Preparation method of metal porous nickel film

By combining flat plate coating and powder loose pressurized sintering technology, the problems of small thickness, low yield and sintering cracking of porous nickel film are solved, and the preparation of metal porous nickel film with thin thickness, uniform pore size and flexibility is achieved, which is suitable for new Applications in the energy field.

CN119076953APending Publication Date: 2024-12-06XI'AN PETROLEUM UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411221510.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art has low yield and high production costs when preparing porous metal nickel films with thickness less than 0.5 mm, and is prone to cracking and mechanical properties during sintering, which limits large-scale production and application.

Method used

Using flat plate coating and powder loose pressurized sintering technology, sintering is carried out through ceramic plate stacking, combining distilled water to mix polyvinyl alcohol solution and nickel powder, and using polyethylene terephthalate film as the coating matrix , control the spatula distance and speed to achieve aperture uniformity and surface flatness.

Benefits of technology

Improve the yield and flexibility of porous nickel films, reduce the flat pressing process after sintering, and realize the preparation of metal porous nickel films with thin thickness, light weight and flexibility. They are suitable for large-scale production and new energy fields. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076953A_ABST
    Figure CN119076953A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a metal porous nickel film, the method combines a plate coating technology with a powder loose loading pressure sintering process, and the preparation process mainly comprises the following steps: preparing metal slurry, coating a film layer, drying a porous nickel film green body, and sintering and molding, the problem that the porous nickel film cracks due to sintering shrinkage in the sintering process can be avoided, it is guaranteed that the film has good surface smoothness after being sintered, and the flattening and pressing procedure after a traditional metal porous film is sintered is omitted. The porous nickel film prepared by the method has the characteristics of small thickness, high porosity and good mechanical property, and is suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal porous membrane materials, and in particular to a method for preparing a flexible, lightweight ultra-thin metal porous nickel membrane. Background Art

[0002] Metal porous membranes can be divided into homogeneous porous metal membranes and gradient porous metal membranes. As functional elements, their shapes can be mainly divided into plate-shaped and tubular. Flat homogeneous porous metal membranes have the characteristics of high mechanical strength, good thermal conductivity, large membrane flux, and good support. Their research and application have been expanded to many fields, including chemical metallurgy, food, medical and biofuel industries. For example, in the chemical industry, stainless steel membranes, nickel and nickel alloy membranes are often used in liquid-solid and gas-solid separation processes under special working conditions; in the food processing field, porous gradient metal separation membranes can filter starch or pectin in juice; in the biomedical field, porous metal membranes can be used as porous coating materials for artificial bones, orthopedics and dentistry; in the field of new energy, porous metal nickel membranes can be used as porous transport layer materials for membrane electrodes in alkaline anion exchange membrane (AEM) electrolyzers, which can improve the heat and mass transfer efficiency of membrane electrodes.

[0003] As early as the 1940s, in order to solve the problem of uranium isotope separation, people invented porous metal nickel membranes, but due to its poor thermal stability under this working condition, it failed to be applied industrially and remained in the exploration stage. For metal porous nickel membranes, the membrane pore structure characteristics and mechanical properties obtained by different preparation technologies are different, resulting in different research and development directions focused on in different application fields. As a type of porous metal membrane, flat metal porous nickel membrane can be used as an anode material for anion exchange membrane electrolysis of water (AEMWE) in addition to filtration and flexible electronic components, laying the foundation for my country's green, highly flexible large-scale energy storage technology. At present, AEM is in the laboratory research and development stage. The service life and ionic conductivity of the anion exchange membrane still need to be tackled. It is crucial to study gas transport layer materials with high electrical and thermal conductivity, strong gas repellency / hydrophilicity, good mechanical properties and high corrosion resistance. Since the structural characteristics of the gas transport layer material, such as porosity, pore morphology, membrane thickness, and permeability, can affect the efficiency of AEM water electrolysis to produce hydrogen, providing a porous metal nickel membrane with high porosity, uniform pores, good mechanical properties and controllable parameters is an urgent problem to be solved in the field of AEM electrolysis of hydrogen.

[0004] At present, common porous metal film preparation methods include dealloying, electrodeposition, wet powder spraying (Chinese patent, application publication number CN103432828A) and powder metallurgy, etc., wherein dealloying and electrodeposition are suitable for preparing metal films with nanoscale pores, while powder metallurgy is generally used to prepare metal films with micrometers and pores. As for flat porous metal films, when using powder metallurgy technology to prepare, the method of powder rolling is generally used to first obtain the porous metal film green body, and then sintering is performed to finally obtain the porous metal film finished product. The disadvantage of this technology is that when preparing a porous metal film with a thickness of less than 0.5 mm, the yield is low, resulting in a high production and preparation cost. The invention patent "A porous titanium plate and its preparation method" (Chinese patent, application publication number CN115475942A) discloses a method for preparing porous titanium plates with a thickness range of 0.1 to 0.3 mm. This method first prepares a porous titanium block by a powder loosening method, and then obtains a titanium plate of the required thickness by wire cutting: the disadvantage of this method is that the added wire cutting process reduces the production efficiency, and because the wire cutting process destroys the powder particle morphology and the sintering necks between the particles, the mechanical properties of the metal porous membrane are affected to a certain extent. The invention patent "A porous material and its preparation method" (Chinese patent, application publication number CN118324515A) discloses a method for preparing nano-wire Ti6O porous membrane. This method also obtains titanium membrane green body by scraping technology, and then obtains nano-wire Ti6O porous membrane finished product after sintering. However, the titanium membrane loading method disclosed in the invention patent is the unlimited free sintering of the film. As a result, when the film size is too large and the thickness is thin, the sintering shrinkage and self-weight of the material will cause the film layer to crack, and the preparation of large-sized porous films cannot be realized. At the same time, the porous film is prone to warping after sintering, which limits the large-scale preparation of commercial products to a certain extent.

[0005] Based on the above problems, the present invention provides a method for preparing a metal porous nickel film, which combines flat coating with powder loose-packing pressure sintering technology, and its preparation process includes metal slurry configuration, film coating, porous nickel film green body drying, sintering molding, and the sintering process adopts a ceramic plate stacking green body method, which can avoid the cracking problem caused by sintering shrinkage during the sintering process of the porous nickel film, and ensure that the film has good surface flatness after sintering, reducing the flat pressing process after sintering of the traditional metal porous film. This process has the advantages of simple operation and high yield rate, and the prepared flat film has the characteristics of thin thickness, light weight, good flexibility, etc., and can be suitable for large-scale production. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for preparing a metal porous nickel film in view of the above-mentioned deficiencies in the prior art. The method has a simple preparation process, controllable pore size, and a wide range of applications. The metal porous film prepared by the method has uniform pore size, good permeability, high flexibility, and has great application prospects in the field of new energy.

[0007] Based on the advantages and disadvantages of different preparation methods of metal porous nickel film, the present invention proposes a novel, high-performance preparation process of metal porous nickel film, the innovation points mainly include the optimal ratio of metal powder slurry, the film coating control parameters and the film sintering process, and its characteristics and the preparation method mainly include the following steps:

[0008] (1) using distilled water to prepare a polyvinyl alcohol (PVA) solution with a concentration ranging from 5% to 9%;

[0009] (2) mixing the PVA solution prepared in (1) with Ni powder of a certain particle size range after screening to obtain a nickel powder slurry; adding a defoaming agent to the nickel powder slurry and stirring evenly to remove bubbles in the slurry; the nickel powder particle size range is 1 to 150 μm, and the solid content range of the nickel powder slurry is 30% to 60%;

[0010] (3) pouring the nickel powder slurry obtained in (2) evenly onto a flat coating machine for coating, the coating substrate is a polyethylene terephthalate (PET) film, the distance between the scraper and the coating substrate is in the range of 0.3 mm to 1.0 mm, and the moving speed of the scraper is in the range of 2.0 to 5.0 mm / s;

[0011] (4) placing the green metal porous nickel film obtained in (3) into an oven for drying, setting a drying program, and peeling off the green metal porous nickel film from the coated substrate after the drying is completed;

[0012] (5) The porous nickel film green body obtained in (4) is placed on an alumina ceramic plate, and an alumina ceramic plate of the same size is placed on it; a pressing block of a certain weight is placed on the top ceramic plate to provide sintering pressure, and then the film green body, the ceramic plate, and the pressing block are placed together in a sintering furnace for sintering. After cooling and taking out of the furnace, a finished metal porous nickel film is obtained.

[0013] As an improvement, the binder for preparing the metal powder slurry is polyvinyl alcohol (PVA); the nickel powder particle size range is 1 to 150 μm, and the solid content range of the nickel powder slurry is 30% to 60%; the minimum thickness value of the formable film is determined by the maximum powder particle size in the powder, and the minimum thickness value is 2 times the maximum powder particle diameter.

[0014] As an improvement, when a flat coater is used for coating, the coating substrate is a PET film, and the thickness of the PET film ranges from 0.1 to 0.3 mm; when coating, the distance between the scraper and the coating substrate ranges from 0.3 mm to 1.0 mm, and the scraper movement speed ranges from 2.0 to 5.0 mm / s.

[0015] As an improvement, when the nickel film green body is dried in step (4), the oven temperature ranges from 40° C. to 80° C., and the drying time ranges from 30 min to 80 min.

[0016] As an improvement, the specific procedure of sintering in step (5) is as follows: the dried metal porous nickel film green body is heated to 240°C to 450°C at a heating rate of 2°C / min to 5°C / min and then kept warm for 40 minutes, then heated to 1000°C to 1200°C at a heating rate of 2°C / min to 5°C / min and then kept warm for 60 minutes, and the sintering atmosphere is vacuum, and the vacuum degree is better than 5×10 - 2 Pa.

[0017] As an improvement, when loading the furnace for sintering, the metal porous nickel film green body needs to be placed between two alumina ceramic plates. The thickness of the ceramic plates above the green body ranges from 1.0mm to 3.0mm. The pressure range provided by the pressing block placed on the top ceramic plate is 0.5kPa-10kPa. The specific pressure value is adjusted according to the specifications of the metal porous nickel film. The larger the specifications of the film green body, the greater the sintering pressure required for sintering.

[0018] As an improvement, the thickness of the porous nickel film prepared by this method is generally in the range of 0.1 mm to 0.8 mm; the material of the porous metal film is not limited to pure nickel, but can also be nickel-based alloy, stainless steel, pure titanium, and titanium alloy.

[0019] As an improvement, the particle size of the metal powder in the coating slurry can be changed and secondary or multiple coating operations can be performed to achieve the preparation of step gradient or continuous gradient metal porous films respectively. The materials of the porous film substrate layer and the gradient layer can be the same or different.

[0020] The present invention relates to a method for preparing a porous metal nickel film. The porous metal nickel film prepared by the method has a thin thickness, uniform pores and high porosity. The film has good tensile strength and flexibility, low surface resistance and contact resistance, and can meet the requirements of supercapacitors and AEM electrolysis hydrogen production devices for the comprehensive performance of porous metal nickel films, and has great application value in the field of new energy.

[0021] The present invention is further described in detail below through the accompanying drawings and examples. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The figure is a process flow chart for preparing a porous nickel film;

[0023] Figure 2 Schematic diagram of loading of metal porous nickel film green body during sintering process, where: 1—ceramic plate, 2—metal porous film green body.

[0024] Figure 3 This is a photo of a porous nickel film: Figure 3 a is a sample with a thickness of 0.1 mm after sintering nickel powder with a particle size of 58 to 95 μm. Figure 3 b is a sample with a thickness of 0.2 mm after sintering nickel powder with a particle size of 1 to 2 μm. Figure 3 c is a sample with a thickness of 0.3 mm after sintering nickel powder with a particle size of 47 to 63 μm;

[0025] Figure 4 This is the SEM photo of the surface of the metal porous nickel film;

[0026] Figure 5 This is the SEM photo of the cross section of the porous nickel film;

[0027] Figure 6 PQ curve of metallic porous nickel film;

[0028] Figure 7 This is the stress-strain curve of porous nickel film. DETAILED DESCRIPTION

[0029] The present invention will be described in detail below in conjunction with the embodiments and drawings, so that those skilled in the art can have a more comprehensive understanding of the present invention. It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not intended to limit the present invention.

[0030] Example 1

[0031] A certain amount of PVA powder was mixed with distilled water in a mass ratio of 8:92, and then a PVA solution with a concentration of 8% was prepared using a magnetic stirrer; 100 g of nickel powder with a particle size range of 95-150 μm was weighed and mixed with the PVA solution, and 1-2 drops of defoaming agent were added to the solution, and the mixture was fully stirred to obtain a metal powder slurry with a solid content of 50%; the slurry was evenly poured on the PET film on the flat coater, and the scraper was turned on for coating at a speed of 2 mm / s, and the distance from the scraper to the PET film was 0.75 mm; after the coating was completed, the prepared green body was placed in an oven for drying, the oven temperature was 60°C, and the drying time was 1 h; after the drying was completed, the green body sample was peeled off the PET film and cut into a size of 40×40 mm; the film green body was placed between two ceramic plates with a thickness of 1.0 mm, and then a press block was placed on the ceramic plate, the pressure provided by the press block was 0.5 kPa, and then placed in a vacuum sintering furnace for sintering: the vacuum degree was better than 5×10 -2 Pa, heating rate is 3℃ / min, heating to 350℃ and then keeping warm for 40min, heating to 1150℃ and then keeping warm for 60min; finally cooling to room temperature with the furnace, a metal porous nickel film with a film thickness of 0.51mm is obtained. The maximum bubbling pore size of the metal porous nickel film is 15.82μm, and the relative permeability coefficient is 1268.79m 3 ·h -1 kPa -1 ·m -2 , tensile strength is 11.06MPa, surface resistance is 0.55mΩ, and contact resistance is 7.51mΩ.

[0032] Example 2

[0033] A certain amount of PVA powder was mixed with distilled water in a mass ratio of 7:93, and then a PVA solution with a concentration of 7% was prepared using a magnetic stirrer; 80 g of nickel powder with a particle size range of 47 to 63 μm was weighed and mixed with the PVA solution, and 1 to 2 drops of defoaming agent were added to the solution, and the mixture was fully stirred to obtain a metal powder slurry with a solid content of 44.4%; the slurry was evenly poured on the PET film on the flat coater, and the scraper was turned on for coating at a speed of 3 mm / s, and the distance from the scraper to the PET film was 0.4 mm; after the coating was completed, the prepared green body was placed in an oven for drying, the oven temperature was 60°C, and the drying time was 1 h; after the drying was completed, the green body sample was peeled off the PET film and cut into a size of 40×40 mm; the film green body was placed between two ceramic plates with a thickness of 1.0 mm, and then a press block was placed on the ceramic plate, the pressure provided by the press block was 1.0 kPa, and then placed in a vacuum sintering furnace for sintering: the vacuum degree was better than 5×10 -2Pa, heating rate is 3℃ / min, heating to 350℃ and then keeping warm for 40min, heating to 1150℃ and then keeping warm for 60min; finally cooling to room temperature with the furnace, a metal porous nickel film with a film thickness of 0.21mm is obtained. The maximum bubbling pore size of the metal porous nickel film is 14.32μm, and the relative permeability coefficient is 2023.18m 3 ·h -1 kPa -1 ·m -2 , tensile strength is 5.14MPa, surface resistance is 1.93mΩ, and contact resistance is 20.35mΩ.

Claims

1. A method for preparing a porous nickel film, characterized in that The preparation process is: Step 1, using distilled water to prepare a polyvinyl alcohol (PVA) solution, the solution concentration range is 5% to 9%; Step 2, mixing the PVA solution prepared in step 1 with Ni powder of a certain particle size range after screening to obtain nickel powder slurry; adding a defoaming agent to the nickel powder slurry and stirring evenly to remove bubbles in the slurry; the nickel powder particle size range is 1 to 150 μm, and the solid content range of the nickel powder slurry is 30% to 60%; Step 3, pouring the nickel powder slurry obtained in step 2 evenly on a flat coater for coating, the coating substrate is a polyethylene terephthalate (PET) film, the distance between the scraper and the coating substrate ranges from 0.3 mm to 1.0 mm, and the scraper moving speed ranges from 2.0 to 5.0 mm / s; Step 4, placing the green metal porous nickel film obtained in step 3 into an oven for drying, setting a drying program, and peeling off the green metal porous nickel film from the coated substrate after the drying is completed; Step 5, placing the porous nickel film green body obtained in step 4 on an alumina ceramic plate, and placing an alumina ceramic plate of the same size on it; placing a certain weight of a pressing block on the top ceramic plate to provide sintering pressure, and then putting the film green body, ceramic plate, and pressing block into a sintering furnace for sintering, and obtaining a finished metal porous nickel film after cooling and taking it out of the furnace.

2. The method for preparing a porous nickel film according to claim 1, characterized in that The binder for preparing the metal powder slurry is polyvinyl alcohol (PVA); the nickel powder particle size range is 1 to 150 μm, and the solid content of the nickel powder slurry ranges from 30% to 60%; the minimum thickness value of the formable film is determined by the maximum powder particle size in the powder, and the minimum thickness value is twice the maximum powder particle diameter.

3. The method for preparing a porous nickel film according to claim 1, characterized in that A flat coater is used for coating, the coating substrate is a PET film, and the thickness of the PET film ranges from 0.1 to 0.3 mm; during coating, the distance between the scraper and the coating substrate ranges from 0.3 mm to 1.0 mm, and the moving speed of the scraper ranges from 2.0 to 5.0 mm / s.

4. The method for preparing a porous nickel film according to claim 1, characterized in that In step 4, the oven temperature range is 40° C. to 80° C., and the drying time range is 30 min to 80 min.

5. The method for preparing a porous nickel film according to claim 1, characterized in that The specific sintering procedure in step 5 is as follows: the dried metal porous nickel film green body is heated to 240°C to 450°C at a heating rate of 2°C / min to 5°C / min and then kept at this temperature for 40 minutes, and then heated to 1000°C to 1200°C at a heating rate of 2°C / min to 5°C / min and then kept at this temperature for 60 minutes. The sintering atmosphere is vacuum, and the vacuum degree is better than 5×10 -2 Pa.

6. The method for preparing a porous nickel film according to claim 5, characterized in that When loading the furnace for sintering, the metal porous nickel film green body needs to be placed between two alumina ceramic plates. The thickness of the ceramic plate above the green body ranges from 1.0mm to 3.0mm. The pressure range provided by the pressing block placed on the top ceramic plate is 0.5kPa-10kPa. The specific pressure value is adjusted according to the specifications of the metal porous nickel film.

7. The method for preparing a porous nickel film according to claim 1, characterized in that The thickness of the porous nickel film prepared by the method ranges from 0.1 mm to 0.8 mm.

8. The method for preparing a porous nickel film according to claim 1, characterized in that The material of the porous metal film is not limited to pure nickel, but may also be nickel-based alloy, stainless steel, pure titanium, or titanium alloy.

9. The method for preparing a porous nickel film according to claim 1, characterized in that The preparation of a stepped gradient or continuous gradient metal porous film can be achieved by changing the particle size of the metal powder in the coating slurry and performing secondary or multiple coating operations. The materials of the porous film substrate layer and the gradient layer can be the same or different.