Pipe material, method for manufacturing pipe material, stent, guidewire, and pressure guidewire
In the manufacturing process of Ni-Ti alloy pipes, the problems of inner wall roughness and core removal accuracy of thin-diameter pipes are solved by using melting/forging, hot processing and drawing processing steps, combined with tensile load and annealing treatment. , realizes high-precision, ultra-elastic and high-durability pipes, meeting the strict specifications of medical devices.
Patent Information
- Application Number
- CN202480002288.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-25
- Publication Date
- 2024-12-03
AI Technical Summary
In the prior art, when manufacturing Ni-Ti alloy pipes, especially thin-diameter pipes, it is difficult to achieve industrial improvement of inner wall roughness and core removal steps, resulting in insufficient durability of the pipes in rotational bending and difficult to meet medical conditions. Strict specifications for carbon and oxygen concentrations in the instrument.
Using Ni-Ti alloy material, through melting/forging, hot processing, drawing processing and core removal steps, combined with tensile load and annealing treatment, the inner wall roughness of the pipe is controlled to be above 0.08μm and below 0.55μm, and the outer diameter is The inner diameter ratio is above 1.01 and below 5.00 to ensure that the pipe has super elastic properties, and reduce scratches and gaps on the inner wall surface through the optimized core removal step.
The industrial manufacturing of Ni-Ti alloy pipes has been realized, which significantly improves the roughness of the inner wall, improves the durability of rotation and bending, meets the high precision and durability requirements of medical devices, and controls the concentration range of carbon and oxygen.
Smart Images

Figure CN119072551A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a tube and a method for manufacturing the tube, as well as a stent, a guide wire and a pressure guide wire. Background Art
[0002] Ni-Ti alloy materials have excellent corrosion resistance and wear resistance. In addition, it is known that Ni-Ti alloy materials show shape memory characteristics and superelastic characteristics, and have special properties, that is, they can withstand more than 5% of the residual deformation of general metals and can return to their original shape without plastic deformation. Furthermore, it is known that Ni-Ti alloy materials show tolerance to repeated deformation under a certain strain state.
[0003] In recent years, with the progress of technology for processing Ni-Ti alloy materials into ultra-fine wires and thin tubes, the application of Ni-Ti alloy materials in medical devices such as stents, artificial heart valves, and guide wires for inserting stents and catheters into the body is expanding.
[0004] Among medical devices, stents and artificial heart valves are called indwelling devices. They are devices with high requirements for many characteristics. Since they are subjected to repeated loads of contraction / expansion caused by the pulsation of blood vessels in the body, they are expected to have excellent fatigue durability for a long period of more than 10 years.
[0005] On the other hand, the use of medical devices that are different from the above-mentioned medical devices, that is, devices that are not indwelling type but disposable type (hereinafter also referred to as disposables (Dispos)), has also been greatly expanded. The use of disposables is mostly to remove the blocked part of a small-diameter blood vessel. In order to make the device pass through the blood vessel and reach the affected part, it is necessary to rotate or bend the device. In addition, there are many methods in which a wire or other device is inserted into the inside of the pipe after the device reaches the affected part.
[0006] In view of this background, particularly in pipes, fracture resistance to rotational bending is required. In addition, in the use of inserting other equipment inside the pipe, since it is required to improve the operability such as being able to smoothly insert other equipment inside the pipe, the state of the inner wall surface of the pipe becomes important.
[0007] Furthermore, various studies have been made conventionally on pipe materials composed of Ni—Ti alloys.
[0008] For example, in Patent Documents 1 and 2, inventions were made from the viewpoint that it is important to improve the roughness of the inner wall surface of a pipe. Furthermore, based on these technologies, in Non-Patent Documents 1 and 2, pipes with an outer diameter of 4 mm or less and good inner wall surface roughness were successfully obtained.
[0009] However, in summary of non-patent documents 1 and 2, in order to obtain a thin tube with an outer diameter of 4 mm or less with a good inner wall surface, fixed mandrel drawing is performed at the stage of an outer diameter of 4 mm or more, and mandrel drawing is performed at the stage of an outer diameter of 4 mm or less. As such, since different steps need to be used simultaneously, it is difficult to industrially manufacture a long thin-diameter tube.
[0010] In addition, in Patent Document 1, which uses a core composed of a shape memory alloy, a pipe having an inner wall surface of 20s (arithmetic mean roughness Ra of about 5 μm) or less is obtained, and in Patent Document 2, which performs a traveling mandrel drawing method known as a method for producing a long pipe, a pipe having an inner wall surface of 5s (arithmetic mean roughness Ra of about 1.25 μm) or less is obtained. However, for the pipes of Patent Documents 1 and 2 to be used for the above-mentioned purposes, the roughness of the inner wall surface of the pipe is large, and there is room for further improvement.
[0011] Here, an overview of the prior art related to the manufacturing method of a tube composed of a shape memory alloy is described. Patent documents 3 and 4 describe a manufacturing method in which a core composed of a shape memory alloy is inserted into a metal tube and processed as a whole. By inserting the cold-processed core into the metal tube and heating it, the gap between the metal tube and the core becomes the smallest, and a composite material is formed by integrating the metal tube and the core. The metal tube (tube) can be processed to the target size in the state of the composite material, so that the outer diameter and wall thickness can be controlled. High-dimensional precision tubes with high dimensional accuracy can be manufactured industrially. Afterwards, in order to obtain a tube processed to the target size, it is necessary to remove the core from the tube. In patent documents 3 and 4, it is necessary to heat the entire processed composite material to 750-825°C, or only the core is electrically heated to remove the strain of the core by heating, and then the core is pulled out by a drawing machine, thereby the core is elongated and reduced in diameter, so that the core can be removed from the tube.
[0012] In addition, Patent Documents 5 and 6 describe a method of inserting a core made of mild steel, carbon steel, stainless steel, brass, etc. into a tube made of a shape memory alloy to make a composite material, and then processing the composite material as an integrated whole. In Patent Documents 5 and 6, as a method of removing the core, if the composite material is heated after processing, only the seamless tube material expands greatly due to thermal expansion, and a gap (hereinafter also referred to as a void) appears between the tube material and the core. Due to the generation of this void, the core can be removed from the tube material.
[0013] Although Patent Documents 3 to 6 are effective technologies for manufacturing pipes, there is still room for improvement in the manufacture of thin-diameter pipes of less than 4 mm. In particular, in the core removal step, especially in the case of thin-diameter pipes, the accuracy of the gap and whether the pipe and the core are effectively separated become key points in the industry. For example, the following problem is confirmed: when the core is pulled out from the pipe in a state where the gap is insufficient or the separation of the pipe and the core is insufficient, stripes in the longitudinal direction of the pipe appear on the inner wall surface of the pipe.
[0014] In addition, the above-mentioned technologies are all technologies developed before 2004. Therefore, there is still room for improvement in terms of being able to adapt to the conditions of ASTM F2063-18 (Standard Specification for Wrought Nickel-Titanium Shape Memory Alloys for Medical Device and Surgical Implants) specified in medical Ni-Ti alloys. When used in medical devices, the above-mentioned specifications are required not only in indwelling types, but also in disposables. In particular, the allowable amounts of carbon concentration and oxygen concentration are both revised to a maximum of 0.04% by mass, and the ranges for controlling carbon concentration and oxygen concentration are narrower than before the above-mentioned specifications. Therefore, it is necessary to develop a technology that realizes the rationalization of manufacturing conditions for controlling the concentrations of these elements while manufacturing thin-diameter tubing.
[0015] Furthermore, in the prior art, when evaluating the roughness of the inner wall surface, the arithmetic mean roughness Ra measured linearly along the long side direction of the pipe is evaluated, so the influence of the roughness of the scratches formed in the long side direction of the pipe cannot be quantitatively determined. Therefore, there is room for improvement in the evaluation technology of the roughness of the inner wall surface of the pipe.
[0016] In summary, there is a need for a pipe material composed of a Ni—Ti alloy, which can be manufactured by an industrially easy method and has improved roughness of the inner wall surface.
[0017] [Prior Technical Literature]
[0018] (Patent Document)
[0019] Patent Document 1: Japanese Patent Application Laid-Open No. 10-17963
[0020] Patent Document 2: Japanese Patent Application Laid-Open No. 11-61301
[0021] Patent Document 3: U.S. Patent No. 5709021
[0022] Patent Document 4: U.S. Patent No. 6799357
[0023] Patent Document 5: Japanese Patent No. 3443206
[0024] Patent Document 6: Japanese Patent No. 2133478
[0025] (Non-patent literature)
[0026] Non-patent document 1: Journal of Materials Processing Technology; 118 (2001); p.251-255 (J. Materials Processing Technology, 118 (2001), p.251-255)
[0027] Non-patent document 2: Journal of Materials Processing Technology, 153-154 (2004), p.145-150 Summary of the invention
[0028] [Problems to be solved by the invention]
[0029] The purpose of the present disclosure is to provide a tube and a method for manufacturing the tube, as well as a stent, a guide wire and a pressure guide wire using the tube, which can be industrially manufactured by an easy method, are composed of Ni-Ti alloy materials, have improved inner wall surface roughness, and have excellent durability against rotational bending.
[0030] [Technical means to solve the problem]
[0031] [1] A pipe material made of a Ni-Ti alloy, wherein an arithmetic mean height Sa of an inner wall surface is not less than 0.08 μm and not more than 0.55 μm.
[0032] [2] The pipe material according to [1] above, comprising 54.5 mass % or more and 57.0 mass % or less of Ni, with the remainder being Ti and unavoidable impurities.
[0033] [3] The pipe material according to [1] or [2] above, wherein the ratio of the outer diameter to the inner diameter of the pipe material (outer diameter / inner diameter) is 1.01 or more and 5.00 or less.
[0034] [4] The pipe according to any one of [1] to [3] above, wherein the outer diameter of the pipe is greater than or equal to 0.15 mm and less than or equal to 4.00 mm, and the inner diameter of the pipe is greater than or equal to 0.10 mm and less than or equal to 3.95 mm.
[0035] [5] The pipe according to any one of [1] to [4] above, which has superelastic properties at 37°C.
[0036] [6] A stent formed from the tube material according to any one of [1] to [5] above.
[0037] [7] A guide wire formed from the tube material according to any one of [1] to [5] above.
[0038] [8] A pressure guide wire formed from the tube material according to any one of [1] to [5] above.
[0039] [9] A method for manufacturing a pipe, which is the method for manufacturing a pipe according to any one of [1] to [5] above, comprising: a step of melting / forging a Ni-Ti alloy raw material (step 1); a hot working step (step 2); a drawing step (step 3), wherein a composite material obtained by inserting a core into the tubular Ni-Ti alloy hot-worked material obtained in the hot working step (step 2) is drawn to obtain a drawn composite material in which a tubular Ni-Ti alloy drawn material and a drawn core extending into the interior of the Ni-Ti alloy drawn material are integrated; and a core removal step (step 4), wherein the Ni-Ti alloy drawn material is heated to a temperature of not less than 150° C. and not more than 800° C. while applying a tensile load of such magnitude to the drawn core in the drawn composite material that the Ni-Ti alloy drawn material in the drawn composite material does not peel off from the drawn core.
[0040]
[10] The method for manufacturing a pipe material according to the above [9], wherein in the core removal step (step 4), the Ni-Ti alloy drawn material is heated to a temperature of 150° C. to 800° C. while a tensile load of 4 MPa to 300 MPa is applied to the drawn core material in the drawn composite material.
[0041]
[11] The method for manufacturing a tube according to the above [9] or
[10] , further comprising a heat treatment step (step 5) for imparting superelasticity, which is performed after the core removal step (step 4), and the tube is heated to impart superelasticity.
[0042] (Effects of the Invention)
[0043] According to the present disclosure, a tube and a method for manufacturing the tube, as well as a stent, a guide wire and a pressure guide wire using the tube can be provided, which can be industrially manufactured by an easy method, are composed of a Ni-Ti alloy material, have improved roughness of the inner wall surface, and have excellent durability against rotational bending. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 It is a perspective view showing an example of a pipe material according to an embodiment.
[0045] Figure 2 It is a cross-sectional view showing an example of the tensile load applying step (step 4-1).
[0046] Figure 3 It is a cross-sectional view showing another example of the tensile load applying step (step 4-1).
[0047] Figure 4 It is a drawing pair Figure 2 The cross-sectional view of the drawn composite material having the structure shown is a state after the annealing step (step 4-2).
[0048] Figure 5 It is a drawing pair Figure 3 The cross-sectional view of the drawn composite material having the structure shown is a state after the annealing step (step 4-2).
[0049] Figure 6 It is a cross-sectional view showing an example of the core diameter reduction step (4-3).
[0050] Figure 7 This is a cross-sectional view showing an example of the core extraction step (step 4-4).
[0051] Figure 8 It is a schematic diagram showing a double-drive type rotary bending fatigue testing machine used in Examples and Comparative Examples.
[0052] Fig. 9 These are the results of observing the inner wall surface of the pipe produced in Example 1 using a three-dimensional (3D) measurement laser microscope.
[0053] Fig.10 These are the results of observing the inner wall surface of the pipe produced in Example 10 using a 3D measurement laser microscope.
[0054] Fig.11 These are the results of observing the inner wall surface of the pipe produced in Comparative Example 6 using a 3D measurement laser microscope. DETAILED DESCRIPTION
[0055] The following is a detailed description based on the implementation modes.
[0056] The inventors of the present invention have been actively conducting research and have found a manufacturing method that can improve the roughness of the inner wall surface of a pipe without performing conventional steps such as floating mandrel drawing, fixed mandrel drawing, and mandrel drawing, and physically or chemically treating the inner wall surface of the pipe by grinding. Furthermore, the inventors have found that by improving the roughness of the inner wall surface of the pipe, excellent durability against rotational bending can be obtained. The present disclosure was completed based on the above findings.
[0057] The pipe material of the embodiment is made of a Ni—Ti alloy, and the arithmetic mean height Sa of the inner wall surface is 0.08 μm or more and 0.55 μm or less.
[0058] Figure 1 It is a perspective view showing an example of a pipe material according to an embodiment. Figure 1 The pipe material 1 shown in FIG. 1 is composed of a Ni—Ti alloy, and the arithmetic mean height Sa of the inner wall surface 1 a is 0.08 μm or more and 0.55 μm or less.
[0059] If the upper limit of the arithmetic mean height Sa of the inner wall surface 1a of the pipe 1 is 0.55 μm or less, the roughness of the inner wall surface 1a will be improved, and the pipe 1 can have excellent durability against rotational bending. From this point of view, the arithmetic mean height Sa of the inner wall surface 1a of the pipe 1 is 0.55 μm or less, preferably 0.45 μm or less, and the smaller the better. In addition, the lower limit of the arithmetic mean height Sa of the inner wall surface 1a is 0.08 μm or more from the perspective of ease of processing.
[0060] The arithmetic mean height Sa is a parameter obtained by extending the calculated average roughness Ra of the line measurement used in the general roughness evaluation to the surface. After the pipe 1 is cut longitudinally along the long side direction, the inner wall surface 1a of the pipe 1 is measured using a 3D measurement laser microscope, thereby obtaining the arithmetic mean height Sa of the inner wall surface 1a.
[0061] The pipe material 1 composed of a Ni-Ti alloy is mainly composed of a parent phase (matrix) (not shown) and a plurality of non-metallic inclusions (not shown) present in the parent phase. In addition, the pipe material 1 preferably has superelastic properties.
[0062] In order to improve the workability, the pipe material 1 preferably contains 54.5 mass % or more and 57.0 mass % or less of Ni (nickel), and the remainder is composed of Ti (titanium) and inevitable impurities. In this alloy composition, if the content ratio of C (carbon) contained in the pipe material 1 is 0.04 mass % or less, and the content ratio of O (oxygen) is 0.04 mass % or less, the pipe material 1 is suitable for the conditions of ASTM F2063-18 specified in Ni-Ti alloys for medical use, and therefore the pipe material 1 can be used for medical purposes.
[0063] Ni is an element necessary for exerting superelasticity and shape memory properties in Ni-Ti alloys. If the Ni content is outside the range of 54.5 mass % or more and 57.0 mass % or less, it is not easy to process the tube shape. Therefore, in the case of attaching importance to processability, the lower limit of the Ni content is preferably 54.5 mass % or more, more preferably 55.6 mass % or more, and the upper limit is preferably 57.0 mass % or less, more preferably 56.7 mass % or less.
[0064] C is an element that forms non-metallic inclusions. If the C content is high, the number of non-metallic inclusions present in the parent phase increases, and the occupancy rate of non-metallic inclusions in the pipe 1 increases, so that early fracture (fracture at a small number of rotations) of the pipe 1 is likely to occur. Therefore, the lower the C content, the more preferable. In particular, based on the provisions of ASTM F2063-18, the C content is preferably 0.04 mass% or less.
[0065] O is an element that forms non-metallic inclusions. If the O content is high, the particle size of the non-metallic inclusions will increase, so that the early fracture of the pipe 1 is likely to occur. Therefore, the lower the O content, the better. In particular, based on the provisions of ASTM 2063-18, the O content is preferably 0.04 mass% or less.
[0066] Furthermore, in order to adjust the superelasticity or shape memory property, the pipe 1 may contain at least one element selected from the group consisting of Cu (copper), Ta (tantalum), Zr (zirconium), Nb (niobium), V (vanadium), Mo (molybdenum), Cr (chromium), Fe (iron) and Co (cobalt) in a total amount exceeding 0.00 mass % and not more than 0.05 mass %. These elements are elements contained in the pipe 1 as needed in order to adjust the superelasticity or shape memory property. If the concentration of each of the above elements is not more than 0.05 mass %, there is no influence on the arithmetic mean height Sa of the inner wall surface 1a of the pipe 1.
[0067] The remainder other than the above components is Ti and inevitable impurities. Inevitable impurities refer to impurities of a certain content level that are inevitably mixed in the manufacturing process. Depending on the content of inevitable impurities, it may become a factor that affects the characteristics of the pipe material, so the smaller the content of inevitable impurities, the better. For example, the content of N (nitrogen) as an inevitable impurity is preferably 0.005 mass% or less.
[0068] The parent phase constituting the pipe material 1 is an austenite phase composed of a Ni—Ti alloy and has a B2 type crystal structure having a CsCI type body-centered cubic lattice structure.
[0069] As non-metallic inclusions existing in the matrix of the pipe material 1 composed of the Ni-Ti alloy, TiC-based inclusions mainly composed of carbides such as TiC, and Ti4Ni2O x If the amount of non-metallic inclusions in the parent phase is large, early fracture starting from the non-metallic inclusions is likely to occur. Among the non-metallic inclusions in the parent phase, the non-metallic inclusions that are particularly likely to become the starting point of early fracture are non-TiC inclusions, among which Ti4Ni2O x .
[0070] In addition, the ratio of the outer diameter R to the inner diameter r (outer diameter R / inner diameter r) of the tube 1 is preferably 1.01 or more and 5.00 or less, and more preferably 1.01 or more and 2.50 or less. When the ratio (outer diameter R / inner diameter r) of the tube 1 is within the above range, the durability against rotational bending is excellent even if the tube 1 has a small diameter, and the tube 1 can be suitably used in medical devices.
[0071] In addition, it is preferred that the outer diameter R of the tube 1 is 0.15 mm or more and 4.00 mm or less, and the inner diameter r of the tube 1 is 0.10 mm or more and 3.95 mm or less. If the outer diameter R and the inner diameter r of the tube 1 are respectively within the above ranges, the tube 1 has excellent durability against rotational bending even if it is a thin diameter, and the tube 1 can be suitably used in medical devices.
[0072] Furthermore, if the tube 1 has superelastic properties at 37° C., the tube 1 can exhibit superelastic properties in vivo, and thus the tube 1 can be preferably used in medical devices.
[0073] Next, a method for manufacturing a pipe material according to the embodiment will be described.
[0074] The manufacturing method of the pipe material of the embodiment comprises: a melting / forging step (step 1) of a Ni-Ti alloy raw material; a hot working step (step 2); a drawing step (step 3) of drawing a composite material obtained by inserting a core into the tubular Ni-Ti alloy hot working material obtained in the hot working step (step 2) to obtain a drawn composite material in which a tubular Ni-Ti alloy drawn material and a drawn core extending into the Ni-Ti alloy drawn material are integrated; and a core removal step (step 4) of applying a tensile load of a magnitude that prevents the Ni-Ti alloy drawn composite material in the drawn composite material from peeling off from the drawn core material while heating the Ni-Ti alloy drawn composite material to 150° C. or more and 800° C. or less. The pipe material manufactured by this manufacturing method is the pipe material 1 of the above-mentioned embodiment.
[0075] In the melting / forging step (step 1) of the Ni-Ti alloy raw material, the Ni-Ti alloy raw material is melted and then forged to obtain a Ni-Ti alloy ingot. Preferably, the carbon concentration ([C]) and oxygen concentration ([O]) in the Ni-Ti alloy ingot are both adjusted to 0.04 mass % or less.
[0076] In addition, in step 1, if the ([C] / [O]) ratio is 0.5 or more, the Ti4Ni2O in the ingot obtained in step 1 is suppressed. x Therefore, the fatigue durability required in particular for indwelling devices can be improved.
[0077] As a method of melting the Ni—Ti alloy raw material, the Ni—Ti alloy raw material is melted in a vacuum atmosphere or in an inert gas atmosphere such as Ar gas by a high-frequency melting method.
[0078] The carbon concentration (mass %) is adjusted by weighing the raw materials so that the total carbon amount including the carbon amount dissolved from the crucible used becomes a predetermined amount. The oxygen concentration (mass %) is adjusted by weighing the raw materials so that the oxygen amount becomes a predetermined amount based on the fact that the oxygen amount contained in the titanium raw material metal varies depending on the grade of the titanium raw material metal used as the raw material.
[0079] The carbon concentration and the oxygen concentration can be measured using a conventionally known carbon concentration analyzer and an oxygen concentration analyzer, respectively.
[0080] The hot working step (step 2) performed after step 1 includes a forging step (step 2-1) and may further include an extrusion step (step 2-2).
[0081] In the forging step (step 2-1), the Ni-Ti alloy ingot obtained in step 1 is forged to obtain a Ni-Ti alloy hot-worked material. The heating temperature during forging of the Ni-Ti alloy ingot is preferably 500° C. to 950° C., more preferably 600° C. to 800° C. In step 2-1, press forging or air hammer forging can be used.
[0082] Then, the Ni—Ti alloy hot-worked material is perforated by a gun drill and then finished by a lathe, thereby obtaining a seamless tubular Ni—Ti alloy hot-worked material.
[0083] In addition, an extrusion step (step 2-2) may be performed after the forging step (step 2-1). In the extrusion step (step 2-2), the Ni-Ti alloy hot-worked material obtained in step 2-1 is extruded to obtain a seamless tubular Ni-Ti alloy hot-worked material. The heating temperature during extrusion of the Ni-Ti alloy hot-worked material is preferably 500°C or more and 950°C or less, more preferably 600°C or more and 800°C or less. In addition, in Patent Document 5, the purpose is to ensure a high reduction rate from the perspective of emphasizing manufacturing efficiency, so the optimal processing temperature during extrusion is set to 800 to 1000°C. On the other hand, in the present embodiment, from the perspective of controlling inclusions (metallic structure) in the tubular material used in medical equipment, the heating temperature range during extrusion is different from that of Patent Document 5 for the purpose of maintaining the carbon concentration ([C]) and oxygen concentration ([O]) controlled in step 1 below 0.04 mass%.
[0084] In the drawing step (step 3) performed after step 2, the composite material obtained by inserting a core into the tubular Ni-Ti alloy hot-worked material obtained in step 2 is drawn.
[0085] First, a core is inserted into the tubular Ni-Ti alloy hot-working material obtained in step 2, thereby manufacturing a composite material formed by inserting a core inside the tubular Ni-Ti alloy hot-working material. When inserting a core into a tubular hot-working material, it is necessary to avoid forming an insertion injury along the long side direction of the hot-working material on the inner wall surface of the hot-working material, and the difficulty varies according to the inner diameter size of the hot-working material. Therefore, in the case where it is difficult to insert the core, a lubricant can also be applied to the inner wall surface of the hot-working material or the outer wall surface of the core. As a lubricant, phosphate film, graphite, molybdenum disulfide, and boron nitride are preferred.
[0086] The outer diameter of the tubular hot-worked material before the core is inserted is preferably 0.75 mm or more and 51.00 mm or less, more preferably 2.50 mm or more and 10.00 mm or less, and the inner diameter is preferably 0.50 mm or more and 9.00 mm or less. In addition, the ratio of the inner diameter to the outer diameter of the hot-worked material is preferably 1.01 or more and 5.00 or less, more preferably 1.01 or more and 2.50 or less, and further preferably 1.15 or more and 2.00 or less.
[0087] Here, if the size difference between the outer diameter of the core before the core is inserted into the hot-worked material and the inner diameter of the hot-worked material is set to 2% or more and 25% or less, the gap when the core is inserted can be sufficiently ensured, so that the composite material can be easily assembled. In addition, if the deformation resistance of the core is made the same as the deformation resistance of the hot-worked material, the bending of the inner wall surface of the hot-worked material can be suppressed, and the processing from the hot-worked material to the thin-diameter pipe can be performed in a good state. At this time, the composite material can also be subjected to warm processing described later for the purpose of adjusting the deformation resistance of the core and the hot-worked material.
[0088] The core is preferably cold-worked before being inserted into the hot-worked material. Here, the inventors have found that the arithmetic mean height Sa of the inner wall surface of the tube is important for the roughness state of the outer wall surface of the core before insertion. Therefore, when the arithmetic mean height Sa of the outer wall surface of the core is measured based on the description of "[3] Arithmetic mean height Sa of the outer wall surface of the core" described later, it is preferably 0.03 μm or more and 0.30 μm or less, and more preferably 0.03 μm or more and 0.20 μm or less. Regarding the annealing conditions of the core, some of them can be carried out in an air atmosphere, but the finishing is preferably carried out in an inert atmosphere.
[0089] Examples of the material of the core include SUS304, SUJ2, SS400, SCM415, SUS316, SUS309S, SUS310S, and Ni (54.5 to 56.0 mass %)-Ti (+ inevitable impurities), but the material is not limited thereto.
[0090] Then, the composite material is drawn. By drawing, a drawn composite material is obtained. The drawn composite material is a tubular Ni-Ti alloy drawn material obtained by drawing a tubular Ni-Ti alloy hot-worked material and a drawn core material extending into the interior of the Ni-Ti alloy drawn material and obtained by drawing a core.
[0091] Drawing is cold working or warm working. Regarding cold working, drawing is performed without putting the composite material into a temperature-controlled furnace. Warm working is to draw the composite material while controlling the temperature of the composite material, and is performed for the purpose of adjusting the deformation resistance of the core and the hot-worked material. The temperature of warm working is preferably 100°C or more and 800°C or less in terms of the set temperature in the furnace. Regarding the heating atmosphere, it can be an air atmosphere in order not to affect the state of the inner wall surface of the pipe, but it is preferably in an inert atmosphere in order to maintain the state of the outer wall surface of the pipe.
[0092] The processing rate in step 3 is at least 10% or more and less than 60%.
[0093] Alternatively, the composite material may be subjected to multiple stretching operations through a die having a continuously decreasing diameter.
[0094] Through step 3, a drawn composite material having an outer diameter of not less than 0.15 mm and not more than 4.00 mm is obtained.
[0095] In addition, in the drawing step (step 3), the composite material may be repeatedly subjected to drawing and annealing. Annealing is performed during or after the drawing process in order to remove and restore the strain generated in the composite material (tubular Ni-Ti alloy processed material) or the drawn composite material (tubular Ni-Ti alloy drawn material) by the annealing.
[0096] The annealing temperature in step 3 is preferably 500° C. to 800° C., more preferably 600° C. to 800° C. The heating atmosphere for annealing may be an air atmosphere so as not to affect the state of the inner wall surface of the tube, but is preferably an inert atmosphere for the purpose of maintaining the state of the outer wall surface of the tube.
[0097] The drawing process and annealing of the composite material are repeated until the composite material reaches the above-mentioned dimensions.
[0098] In the core removal step (step 4) performed after step 3, only the drawn core material is removed from the drawn composite material obtained in step 3 to obtain a tube. The core removal step (step 4) includes a tensile load imparting step (step 4-1), an annealing step (step 4-2), a core diameter reduction step (step 4-3), and a core extraction step (step 4-4). The core diameter reduction step (step 4-3) is an optional step.
[0099] In the tensile load imparting step (step 4-1), a tensile load of a magnitude that prevents the tubular Ni-Ti alloy drawn material in the drawn composite material from peeling off from the drawn core material is imparted to the drawn core material in the drawn composite material. The tensile load imparted to the drawn core material is preferably 4 MPa to 300 MPa, more preferably 20 MPa to 150 MPa.
[0100] Figure 2 is a cross-sectional view showing an example of the tensile load imparting step (step 4-1). Figure 3 FIG. 4 is a cross-sectional view showing another example of the tensile load imparting step (step 4-1). Figure 2As shown in FIG. 1 , a score line 21 may be drawn along the entire circumferential direction at both ends of the tubular Ni-Ti alloy drawn material 20 constituting the drawn composite material 10. The score line 21, for example, passes through the outer wall surface of the Ni-Ti alloy drawn material 20 to the inner wall surface. In this structure, a tensile load is applied to the drawn core material 30 while grasping a portion of the drawn composite material 10 closer to the end side than the score line 21. In addition, as Figure 3 As shown, the two ends of the Ni-Ti alloy drawn material 20 may be cut off to expose the drawn core material 30 from the two ends of the drawn composite material 10. In this structure, the drawn core material 30 exposed at the two ends of the drawn composite material 10 is grasped while applying a tensile load to the drawn core material 30.
[0101] If the tensile load applied to the drawing core material 30 of the drawing composite material 10 is larger than the above range, that is, if the tensile load is applied to a magnitude such that the Ni-Ti alloy drawing material 20 in the drawing composite material 10 is peeled off from the drawing core material 30, plastic deformation of the Ni-Ti alloy drawing material 20 occurs, and thus the material properties of the pipe material 1 including the arithmetic mean height Sa deteriorate. As a result, the arithmetic mean height Sa of the inner wall surface 1a of the pipe material 1 exceeds 0.55 μm.
[0102] In the annealing step (step 4-2) performed after the tensile load applying step (step 4-1), the Ni-Ti alloy drawn material 20 is heated in a state where the tensile load of the magnitude described above is applied to the drawn core material 30 in the drawn composite material 10 in the tensile load applying step (step 4-1). The heating temperature is 150° C. to 800° C., preferably 450° C. to 700° C.
[0103] Figure 4 It is a drawing pair Figure 2 The cross-sectional view of the drawn composite material 10 of the structure shown in FIG. 1 is a state after the annealing step (step 4-2). Figure 5 It is a drawing pair Figure 3 The cross-sectional view of the drawn composite material 10 after the annealing step (step 4-2) is performed. Figures 4-5As shown, an annealing step (step 4-2) is performed, and due to the difference in thermal expansion between the Ni-Ti alloy drawn material 20 and the drawn core material 30, the drawn core material 30 is peeled off from the drawn composite material 10 to obtain the tube material 1. In the annealing step (step 4-2), since the Ni-Ti alloy drawn material 20 is uniformly expanded due to thermal expansion, it is possible to suppress the occurrence of abrasions or scratches on the inner wall surface of the tubular Ni-Ti alloy drawn material 20 caused by the drawing core material 30 being peeled off from the Ni-Ti alloy drawn material 20. In addition, the drawing core material 30 can be peeled off from the drawn composite material 10 to obtain the tube material 1 by the annealing step (step 4-2), and the tube material 1 can be given superelastic properties.
[0104] Alternatively, after the annealing step (step 4-2), a core diameter reduction step (step 4-3) may be performed. Figure 6 is a cross-sectional view showing an example of the core diameter reduction step (step 4-3), showing the Figure 4 The structure of the core is implemented in the state of the core diameter reduction step (step 4-3). Figure 6 As shown, in the core diameter reduction step (step 4-3), a tensile load is applied to the annealed drawn core material 30 separated from the tube material 1. The tensile load applied to the drawn core material 30 in the core diameter reduction step (step 4-3) is greater than the tensile load applied to the drawn core material 30 in the tensile load applying step (step 4-1). In addition, the tensile load in the core diameter reduction step (step 4-3) is not applied to the tube material 1.
[0105] By applying a large tensile load only to the drawing core material 30 in the core diameter reduction step (step 4-3), the diameter of the drawing core material 30 can be reduced. Therefore, the gap between the inner wall surface of the tube material 1 and the outer wall surface of the drawing core material 30 can be increased compared to the structure after the annealing step (step 4-2).
[0106] Figure 7 FIG. 4 is a cross-sectional view showing an example of the core extraction step (step 4-4). Figure 7 As shown, in the core extraction step (step 4-4) performed after the annealing step (step 4-2) or the core diameter reduction step (step 4-3), the drawing core material 30 is extracted from the tube material 1, thereby manufacturing the tube material 1. In the core extraction step (step 4-4), since the drawing core material 30 is extracted from the tube material 1 in a state where the inner wall surface 1a of the tube material 1 and the outer wall surface 30a of the drawing core material 30 are completely separated, it is possible to suppress the occurrence of abrasions or scratches on the inner wall surface 1a of the tube material 1 due to the extraction of the drawing core material 30, so that the tube material 1 can be manufactured in which the arithmetic mean height Sa of the inner wall surface 1a is within the above-mentioned range.
[0107] In addition, for Figure 4 and Figure 6 In the case of a construction such as Figure 7 As shown, after one end side of the drawing core material 30 is cut off and the one-side end of the drawing core material 30 integrated with a part of the Ni-Ti alloy drawing material 20 is removed, the drawing core material 30 is extracted from the tube material 1. Therefore, when the drawing core material 30 is extracted from the tube material 1, it is possible to avoid that a part of the Ni-Ti alloy drawing material 20 attached to the one-side end of the drawing core material 30 contacts the inner wall surface 1a of the tube material 1, so it is possible to prevent the inner wall surface 1a of the tube material 1 from being scratched or scratched by the material 20.
[0108] In addition, if Figure 6 The core reduction step (step 4-3) shown in FIG. Figure 4 and Figure 5 Compared with the structure after the annealing step (step 4-2) shown in the figure, the gap between the inner wall surface 1a of the tube material 1 and the outer wall surface 30a of the drawing core material 30 can be increased. Therefore, in the core extraction step (step 4-4), it is possible to further suppress the occurrence of scratches or scratches on the inner wall surface 1a of the tube material 1 caused by the extraction of the drawing core material 30. As a result, the arithmetic mean height Sa of the inner wall surface 1a of the tube material 1 can be further reduced.
[0109] Thus, a pipe having a fine inner wall surface roughness can be manufactured by the above industrially easy method without performing special post-processing steps such as mandrel drawing, mandrel processing, inner wall surface grinding, etc. that are required in the prior art. Furthermore, a pipe longer than before, for example, a pipe having a length of about 10 m to 100 m, can be manufactured easily by the above industrially easy method.
[0110] In addition, the manufacturing method of the pipe material of the embodiment may further include a heat treatment step (step 5) for imparting superelasticity, which is performed after the core removal step (step 4) and heats the pipe material 1 to impart superelasticity. The conditions for heating to impart superelasticity, such as the heating atmosphere and the heating temperature of the pipe material 1, are not particularly limited as long as the pipe material 1 can be imparted with superelastic properties.
[0111] For example, if the pipe is heated at a temperature of 600°C or less in an inert gas atmosphere, the amount of non-metallic inclusions present in the pipe composed of a Ni-Ti alloy can be suppressed. In addition, the heating temperature is preferably 450°C or more and 580°C or less. In addition, if a heat treatment step (step 5) is performed to impart superelasticity in a state where the pipe is straightly stretched by applying a tensile load, the straightness of the pipe can be improved.
[0112] In addition, the method for manufacturing a tube of the embodiment may perform additional processing between the core removal step (step 4) and the heat treatment step (step 5) for imparting superelasticity, or after the core removal step (step 4) when the heat treatment step (step 5) for imparting superelasticity is not performed, for the purpose of fine-tuning the size of the tube or for the purpose of pre-processing of the heat treatment step (step 5) for imparting superelasticity.
[0113] The total reduction ratio of the pipe material in the additional processing is preferably 10% or more and less than 120%, and more preferably 10% or more and less than 84%. The total reduction ratio of the pipe material, as described in Japanese Industrial Standards (JIS) H0500: 1998, is the ratio of the cross-sectional area reduced by processing to the original cross-sectional area, and is expressed as the percentage (%) obtained by dividing the difference between the cross-sectional area Ao of the material before processing and the cross-sectional area A after processing by the cross-sectional area Ao of the material before processing ((Ao-A) / Ao×100%). Here, the cross-sectional area Ao of the pipe material before the additional processing and the cross-sectional area A of the pipe material after the additional processing are measured, and the total reduction ratio is calculated using the above calculation formula.
[0114] As described above, the pipe material of the embodiment can be industrially manufactured by an easy method, the roughness of the inner wall surface is improved, and the durability to rotation and bending is excellent, so it can be suitably used in the pipe material constituting medical equipment. As the medical equipment, stents, guide wires, and pressure guide wires are preferred. Such stents, guide wires, and pressure guide wires are respectively formed by pipe materials. Furthermore, since the roughness of the inner wall surface of the pipe material is improved, it can be expected that the form of inserting other equipment into the pipe material for use can be used as a novel medical equipment.
[0115] According to the above-described embodiment, a pipe material made of a Ni—Ti alloy material, with improved inner wall surface roughness and excellent durability against rotational bending can be obtained by an easy method.
[0116] Although the embodiments have been described above, the present invention is not limited to the above embodiments, but includes the concept of the present disclosure and all aspects included in the claims, and various changes can be made within the scope of the present disclosure.
[0117] Example
[0118] Next, examples and comparative examples are described, but the present disclosure is not limited to these examples. In addition, the composition (mass %) of each component shown in Tables 1 and 2 is obtained by the reference intensity ratio (RIR) method.
[0119] (Example 1)
[0120] As a melting / forging step (step 1), the molten metal obtained by melting the Ni raw material metal and the Ti raw material metal as the raw materials of the Ni-Ti alloy in a high-frequency melting furnace is poured to obtain a Ni-Ti alloy ingot having an alloy composition shown in Table 1. Then, as a hot working step (step 2), the obtained ingot is forged at 500°C or more and 950°C or less to obtain a Ni-Ti alloy forging material. Then, after the forging material is perforated with a gun barrel drill, it is finished by a lathe to obtain a seamless tubular Ni-Ti alloy hot-working material. Then, as a drawing step (step 3), the composite material formed by inserting the core shown in Table 3 into the tubular working material is drawn. In this way, a tubular Ni-Ti alloy drawing material and a drawing composite material formed by integrating a drawing core material extending into the interior of the Ni-Ti alloy drawing material are obtained.
[0121] Next, as a core removal step (step 4), a line is drawn along the entire circumferential direction at both ends of the tubular Ni-Ti alloy drawn material constituting the drawn composite material. Furthermore, while grasping the portion of the drawn composite material closer to the end side than the line, the tensile load shown in Table 3 is applied to the drawn core material. Subsequently, the Ni-Ti alloy drawn material is heated at the annealing temperature shown in Table 3 while the tensile load shown in Table 3 is applied to the drawn core material. In this way, superelastic properties are imparted, and the drawn core material is peeled off from the drawn composite material to obtain a tube. Subsequently, after cutting off one end side of the drawn core material and removing the single-side end of the drawn core material integrated with a part of the Ni-Ti alloy drawn material, the drawn core material is extracted from the tube. In this way, a tube having a length of 10 to 100 m and having an inner wall surface having the dimensions, arithmetic mean height Sa, and calculated average roughness Ra shown in Table 3 is manufactured.
[0122] (Example 2)
[0123] A pipe having an inner wall surface having an arithmetic mean height Sa and a calculated average roughness Ra shown in Table 3 was manufactured in the same manner as in Example 1, except that the tensile load and the annealing temperature before annealing in the core removal step (step 4) were changed to the values shown in Table 3 and the pipe was subjected to additional processing with a total area reduction rate shown in Table 3.
[0124] (Examples 3 to 8)
[0125] A pipe having an inner wall surface having an arithmetic mean height Sa and a calculated average roughness Ra shown in Table 3 was manufactured in the same manner as in Example 1, except that the core shown in Table 3 was used and the tensile load and annealing temperature before annealing in the core removal step (step 4) were changed to the values shown in Table 3.
[0126] (Examples 9 to 16)
[0127] A pipe having an inner wall surface having an arithmetic mean height Sa and a calculated average roughness Ra shown in Table 3 was manufactured in the same manner as in Example 1, except that the core shown in Table 3 was used, the tensile load and the annealing temperature before annealing in the core removal step (step 4) were changed to the values shown in Table 3, and the pipe was subjected to additional processing with a total area reduction rate shown in Table 3.
[0128] (Comparative Examples 1 to 4)
[0129] A pipe material having an inner wall surface having an arithmetic mean height Sa and a calculated average roughness Ra shown in Table 3 was manufactured in the same manner as in Example 1, except that the core shown in Table 3 was used and the tensile load and annealing temperature before annealing in the core removal step (step 4) were changed to the values shown in Table 3. In addition, in Comparative Examples 1 and 2, annealing was performed in a state where a tensile load was not applied before annealing and a tensile load was not applied to the drawn core material. In Comparative Example 4, annealing was not performed.
[0130] (Comparative Examples 5 to 13)
[0131] A pipe material having an inner wall surface having an arithmetic mean height Sa and a calculated average roughness Ra shown in Table 3 was manufactured in the same manner as in Example 1, except that the core shown in Table 3 was used, the tensile load and the annealing temperature before annealing in the core removal step (step 4) were changed to the values shown in Table 3, and the pipe material was subjected to additional processing with a total area reduction ratio shown in Table 3. In Comparative Examples 6 to 11, annealing was performed without applying a tensile load before annealing and without applying a tensile load to the drawn core material.
[0132] (Examples 17 to 21)
[0133] A pipe having an inner wall surface having an arithmetic mean height Sa and a calculated average roughness Ra shown in Table 4 was manufactured in the same manner as in Example 1, except that in the drawing step (step 3), the core shown in Table 4 was used, and the drawing and annealing at the temperature shown in Table 4 were repeatedly performed on the composite material, and the tensile load before annealing and the annealing temperature in the core removal step (step 4) were changed to the values shown in Table 4.
[0134] (Examples 22 to 25)
[0135] A pipe having an inner wall surface having an arithmetic mean height Sa and a calculated average roughness Ra shown in Table 4 was manufactured in the same manner as in Example 1, except that in the drawing step (step 3), the core shown in Table 4 was used, and the composite material was repeatedly subjected to drawing and annealing at the temperature shown in Table 4, the tensile load and annealing temperature before annealing in the core removal step (step 4) were changed to the values shown in Table 4, and the pipe was subjected to additional processing with a total area reduction rate shown in Table 4.
[0136] (Examples 26 to 37)
[0137] A pipe having an inner wall surface having the dimensions, arithmetic mean height Sa, and calculated average roughness Ra shown in Table 5 was manufactured in the same manner as in Example 1, except that the core shown in Table 5 was used, the tensile load and the annealing temperature before annealing in the core removal step (Step 4) were changed to the values shown in Table 5, and the pipe was subjected to additional processing with a total area reduction ratio shown in Table 5. In Examples 27 and 31, no additional processing was performed.
[0138] (Examples 38 to 49, Comparative Examples 14 to 15)
[0139] A pipe having an inner wall surface having an arithmetic mean height Sa and a calculated average roughness Ra shown in Table 6 was manufactured in the same manner as in Example 1, except that a Ni-Ti alloy ingot having an alloy composition shown in Tables 1 and 2 was used, a core shown in Table 6 was used, the tensile load before annealing and the annealing temperature in the core removal step (step 4) were changed to the values shown in Table 6, and the pipe was subjected to additional processing with a total area reduction rate shown in Table 6.
[0140] (Examples 50 to 59)
[0141] As shown in Table 7, a pipe having an inner wall surface having an arithmetic mean height Sa and a calculated average roughness Ra shown in Table 7 was manufactured in the same manner as in Example 1, except that a Ni-Ti alloy ingot having an alloy composition shown in Table 2 was used and the tensile load before annealing and the annealing temperature in the core removal step (step 4) were changed to the values shown in Table 7.
[0142] [Measurement and evaluation]
[0143] The following measurements and evaluations were performed on the pipes obtained in the above-described Examples and Comparative Examples.
[0144] [1] Arithmetic mean height Sa of the inner wall of the tube
[0145] A tubular sample was collected by cutting a portion of the obtained pipe material at a distance of 100 mm or more from both ends along the longitudinal direction, and then four locations of the inner wall surface of the pipe material were measured using a LEXT OLS5100 3D measurement laser microscope.
[0146] As described in the International Organization for Standardization (ISO) 42881996E (JIS B0633: 2001), in 0.1<Ra(μm)<2.0, the evaluation length (mm) of the roughness curve is specified to be at least 4 mm, but no detailed measurement length is specified for the arithmetic mean height Sa. In addition, JIS B0681-2: 2018 and JIS B0681-3: 2019 describe conditions related to three-dimensional surface properties, but there is no equivalent to λ compared to two-dimensional roughness measurement. c The L filter is equivalent to λ s The relevant provisions for the cut-off of the S filter.
[0147] Therefore, in this measurement, the circumferential direction of the pipe is taken as the X direction, and the long side direction of the tube is taken as the Y direction. The image formed by connecting 5 fields of view in the Y direction is used for the measurement surface (1 field of view) of 35 μm in the X direction and 125 μm in the Y direction (there are repeated parts in the connected image, so the length of the connected image in the Y direction is about 592 μm). At this time, the cutoff value of each filter (L and S) is none. Regarding the F operator corresponding to the boundary λf of the corrugation component specified in JIS B0681-3:2019, the multi-curve quartic operator is used to remove the corrugation component, and the curvature in the X and Y directions is converted into a plane, and then analyzed to obtain the arithmetic mean height. Then, the smallest value among the arithmetic mean heights obtained at the four measured locations is taken as the arithmetic mean height Sa of the inner wall surface of the pipe.
[0148] [2] Arithmetic mean roughness Ra of the inner wall surface of the tube
[0149] In the same manner as above, in the image obtained by measuring the inner wall surface of the pipe using a 3D measuring laser microscope, 7 lines with an evaluation length of 4 mm or more along the Y direction were measured. Then, the smallest value among the arithmetic mean roughness obtained at the four measured locations was taken as the arithmetic mean roughness Ra of the inner wall surface of the pipe.
[0150] [3] The arithmetic mean height Sa of the outer wall of the core
[0151] For the portion of the core that is more than 100 mm away from both ends and the central portion, the outer wall surface of the core is measured using a 3D measurement laser microscope in the same manner as above to obtain the arithmetic mean height. Then, the value of the second decimal place of the largest value of the arithmetic mean height obtained at the three measured locations is summarized as follows for every 0.05 μm and is taken as the arithmetic mean height Sa of the outer wall surface of the core. Specifically, a value of 0.08 μm or more and 0.10 μm or less is regarded as the arithmetic mean height Sa 0.10 μm, a value of 0.11 μm or more and 0.15 μm or less is regarded as the arithmetic mean height Sa 0.15 μm, a value of 0.16 μm or more and 0.20 μm or less is regarded as the arithmetic mean height Sa 0.20 μm, and a value of 0.25 μm or more and 0.30 μm or less is regarded as the arithmetic mean height Sa0.30 μm. In addition, regarding 0.05 μm of Example 18 and 0.03 μm of Example 19 in Table 1, the values are too small to be summarized as 0.05 as described above, so the largest value is taken as the arithmetic mean height Sa of the core outer wall surface.
[0152] [4] Fracture durability at 1.0% bending strain
[0153] As the durability against rotational bending, a rotational bending test was performed with a 1.0% bending strain applied to the pipe, and the fracture durability against the strain was measured. Figure 8 The double-drive type rotary bending fatigue testing machine 50 shown in the figure performs a fracture durability test for a 1.0% bending strain of the pipe 1. In addition, the maximum bending strain 1.0% (strain) applied to the pipe is set according to the following formula (1). In addition, the distance C between the chucks is set according to the following formula (2). R is the outer diameter of the pipe, and L is the length of the pipe.
[0154] In a double-drive rotary bending fatigue testing machine 50, a heater power supply 53 with a stirring device motor having a heater 51 and a stirring device 52 is used to circulate the silicone oil 54 while maintaining the temperature of the silicone oil 54 at 37°C. Then, the motor 55 with an integrated tachometer is used to rotate the tube 1 at a speed of 300 times / min while imparting a bending strain of 1.0% to the tube 1, and the number of times (number of fractures) until the tube 1 breaks is measured. Among them, only in Example 49 with a high phase transition temperature, the temperature of the silicone oil 54 is maintained at 100°C. For this measurement, three samples were measured (n=3), and the lowest number was taken as the number of fractures. The following classification was performed for fracture durability.
[0155] ◎: The number of breakages is 9,000 or more.
[0156] ○: The number of breakages is 7500 or more and less than 9000 times.
[0157] ×: The number of breakages is less than 7500 times.
[0158] [Number 1]
[0159]
[0160] [Number 2]
[0161] =2.19×C(2)
[0162] In addition, the rotating bending test is usually affected by the physical state of the sample surface (roughness, voids, defects, etc.), so the physical state of the sample surface is stabilized by electrolytic grinding of the sample surface. However, it is known that in the case of high-strain bending of the pipe, the electrolytic grinding state of the pipe affects the number of pipe fractures, so here, the rotating bending test is performed after the arithmetic mean height Sa of the outer wall surface of the pipe is processed to be 0.15μm or more and 0.25μm or less.
[0163] [5] Evaluation of pipe properties
[0164] In the pipes manufactured in Examples 1 to 59, after a 6% strain was applied in a tensile test, the load was removed or the pipes were heated after the load was removed, whereby the residual strain was 0.5% or less. Therefore, the pipes in Examples 1 to 59 had superelastic properties and shape memory properties.
[0165] [6] Oxygen concentration and carbon concentration
[0166] The oxygen concentration and carbon concentration contained in the pipes produced in Examples 1 to 59 were measured using a carbon concentration analyzer and an oxygen concentration analyzer, and the results were all 0.04 mass % or less.
[0167] [Table 1]
[0168]
[0169] [Table 2]
[0170]
[0171]
[0172]
[0173]
[0174]
[0175]
[0176]
[0177]
[0178]
[0179] Fig. 9 These are the results of observing the inner wall surface of the pipe produced in Example 1 using a 3D measurement laser microscope. Fig.10 These are the results of observing the inner wall surface of the pipe produced in Example 10 using a 3D measurement laser microscope. Fig.11 These are the results of observing the inner wall surface of the pipe produced in Comparative Example 6 using a 3D measurement laser microscope.
[0180] As shown in Tables 1 to 7 and Figures 9-11 As shown in the figure, in all the examples, the pipe materials manufactured by the steps under the specified conditions are composed of Ni-Ti alloy, and the arithmetic mean height Sa of the inner wall surface is 0.08 μm or more and 0.55 μm or less. Therefore, the durability against rotational bending is excellent. On the other hand, in all the comparative examples, the pipe materials manufactured by the steps not under the specified conditions have an arithmetic mean height Sa of the inner wall surface exceeding 0.55 μm, and therefore the durability against rotational bending is poor.
[0181] Specifically, according to the results of Examples 1 to 16, even if the material of the core used is changed, the arithmetic mean height Sa of the inner wall surface can be controlled within the above range by manufacturing the tube in a step under specified conditions. According to the results of Examples 17 to 25, in the drawing step (step 3), even if the Sa of the outer wall surface of the core is changed, the arithmetic mean height Sa of the inner wall surface can be controlled within the above range. In addition, in the drawing step (step 3), even if the drawing and annealing are repeatedly performed, the arithmetic mean height Sa of the inner wall surface can be controlled within the above range. According to the results of Examples 26 to 37, for tubes with different outer diameters and inner diameters, the arithmetic mean height Sa of the inner wall surface can be controlled within the above range. According to the results of Examples 38 to 59, for tubes with different alloy compositions, the arithmetic mean height Sa of the inner wall surface can be controlled within the above range.
[0182] In addition, in Comparative Examples 1 and 2, since the annealing was performed without applying a tensile load before annealing and without applying a tensile load to the drawing core material, the drawing core material could not be peeled off from the drawing composite material, and as a result, the pipe material could not be manufactured. In Comparative Example 3, since a tensile load of such magnitude that the tubular Ni-Ti alloy drawing material would peel off from the drawing core material was applied to the drawing core material in the drawing composite material, the Ni-Ti alloy drawing material was plastically deformed and the pipe shape could not be controlled, so it was determined that the pipe material could not be manufactured. In Comparative Example 4, since the annealing was not performed in a state where a tensile load was applied to the drawing core material, the drawing core material could not be peeled off from the drawing composite material, and as a result, the pipe material could not be manufactured. In Comparative Example 5, since the annealing temperature exceeded 800°C, the control of non-metallic inclusions was insufficient, and therefore the Sa of the inner wall surface of the pipe material exceeded 0.55μm, and the durability against rotational bending was inferior to that of the pipe material of the embodiment. In Comparative Examples 6 to 11, depending on the material of the core, it is sometimes possible to manufacture a pipe even if annealing is performed without applying a tensile load before annealing and without applying a tensile load to the drawing core material. However, when the drawing core material is pulled out from the pipe material, friction resistance that is not generated in the embodiment is felt. As a result, the Sa of the inner wall surface of the pipe material exceeds 0.55 μm, and the durability to rotation bending is inferior to that of the pipe material in the embodiment. In Comparative Examples 12 to 13, since the total reduction rate of the additional processing of the pipe material is too large, the Sa of the inner wall surface of the pipe material exceeds 0.55 μm, and the durability to rotation bending is inferior to that of the pipe material in the embodiment. In Comparative Example 14, since the Ni concentration of the alloy composition is low, cracks occur due to forging, and the subsequent steps cannot be performed. In Comparative Example 15, since the Ni concentration of the alloy composition is high, cracks occur in the same way as in Comparative Example 14, and the subsequent steps cannot be performed.
[0183] Reference numerals
[0184] 1. Pipe
[0185] 1a Inner wall of the pipe
[0186] 10Drawing processing of composite materials
[0187] 20 Tubular Ni-Ti alloy drawing materials
[0188] 21 dash
[0189] 30 Drawing core material
[0190] 30a Drawing processing of the outer wall of the core material
[0191] 50 double drive rotary bending fatigue testing machine
[0192] 51 Heater
[0193] 52 stirring device
[0194] 53 Heater power supply with stirring device motor
[0195] 54 Silicone oil
[0196] 55 Motor with cumulative tachometer
Claims
1. A pipe material, comprising a Ni-Ti alloy, wherein an arithmetic mean height Sa of an inner wall surface is not less than 0.08 μm and not more than 0.55 μm.
2. The pipe according to claim 1, comprising 54.5 mass % or more and 57.0 mass % or less of Ni, with the remainder being Ti and unavoidable impurities.
3. The pipe according to claim 1, wherein: The ratio of the outer diameter to the inner diameter of the pipe (outer diameter / inner diameter) is 1.01 or more and 5.00 or less.
4. The pipe according to claim 1, wherein: The outer diameter of the pipe is greater than or equal to 0.15 mm and less than or equal to 4.00 mm, and the inner diameter of the pipe is greater than or equal to 0.10 mm and less than or equal to 3.95 mm. The tube according to claim 1 , having superelastic properties at 37° C. .
6. A stent formed from the tube according to any one of claims 1 to 5.
7. A guide wire formed by the tube according to any one of claims 1 to 5.
8. A pressure guide wire, formed by the tube according to any one of claims 1 to 5.
9. A method for manufacturing a pipe, which is the method for manufacturing a pipe according to any one of claims 1 to 5, comprising: A step of melting / forging the Ni-Ti alloy raw material (step 1); Thermal processing step (step 2); A drawing step (step 3) of drawing a composite material obtained by inserting a core into the tubular Ni-Ti alloy hot-worked material obtained in the aforementioned hot working step (step 2) to obtain a drawn composite material in which the tubular Ni-Ti alloy drawn material and the drawn core extending into the interior of the aforementioned Ni-Ti alloy drawn material are integrated; and In the core removal step (step 4), a tensile load of a magnitude that prevents the Ni—Ti alloy drawn material in the drawn composite material from peeling off from the drawn core material is applied to the drawn core material in the drawn composite material, while the Ni—Ti alloy drawn material is heated to a temperature of 150° C. to 800° C.
10. The method for manufacturing a pipe according to claim 9, wherein: In the core removal step (step 4), the Ni—Ti alloy drawn material is heated to 150° C. to 800° C. while applying a tensile load of 4 MPa to 300 MPa to the drawn core material in the drawn composite material.
11. The method for manufacturing a pipe according to claim 9, wherein: The method further comprises a heat treatment step (step 5) for imparting superelasticity, which is performed after the core removal step (step 4) and involves heating the tube material to impart superelasticity.
Citation Information
Cited By
Nickel-titanium memory alloy pipe as well as preparation method and application thereof
CN120394605A
A nickel-titanium memory alloy pipe and a preparation method and application thereof