery black powder and the S content in the nickel-cobalt sulfide slag. 2- The content is calculated according to the following chemical reaction equation: MeS+8LiMeO2+24H + =9Me 2+ +8Li + +12H2O+SO4 2- ; and the excess coefficient of nickel-cobalt sulfide slag is 0.95~1.05.

[0016] Furthermore, the solid-liquid ratio of the nickel-cobalt sulfide slag and the ternary battery black powder treated with microwave activation during slurrying is in the range of 3L / kg to 10L / kg, the leaching reaction temperature is 60°C to 100°C, the reaction pH value is 0 to 2.0, and the reaction time is 0.5h to 4h.

[0017] Furthermore, the neutralizing agent is one or more of alkaline metal oxides, hydroxides, ammonia water, hydrogen peroxide, or alkaline salts. After adding the neutralizing agent, the pH of the leachate is 4.5-5.5, the temperature during the impurity removal treatment is 25°C-99°C, and the time is 0.5-10h.

[0018] Furthermore, the extraction method is as follows: the extractant is HBL116 with a concentration of 20 to 40%, the extraction ratio range is 10:1.0 to 2.0, the extraction is carried out at room temperature, and the extraction time is 5 to 10 minutes; the stripping agent is 0.5 to 2 mol / L dilute sulfuric acid, the stripping ratio range is 10:1.0 to 2.0, and the stripping time is 5 to 10 minutes.

[0019] Furthermore, the precipitant is a sulfide salt or an alkaline pH regulator.

[0020] Furthermore, the lithium precipitation agent is a soluble salt of phosphate, fluoride or carbonate. During the lithium precipitation treatment, the reaction temperature is 60° C. to 99° C. and the reaction time is 0.5 to 10 hours.

[0021] Furthermore, during the lithium precipitation treatment process, the amount of lithium precipitation agent added is 1.05 to 1.2 times the theoretical amount.

[0022] Beneficial effects:

[0023] The method for resource recovery of nickel-cobalt sulfide slag and ternary battery black powder of the present invention utilizes microwave activation treatment to destroy the sulfide crystal structure in the nickel-cobalt sulfide slag, activates more reaction sites, and makes it have higher reaction activity. Therefore, during the leaching reaction, the oxidizing property of the ternary battery black powder is utilized, and the two fully undergo redox reaction to realize the recovery of valuable metals in the nickel-cobalt sulfide slag and the ternary battery black powder, and realize the comprehensive recovery rate of nickel ≥98.45%, the recovery rate of cobalt ≥99.9%, the recovery rate of manganese ≥98.45%, and the recovery rate of lithium ≥98.64%.

[0024] The nickel-cobalt sulfide slag and ternary battery black powder resource recovery method described in the present invention does not require the addition of external oxidants and reductants, reduces the cost of raw and auxiliary materials and reduces the introduction of external impurities, and the copper element in the ternary battery black powder does not enter the leaching solution, reducing the difficulty of subsequent copper removal.

[0025] The method for resource recovery of nickel-cobalt sulfide slag and ternary battery black powder described in the present invention generates wastewater that does not contain heavy metals such as nickel, cobalt, and manganese, which helps to reduce the difficulty of wastewater treatment. DETAILED DESCRIPTION

[0026] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments.

[0027] Example 1

[0028] In this embodiment, the ternary battery black powder is a solid powder obtained by crushing, pulverizing and roasting the ternary battery. The nickel-cobalt sulfide slag is the nickel and cobalt slag removed in the production process of battery-grade manganese sulfate. The main components of the nickel-cobalt sulfide slag are nickel sulfide, cobalt sulfide and manganese sulfide.

[0029] The method for recycling nickel-cobalt sulfide slag and ternary battery black powder includes the following steps:

[0030] Microwave activation treatment: The nickel-cobalt sulfide slag is subjected to microwave activation treatment. The microwave treatment power is 100W and the microwave treatment time is 2h. After the microwave treatment, sulfide lattice defects are generated in the nickel-cobalt sulfide slag, more active sites are excited, and the slag has higher reaction activity;

[0031] The nickel-cobalt sulfide slag is activated by microwave and then ground to a particle size D90 less than 1 μm.

[0032] Synergistic leaching treatment: Mix nickel cobalt sulfide slag with ternary battery black powder, and add the nickel cobalt sulfide slag and ternary battery black powder at a ratio of 1.0 times the theoretical value. Specifically, in this embodiment, according to ICP analysis, the concentrations of each element in the mixture are: nickel 18.43%, cobalt 5.06%, manganese 8.54%, and lithium 3.76%. 170g of the above mixture is slurried at a liquid-to-solid ratio of 4L / kg to obtain a mixed slurry. Under 80°C water bath conditions, sulfuric acid was added to the mixed slurry, and the pH value was controlled to be 1.0 after the addition of sulfuric acid. After leaching reaction for 2 hours, the mixture was filtered to obtain leaching residue and leaching solution. The weight of the leaching residue was 20.7g. The residual amounts of nickel, cobalt, manganese and lithium in the leaching residue were obtained by ICP detection. The contents of each element were 2.43% nickel, 0.04% cobalt, 1.09% manganese and 0.12% lithium. The leaching rates were 98.45% nickel, 99.9% cobalt, 98.45% manganese and 99.61% lithium. In addition, the leaching solution contained 0.02g / L copper, 2.22g / L iron and 2.83g / L aluminum.

[0033] Impurity removal treatment: sodium carbonate and hydrogen peroxide are added to the leachate to oxidize the ferrous ions that may exist in the solution through hydrogen peroxide. The pH of the leachate after adding sodium carbonate and hydrogen peroxide is 5.0. The temperature during the impurity removal treatment is 60°C and the time is 0.5h. The impurity removal treatment removes impurities such as iron and aluminum in the leachate. After impurity removal, the filtrate is filtered and the iron in the filtrate is reduced to 10ppm and the aluminum is reduced to 86ppm.

[0034] Extraction treatment: The obtained filtrate is extracted and stripped through a nickel-cobalt-manganese joint extraction system, the extractant is 30% HBL116, the extraction phase ratio O / A=10:1, the feed solution pH=2.0, room temperature, and the extraction time is 5 min; the stripping agent is 1 mol / L dilute sulfuric acid, the stripping phase ratio O / A=5:1, room temperature, and the extraction time is 5 min. The final stripping solution concentration is a nickel-cobalt-manganese solution, wherein Ni: 22.65g / L, Co: 6.31g / L, Mn: 10.51g / L, which can be used as a raw material for a nickel-cobalt-manganese ternary precursor, and the extractant can be recycled after regeneration;

[0035] Sodium hydroxide is added to the raffinate to remove heavy metals, and the lithium-containing solution and the heavy metal-free slag are obtained by filtration; the heavy metal elements such as nickel, cobalt and manganese in the lithium-containing solution are all less than 0.5 ppm by ICP detection, and the element contents in the heavy metal-free slag are 3.73% nickel, 0.21% cobalt, 3.39% manganese and 0.25% lithium respectively;

[0036] Lithium precipitation treatment: add 1.4 times the theoretical amount of saturated sodium phosphate solution to the lithium-containing solution, keep it at 60°C for 0.5h, and filter to obtain filtrate and residue; after testing, the lithium concentration in the filtrate is 0.1g / L, and the lithium precipitation rate is calculated to be 99.03%. The obtained residue is lithium phosphate with a purity of 98.01%, which meets the requirements of industrial-grade products.

[0037] In the acid leaching process of this embodiment, no additional oxidant and reductant are needed, and the leaching rates of nickel, cobalt, manganese and lithium are relatively high; the black powder of the ternary battery exhibits strong oxidizability under acid leaching conditions, and S 2- Ions have strong reducing properties. The activated nickel-cobalt sulfide slag has more active sites and higher reaction activity. It can make more sufficient contact with the heavy metals in the ternary battery black powder and undergo redox reactions. The nickel-cobalt sulfide slag will not promote the leaching of copper in the ternary battery black powder. Therefore, the solution can reduce the difficulty of impurity removal in subsequent processes. In the de-heaving process, adding sodium hydroxide as a de-heaving agent can effectively remove heavy metal ions in the raffinate on the one hand, and on the other hand, the de-heaving slag can be returned to the front end as a raw material for leaching without causing the loss of valuable metals. The wastewater generated does not contain heavy metals such as nickel, cobalt, and manganese, which helps to reduce the difficulty of wastewater treatment.

[0038] After calculation, in this embodiment, the comprehensive recovery rate of nickel in the raw material is 98.32%, the recovery rate of cobalt is 99.76%, the recovery rate of manganese is 98.45%, and the recovery rate of lithium is 98.64%.

[0039] Example 2

[0040] In this embodiment, the ternary battery black powder is a solid powder obtained by crushing, pulverizing and roasting the ternary battery. The nickel-cobalt sulfide slag is the nickel and cobalt slag removed in the production process of battery-grade manganese sulfate. The main components of the nickel-cobalt sulfide slag are nickel sulfide, cobalt sulfide and manganese sulfide.

[0041] The method for recycling nickel-cobalt sulfide slag and ternary battery black powder includes the following steps:

[0042] Microwave activation treatment: The nickel-cobalt sulfide slag is subjected to microwave activation treatment. The microwave treatment power is 600W and the microwave treatment time is 0.5h. After the microwave treatment, sulfide lattice defects are generated in the nickel-cobalt sulfide slag, more active sites are excited, and the reaction activity is higher;

[0043] The nickel-cobalt sulfide slag is activated by microwave and then ground to a particle size D90 less than 1 μm.

[0044] Synergistic leaching treatment: Mix nickel cobalt sulfide slag with ternary battery black powder, and add the nickel cobalt sulfide slag to ternary battery black powder at a ratio of 1.0 times the theoretical value. Specifically, in this embodiment, according to ICP analysis, the concentrations of each element in the mixture are: nickel 18.43%, cobalt 5.06%, manganese 8.54%, and lithium 3.76%. 170g of the above mixture is slurried at a solid-liquid ratio of 4kg / L to obtain a mixed slurry. Under 60°C water bath conditions, sulfuric acid was added to the mixed slurry, and the pH value was controlled to be 2.0 after the addition of sulfuric acid. After leaching reaction for 2 hours, the mixture was filtered to obtain leaching residue and leaching solution. The weight of the leaching residue was 25.1 g. The residual amounts of nickel, cobalt, manganese and lithium in the leaching residue were obtained by ICP detection. The contents of each element were 2.21% nickel, 0.06% cobalt, 1.41% manganese and 0.12% lithium. The leaching rates were 98.23% nickel, 99.8% cobalt, 97.56% manganese and 99.53% lithium. In addition, the leaching solution contained 0.02 g / L copper, 2.31 g / L iron and 1.96 g / L aluminum.

[0045] Impurity removal treatment: sodium carbonate and hydrogen peroxide are added to the leachate. The pH of the leachate after adding sodium carbonate and hydrogen peroxide is 5.0. The temperature during the impurity removal treatment is 60°C and the time is 0.5h. The impurity removal treatment removes impurities such as iron and aluminum in the leachate. After impurity removal, the filtrate is filtered and the iron in the filtrate is reduced to 12ppm and the aluminum is reduced to 73ppm.

[0046] Extraction treatment: The obtained filtrate is extracted and stripped through a nickel-cobalt-manganese joint extraction system, the extractant is 35% HBL116, the extraction phase ratio O / A=10:1, the feed solution pH=2.0, room temperature, and the extraction time is 5 min; the stripping agent is 0.6 mol / L dilute sulfuric acid, the stripping phase ratio O / A=5:1, room temperature, and the extraction time is 5 min. The final stripping solution concentration is Ni: 22.4 g / L, Co: 6.25 g / L, Mn: 10.31 g / L, and the extractant can be recycled after regeneration;

[0047] Sodium hydroxide is added to the raffinate to remove heavy metals, and the lithium-containing solution and the heavy metal-free slag are obtained by filtration; the heavy metal elements such as nickel, cobalt and manganese in the lithium-containing solution are all less than 0.5 ppm by ICP detection, and the element contents in the heavy metal-free slag are 2.51% nickel, 0.18% cobalt, 3.01% manganese and 0.23% lithium respectively;

[0048] Lithium precipitation treatment: add saturated sodium carbonate solution at 1.4 times the theoretical amount to the lithium-containing solution, keep warm at 60°C for 0.5h, and filter to obtain filtrate and residue; after testing, the lithium concentration in the filtrate is 2.31g / L, and the calculated lithium precipitation rate is 73.51%. The obtained residue is 98.05% lithium carbonate, which meets the requirements of industrial-grade products.

[0049] After calculation, in this embodiment, the comprehensive recovery rate of nickel in the raw material is 97.23%, the recovery rate of cobalt is 98.81%, the recovery rate of manganese is 96.58%, and the recovery rate of lithium is 73.16%. The obtained lithium precipitation mother liquor can be returned to the leaching process without causing lithium loss.

[0050] Comparative Example 1

[0051] The black powder of ternary battery is the solid powder obtained by crushing, pulverizing and roasting the ternary battery. The nickel-cobalt sulfide slag is the slag without nickel and cobalt in the production process of battery-grade manganese sulfate. The main components of the nickel-cobalt sulfide slag are nickel sulfide, cobalt sulfide and manganese sulfide.

[0052] The method for recycling nickel-cobalt sulfide slag and ternary battery black powder includes the following steps:

[0053] Microwave activation treatment: The nickel-cobalt sulfide slag is subjected to microwave activation treatment, the microwave treatment power is 100W, the microwave treatment time is 4h, and after the microwave treatment is completed, sulfide lattice defects are generated in the nickel-cobalt sulfide slag;

[0054] The nickel-cobalt sulfide slag is activated by microwave and then ground to a particle size D90 less than 1 μm.

[0055] Synergistic leaching treatment: Mix nickel cobalt sulfide slag with ternary battery black powder, the ratio of nickel cobalt sulfide slag to ternary battery black powder is calculated according to the nickel, cobalt, manganese content in the ternary battery black powder and the S2- content in the nickel cobalt sulfide slag, and the nickel cobalt sulfide slag is 0.65 times the theoretical amount. Specifically, in this embodiment, according to ICP analysis, the concentrations of each element in the mixture are: nickel 21.29%, cobalt 5.03%, manganese 7.75%, lithium 4.38%. 150g of the above mixture is slurried at a liquid-to-solid ratio of 4L / kg to obtain a mixed slurry. Under 80°C water bath conditions, sulfuric acid was added to the mixed slurry. After adding sulfuric acid, the pH value was controlled to be 1.0, and 40mL of hydrogen peroxide was added. After leaching reaction for 2h, the mixture was filtered to obtain leaching residue and leaching solution. The weight of the leaching residue was 15.3g. The residual amounts of nickel, cobalt, manganese and lithium in the leaching residue were obtained by ICP detection, and the leaching rates of each element were 99.16% for nickel, 99.5% for cobalt, 98.98% for manganese and 99.71% for lithium. In addition, the leaching solution contained 1.9g / L copper, 2.02g / L iron and 3.19g / L aluminum.

[0056] Impurity removal treatment: iron powder is added to the leachate to remove copper, and then sodium carbonate and hydrogen peroxide are added. The pH of the leachate after adding sodium carbonate and hydrogen peroxide is 5.0. The temperature during the impurity removal treatment is 60°C and the time is 0.5h. The impurity removal treatment removes impurities such as iron and aluminum in the leachate. After impurity removal, the filtrate is filtered and the iron in the filtrate is reduced to 10ppm and the aluminum is reduced to 102ppm.

[0057] The subsequent treatment is the same as in Example 1.

[0058] During the acid leaching process of this comparative example, after reducing the amount of nickel cobalt sulfide slag added during the leaching process, adding some hydrogen peroxide as a reducing agent can still obtain a higher leaching rate of valuable metals. However, in the presence of hydrogen peroxide, the copper ion content in the leachate increases, resulting in an increase in the subsequent impurity removal procedures.

[0059] Comparative Example 2

[0060] The black powder of ternary battery is the solid powder obtained by crushing, pulverizing and roasting the ternary battery. The nickel-cobalt sulfide slag is the slag without nickel and cobalt in the production process of battery-grade manganese sulfate. The main components of the nickel-cobalt sulfide slag are nickel sulfide, cobalt sulfide and manganese sulfide.

[0061] The method for recycling nickel-cobalt sulfide slag and ternary battery black powder includes the following steps:

[0062] Microwave activation treatment: The nickel-cobalt sulfide slag is subjected to microwave activation treatment. The microwave treatment power is 100W and the microwave treatment time is 4 hours. After the microwave treatment, sulfide lattice defects are generated in the nickel-cobalt sulfide slag, and more active sites are excited, which has higher reaction activity;

[0063] The nickel-cobalt sulfide slag was directly ground to a particle size D90 less than 1 μm without microwave activation.

[0064] Synergistic leaching treatment: Mix nickel cobalt sulfide slag with ternary battery black powder, and add nickel cobalt sulfide slag and ternary battery black powder at a ratio of 1.42 times the theoretical amount. Specifically, in this embodiment, according to ICP analysis, the concentrations of each element in the mixture are: nickel 15.94%, cobalt 5.09%, manganese 9.23%, and lithium 3.13%. 200g of the above mixture is slurried at a solid-liquid ratio of 4kg / L to obtain a mixed slurry. Under 80°C water bath conditions, sulfuric acid was added to the mixed slurry, and the pH value was controlled to be 1.0 after the addition of sulfuric acid. After leaching reaction for 2 hours, the mixture was filtered to obtain leaching residue and leaching solution. The weight of the leaching residue was 49.3g. The residual amounts of nickel, cobalt, manganese and lithium in the leaching residue were obtained by ICP detection, and the contents of each element were 2.34% nickel, 3.26% cobalt, 6.48% manganese and 0.15% lithium, respectively. The leaching rates of each element were 96.38% nickel, 84.21% cobalt, 82.69% manganese and 98.82% lithium. In addition, the leaching solution contained 0.11g / L copper, 1.31g / L iron and 2.09g / L aluminum.

[0065] The leaching rates of nickel, cobalt and manganese decreased, and the control experiment was terminated.

[0066] In the acid leaching process of this control example, although the sulfide slag can react with the ternary black powder after microwave activation, the sulfide slag is added in excess and the remaining sulfide slag does not react directly with the acid, and the ideal leaching rate cannot be achieved.

[0067] Comparative Example 3

[0068] The black powder of ternary battery is the solid powder obtained by crushing, pulverizing and roasting the ternary battery. The nickel-cobalt sulfide slag is the slag without nickel and cobalt in the production process of battery-grade manganese sulfate. The main components of the nickel-cobalt sulfide slag are nickel sulfide, cobalt sulfide and manganese sulfide.

[0069] The method for recycling nickel-cobalt sulfide slag and ternary battery black powder includes the following steps:

[0070] Microwave activation treatment: The nickel-cobalt sulfide slag is subjected to microwave activation treatment. The microwave treatment power is 50W and the microwave treatment time is 10min.

[0071] The nickel-cobalt sulfide slag is activated by microwave and then ground to a particle size D90 less than 1 μm.

[0072] Synergistic leaching treatment: Mix nickel cobalt sulfide slag with ternary battery black powder, and the ratio of nickel cobalt sulfide slag to ternary battery black powder is 1.0 times the theoretical amount. Specifically, in this embodiment, according to ICP analysis, the concentrations of each element in the mixture are: nickel 18.43%, cobalt 5.06%, manganese 8.54%, and lithium 3.76%. 170g of the above mixture is slurried at a liquid-to-solid ratio of 4L / kg to obtain a mixed slurry. Under 80°C water bath conditions, sulfuric acid was added to the mixed slurry, and the pH value was controlled to be 1.0 after the addition of sulfuric acid. After leaching reaction for 2 hours, the mixture was filtered to obtain leaching residue and leaching solution. The weight of the leaching residue was 92.6g. The residual amounts of nickel, cobalt, manganese and lithium in the leaching residue were determined by ICP test. The contents of each element were 11.41% for nickel, 4.57% for cobalt, 5.83% for manganese and 1.68% for lithium, respectively. The leaching rates of each element were 66.27% for nickel, 50.77% for cobalt, 62.84% for manganese and 75.64% for lithium. In addition, the leaching solution contained 0.03g / L copper, 1.94g / L iron and 2.50g / L aluminum.

[0073] The leaching rates of nickel, cobalt, manganese and lithium were low, so the control experiment was terminated.

[0074] In this control example, the microwave activation power is low and the activation time is short. Under the same conditions, the reaction rate with the black powder of the ternary battery as a reducing agent is greatly reduced, and the high-value recovery of nickel, cobalt, manganese and lithium cannot be achieved.

[0075] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for recycling nickel-cobalt sulfide slag and ternary battery black powder, It is characterized in that The steps include: Microwave activation treatment: subjecting the nickel-cobalt sulfide slag to microwave activation treatment to produce sulfide lattice defects; Leaching treatment: The nickel-cobalt sulfide slag treated with microwave activation is mixed with the ternary battery black powder to make pulp and then leached under acidic conditions. After the reaction is completed, the solid-liquid separation is performed to obtain the leachate and the leaching slag; Impurity removal treatment: adding a neutralizing agent to the obtained leachate for impurity removal treatment, and filtering after treatment to obtain a filtrate and a filter residue; Extraction treatment: extracting and stripping the obtained filtrate to obtain a nickel-cobalt-manganese solution and a raffinate; the raffinate is deweighted by a precipitant and then filtered to obtain a lithium-containing solution; Lithium precipitation treatment: Add lithium precipitation agent to the lithium-containing solution to obtain lithium salt product.

2. The method for recycling nickel-cobalt sulfide slag and ternary battery black powder according to claim 1, It is characterized in that The microwave activation treatment time is 0.5 to 4 hours, and the microwave power is 100 to 600W.

3. The method for recycling nickel-cobalt sulfide slag and ternary battery black powder according to claim 1, It is characterized in that After microwave activation treatment, the obtained nickel-cobalt sulfide slag is ground to a particle size of less than 1 μm.

4. The method for recycling nickel-cobalt sulfide slag and ternary battery black powder according to claim 1, It is characterized in that In the coordinated leaching step, the ratio of nickel-cobalt sulfide slag to ternary battery black powder is determined by the nickel, cobalt, and manganese contents in the ternary battery black powder and the S content in the nickel-cobalt sulfide slag. 2- The content is calculated according to the following chemical reaction equation: MeS+8LiMeO 2 +24H + =9Me 2+ +8Li + +12H 2 O+SO 4 2- ; and the excess coefficient of nickel-cobalt sulfide slag is 0.95~1.

05.

5. The method for recycling nickel-cobalt sulfide slag and ternary battery black powder according to claim 1, It is characterized in that The solid-liquid ratio of the nickel-cobalt sulfide slag and the ternary battery black powder treated with microwave activation during slurry preparation is in the range of 3L / kg to 10L / kg, the leaching reaction temperature is 60°C to 100°C, the reaction pH value is 0 to 2.0, and the reaction time is 0.5h to 4h.

6. The method for recycling nickel-cobalt sulfide slag and ternary battery black powder according to claim 1, It is characterized in that The neutralizing agent is one or more of alkaline metal oxides, hydroxides, ammonia water, hydrogen peroxide, or alkaline salts. After adding the neutralizing agent, the pH of the leaching solution is 4.5-5.

5. The temperature during the impurity removal treatment is 25°C-99°C and the time is 0.5-10h.

7. The method for recycling nickel-cobalt sulfide slag and ternary battery black powder according to claim 1, It is characterized in that The extraction method is as follows: the extractant is HBL116 with a concentration of 20-40%, the extraction phase ratio range is 10:1.0-2.0, the extraction is carried out at room temperature, and the extraction time is 5-10 minutes; the stripping agent is 0.5-2 mol / L dilute sulfuric acid, the stripping phase ratio range is 10:1.0-2.0, and the stripping time is 5-10 minutes.

8. The method for recycling nickel-cobalt sulfide slag and ternary battery black powder according to claim 7, It is characterized in that After the extraction is completed, the precipitant used is a sulfide salt or an alkaline pH regulator.

9. The method for recycling nickel-cobalt sulfide slag and ternary battery black powder according to claim 1, It is characterized in that The lithium precipitation agent is a soluble salt of phosphate, fluoride or carbonate. During the lithium precipitation treatment process, the reaction temperature is 60° C. to 99° C. and the reaction time is 0.5 to 10 hours.

10. The method for recycling nickel-cobalt sulfide slag and ternary battery black powder according to claim 9, It is characterized in that During the lithium precipitation treatment process, the amount of lithium precipitation agent added is 1.05 to 1.2 times the theoretical amount.

Citation Information

Patent Citations

  • Method for synergistically preparing ternary precursor and lithium carbonate by utilizing waste lithium ion battery black powder and nickel-cobalt sulfide ore and application

    CN112250120A

  • Recycling method for ternary positive electrode powder of nickel cobalt lithium manganate

    CN112831662A

  • Method for directly preparing ternary precursor through co-extraction of nickel, cobalt and manganese in laterite-nickel ore high-pressure leachate

    CN115818732A

Cited By

  • Method for auxiliary leaching of waste lithium ion batteries by using sulphide ore

    CN119852576A

  • Co-treatment method of waste lithium battery pole powder and sulfide slag waste

    CN120818689A

  • Co-processing method of waste lithium battery pole powder and vulcanized slag waste

    CN120818689B