Preparation method of high-strength environment-friendly bamboo-wood composite shaving board

By introducing titanate coupling groups and phosphorus groups into polyurethane adhesives, the problem of formaldehyde carcinogenicity in particleboard and insufficient bonding performance of bamboo and wood was solved, and bamboo with high strength, environmental protection and flame retardant were prepared. Wood composite particle board.

CN119077882AActive Publication Date: 2024-12-06JIANGXI LULI WOOD CO LTD

Patent Information

Application Number
CN202411417840.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-12-06
Estimated Expiration
2044-10-11

AI Technical Summary

Technical Problem

The formaldehyde carcinogens used in the manufacturing process of existing particle boards have environmental protection problems, and the poor bonding performance of wood materials to bamboo, resulting in insufficient strength and flame retardant properties of particle boards.

Method used

Polyurethane adhesives are used to replace traditional trialdehyde glue, and titanate coupling groups and phosphorus groups are introduced into its molecular chains to modify the polyurethane adhesive to improve the bonding performance and flame retardancy. By pulverizing, Prepare high-strength, environmentally friendly bamboo and wood composite particle board by drying, compounding and hot pressing.

Benefits of technology

The bamboo and wood composite particle board with high strength, environmental protection and flame retardant properties is achieved, which avoids the generation of formaldehyde and improves the bonding effect of bamboo and wood materials and the overall performance of particle board.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005079928110000021
    Figure BDA0005079928110000021
  • Figure BDA0005079928110000031
    Figure BDA0005079928110000031
  • Figure BDA0005079928110000061
    Figure BDA0005079928110000061
Patent Text Reader

Abstract

According to the preparation method of the high-strength environment-friendly bamboo-wood composite shaving board, a more environment-friendly polyurethane adhesive is adopted to replace a traditional three-aldehyde adhesive, and formaldehyde is prevented from being generated, so that the environment-friendly performance of the prepared composite shaving board is improved. And aiming at the use of the bamboo shaving board, the polyurethane adhesive is modified, and a titanate coupling group and a phosphorus-containing group are introduced, so that the adhesive property and the flame retardant property aiming at the bamboo board are improved. The technical effect of improving the strength and flame retardance of the shaving board is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite artificial board processing, and in particular to a method for preparing a high-strength environmentally friendly bamboo-wood composite particle board. Background Art

[0002] With the rapid development of the economy and society, the demand for wood is increasing day by day. However, due to the long production cycle and limited resources of wood, as people continue to strengthen the protection of forest resources, the gap in demand for wood is getting bigger and bigger. In order to solve this problem, people have developed their own alternative resources, including steel, plastic, artificial boards, etc. Artificial boards are made of wood or non-wood plant fibers as the main raw materials, with adhesives and other additives added, and pressed together to form a board or molded product. my country's artificial board industry began in the 1920s and has a history of more than 100 years. Artificial boards are an important way to comprehensively utilize and use wood at a high value. Using artificial boards instead of solid wood saves precious forest resources and is of great significance to ecological protection.

[0003] The types of man-made boards mainly include plywood, density board and particle board. Particle board is mainly made of branches, small diameter wood, processing residues and other raw materials. It is a comprehensive resource utilization product with the advantages of high resource utilization and low processing energy consumption. The products are widely used in home furnishing, decoration, renovation, packaging and other fields. The particle board industry is an important part of the forestry processing industry and one of the pillar industries of the forestry economy.

[0004] The main raw materials of particleboard include wood chips and adhesives. Adhesives are used to bond wood chips together and are the main raw material of particleboard. They have an important influence on the static bending strength, elastic modulus and other properties of particleboard. Adhesives used for particleboard usually include urea-formaldehyde resin adhesives, phenolic resin adhesives and melamine resin adhesives. The raw material formaldehyde used in the above adhesives is a carcinogen. During use, the prepared particleboard will also volatilize a certain amount of formaldehyde, and its use in home furnishings and other fields is restricted.

[0005] Traditional particleboard manufacturing generally uses wood as raw material, which can ensure the performance of the product. Bamboo is a renewable resource with the advantages of high strength and low cost. Mixing bamboo and wood to prepare composite particleboard can improve the strength of particleboard and reduce costs, which has a large development space.

[0006] In view of the shortcomings of the prior art, this application provides a method for preparing a high-strength environmentally friendly bamboo-wood composite particleboard, which is to use a polyurethane adhesive to replace the existing "trialdehyde glue" to avoid the generation of formaldehyde and improve environmental performance. In addition, in view of the technical problem that the bonding performance between wood materials and bamboo is not good, the polyurethane adhesive is modified, and a coupling group is introduced into its molecular chain to improve the bonding effect on bamboo and wood materials. In addition, by introducing a phosphorus-containing group, the flame retardancy of the composite particleboard is improved. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing a high-strength environmentally friendly bamboo-wood composite particleboard, by adopting a more environmentally friendly polyurethane adhesive to replace the traditional "trialdehyde glue" to avoid the generation of formaldehyde, so as to improve the environmental performance of the prepared composite particleboard. In addition, in view of the use of bamboo-wood particleboard, the polyurethane adhesive is modified to introduce a titanate coupling group and a phosphorus-containing group to improve the bonding performance and flame retardant performance for the bamboo-wood board. The technical effect of improving the strength and flame retardancy of the particleboard is obtained.

[0008] The purpose of the present invention is achieved through the following technical solutions:

[0009] The present invention provides a method for preparing a high-strength environmentally friendly bamboo-wood composite particleboard, which is characterized by:

[0010] The following steps are involved:

[0011] Step 1: crush the bamboo material into bamboo raw materials with a particle size of 1-10mm using a crusher;

[0012] Step 2: crush the wood material into wood raw materials with a particle size of 0.2-5 mm using a crusher;

[0013] Step 3: Dry the bamboo raw material and the wood raw material separately to make their moisture content reach 2-10%.

[0014] Step 4: compound the bamboo raw material and the wood raw material in a mass ratio of 1:1, send them into a sizing machine, and apply polyurethane adhesive;

[0015] Step 5: Send the glued mixture to the paving machine for paving, and then undergo pre-pressing, hot pressing, cooling and shaping to obtain a high-strength environmentally friendly bamboo-wood composite particleboard with a thickness of 12-16mm.

[0016] Furthermore, as a preferred technical solution of the present invention, the hot pressing temperature is 160-190°C, the hot pressing time is 25-30s / mm, and the hot pressing pressure is 2-3MPa.

[0017] Further, as a preferred technical solution of the present invention, the raw materials for preparing the polyurethane adhesive are as follows: 40-50 parts of polyether diol, 20-30 parts of polyester diol, 6-12 parts of modified polyether compound, 1-3 parts of 1,4-butanediol, 100 parts of polyphenyl polymethylene polyisocyanate, 0.2-3 parts of catalyst, and 10-30 parts of ethyl acetate;

[0018] The polyphenyl polymethylene polyisocyanate is a mixture of diphenylmethane diisocyanate and polyisocyanate with a functionality greater than 2, with an average functionality of 2.6-2.7 and an NCO% content of 30-32%. The polyphenyl polymethylene polyisocyanate can be purchased through commercial channels, and its trade name is "PAPI".

[0019] Further, as a preferred technical solution of the present invention, the polyether diol is selected from one or more of polyethylene glycol and polypropylene glycol, and the molecular weight range is 600-3000;

[0020] Furthermore, as a preferred technical solution of the present invention, the polyester diol is selected from any one or more of polycaprolactone diol, polyethylene adipate or polybutylene adipate, and has a molecular weight range of 2000-3000.

[0021] Further, as a preferred technical solution of the present invention, the catalyst is bismorpholinyl ethyl ether;

[0022] Furthermore, as a preferred technical solution of the present invention, the preparation process of the modified polyether compound is as follows:

[0023] 1) Add 100-200 ml of solvent oil into a container, then add isooctyl alcohol and polyether N204, then add 0.5% of the reducing agent of the reaction raw materials, then add P2O5, after adding, raise the temperature to 50-60° C., react for 1-2 hours, then remove the solvent by reduced pressure distillation to obtain intermediate product 1;

[0024] 2) Add 100-200 ml of solvent oil into a container, add tetraisopropyl titanate at the same time, stir evenly, then dropwise add the intermediate product 1 at room temperature, react at 80-90° C. for 1-3 hours after the dropwise addition is complete, and then distill under reduced pressure to obtain a modified polyether compound.

[0025] Furthermore, as a preferred technical solution of the present invention, the molar ratio of isooctyl alcohol, polyether N204 and P2O5 is 1:1:1, the mass ratio of the intermediate product 1 to tetraisopropyl titanate is 3:1-1:3; and the reducing agent is sodium phosphite and / or potassium phosphite.

[0026] Further, as a preferred technical solution of the present invention, the reaction of polyether N204 with isooctyl alcohol and tetraisopropyl titanate is carried out according to the following steps:

[0027] Step a:

[0028]

[0029] Step b:

[0030]

[0031] Through the above reaction, the structures of P2O5 and tetraisopropyl titanate are introduced into the polyether molecular chain to form a modified polyether compound. The modified polyether compound not only contains the structure of the titanate coupling agent, but also contains the structure of P2O5. Since the titanate coupling agent can improve the adhesion with the inorganic filler and P2O5 has good flame retardancy, the compound has the characteristics of improving the adhesion and flame retardancy of inorganic materials.

[0032] At the same time, the compound contains a hydroxyl functional group. As a functional modifier, it can be added to the polyurethane adhesive formula and grafted onto the polyurethane molecular chain to prevent the precipitation of phosphorus-containing groups. It can improve the adhesion and flame retardancy of the resulting polyurethane adhesive. When used in bamboo-wood composite particleboard, it can improve the strength and flame retardancy of the resulting particleboard.

[0033] Furthermore, as a preferred technical solution of the present invention, the preparation process of the polyurethane adhesive is as follows:

[0034] 40-50 parts of polyether diol and 20-30 parts of polyester diol are dehydrated and added to a container, and stirred evenly. 100 parts of polyphenyl polymethylene polyisocyanate are added to the container, mixed and heated to 70-80°C, stirred and reacted for 1-2 hours, and then 6-12 parts of modified polyether compound, 1-3 parts of 1,4-butanediol, 0.2-3 parts of catalyst and 10-30 parts of solvent are added, and the stirring reaction is continued for 1-3 hours. The viscosity and NCO% are tested. When the viscosity and NCO% are qualified, the material is discharged, sealed and packaged to obtain the polyurethane adhesive.

[0035] The NCO content of the one-component moisture-curing polyurethane adhesive is 10-12%, the viscosity is 2000-3000 mPa.s at 25°C, and the dosage of the polyurethane adhesive is 30-50 kg / m 3 .

[0036] The polyurethane adhesive prepared by the invention is a moisture-curing polyurethane adhesive with terminal NCO groups, which can undergo a crosslinking reaction with moisture in the air to achieve crosslinking, has low viscosity, does not contain formaldehyde, and has high bonding strength, and is an environmentally friendly and efficient polyurethane adhesive for wood particleboards.

[0037] Beneficial effects of the present invention:

[0038] (1) The present application is directed to modifying polyurethane adhesives for bamboo particleboards, introducing the structures of P2O5 and tetraisopropyl titanate into polyether molecular chains to form a modified polyether compound, which contains not only the structure of a titanate coupling agent but also the structure of P2O5. Since the titanate coupling agent can improve the adhesion to inorganic fillers and P2O5 has good flame retardancy, the compound has the characteristics of improving the adhesion and flame retardancy of inorganic materials. At the same time, the compound contains hydroxyl functional groups, which can be added to the polyurethane adhesive formula as a functional modifier, and can be grafted onto the polyurethane molecular chain to prevent the precipitation of phosphorus-containing groups, thereby improving the adhesion and flame retardancy of the obtained polyurethane adhesive. When applied to bamboo composite particleboards, the strength and flame retardancy of the obtained bamboo composite particleboards can be improved.

[0039] (2) The polyurethane adhesive used in the present application is a moisture-curing polyurethane adhesive with terminal NCO groups, which can undergo a cross-linking reaction with moisture in the air to achieve cross-linking, and has low viscosity, does not contain formaldehyde, and has high bonding strength. It is an environmentally friendly and efficient polyurethane adhesive for wood particleboard. DETAILED DESCRIPTION

[0040] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0041] Example 1

[0042] 1. The preparation process of modified polyether compound is as follows:

[0043] Step 1: Add 100 ml of solvent oil into a container, add 1 mol of isooctyl alcohol and 1 mol of polyether N204 according to the ratio, then add 0.5% by weight of the reducing agent sodium phosphite of the reaction raw materials, and then add 1 mol of P2O5. After the addition, raise the temperature to 55°C, react for 2 hours, and then remove the solvent by reduced pressure distillation to obtain intermediate product 1;

[0044] Step 2: Add 100 ml of solvent oil into a container, add 10 g of tetraisopropyl titanate at the same time, stir evenly, then add 30 g of intermediate product 1 dropwise at room temperature. After the addition is complete, react at 85° C. for 3 h, then distill under reduced pressure to obtain a modified polyether compound.

[0045] 2. The preparation process of polyurethane adhesive is as follows:

[0046] 40g of polyethylene glycol with a molecular weight of 1000 and 30g of polyethylene adipate with a molecular weight of 2000 were dehydrated and added to the container, stirred evenly, 100g of polyphenyl polymethylene polyisocyanate (NCO% content 30%) was added to the container, mixed and heated to 75°C, stirred and reacted for 1.5h, then 6g of modified polyether compound, 3g of 1,4-butanediol, 0.5g of catalyst dimorpholinyl ethyl ether and 20g of ethyl acetate were added, and the stirring reaction continued for 2h. The viscosity and NCO% were tested. After the viscosity and NCO% were qualified, the material was discharged, sealed, and packaged to obtain a one-component moisture-curing polyurethane adhesive. The NCO content of the one-component moisture-curing polyurethane adhesive was 11.3%, and the viscosity at 25°C was 2500mPa.s.

[0047] 3. The preparation method of high-strength environmentally friendly bamboo-wood composite particleboard is as follows:

[0048] Step 1: crush the bamboo material into bamboo raw materials with a particle size of 1-10mm using a crusher;

[0049] Step 2: crush the wood material into wood raw materials with a particle size of 0.2-5 mm using a crusher;

[0050] Step 3: Dry the bamboo raw material and the wood raw material separately to make their moisture content reach 5%.

[0051] Step 4: compound the bamboo raw material and the wood raw material in a mass ratio of 1:1, send them into a sizing machine, and apply the prepared polyurethane adhesive by spraying, wherein the amount of the polyurethane adhesive is 40kg / m3;

[0052] Step 5: Send the glued mixture to the paving machine for paving, and then undergo pre-pressing, hot pressing, cooling and shaping to obtain the high-strength environmentally friendly bamboo-wood composite particleboard with a thickness of 15 mm. The hot pressing temperature is 180°C, the hot pressing time is 25s / mm, and the hot pressing pressure is 2.5MPa.

[0053] Embodiment 2:

[0054] The modified polyether compound prepared in Example 1 was used to prepare the polyurethane adhesive of Example 2, as follows:

[0055] 40g of polyethylene glycol with a molecular weight of 1000 and 30g of polyethylene adipate with a molecular weight of 2000 were dehydrated and added to the container, stirred evenly, 100g of polyphenyl polymethylene polyisocyanate (NCO% content 30%) was added to the container, mixed and heated to 75°C, stirred and reacted for 1.5h, then 8g of modified polyether compound, 3g of 1,4-butanediol, 0.5g of catalyst dimorpholinyl ethyl ether and 20g of ethyl acetate were added, and the stirring reaction continued for 2h. The viscosity and NCO% were tested. After the viscosity and NCO% were qualified, the material was discharged, sealed, and packaged to obtain a one-component moisture-curing polyurethane adhesive. The NCO content of the one-component moisture-curing polyurethane adhesive was 11.2%, and the viscosity at 25°C was 2600mPa.s.

[0056] The preparation method of high-strength environmentally friendly bamboo-wood composite particleboard is as follows:

[0057] Step 1: crush the bamboo material into bamboo raw materials with a particle size of 1-10mm using a crusher;

[0058] Step 2: crush the wood material into wood raw materials with a particle size of 0.2-5 mm using a crusher;

[0059] Step 3: Dry the bamboo raw material and the wood raw material separately to make their moisture content reach 5%.

[0060] Step 4: compound the bamboo raw material and the wood raw material in a mass ratio of 1:1, send them into a sizing machine, and apply the prepared polyurethane adhesive by spraying, wherein the amount of the polyurethane adhesive is 40kg / m3;

[0061] Step 5: Send the glued mixture to the paving machine for paving, and then undergo pre-pressing, hot pressing, cooling and shaping to obtain the high-strength environmentally friendly bamboo-wood composite particleboard with a thickness of 15 mm. The hot pressing temperature is 180°C, the hot pressing time is 25s / mm, and the hot pressing pressure is 2.5MPa.

[0062] Embodiment 3:

[0063] The modified polyether compound prepared in Example 1 was used to prepare the polyurethane adhesive of Example 3, as follows:

[0064] 40g of polyethylene glycol with a molecular weight of 1000 and 30g of polyethylene adipate with a molecular weight of 2000 are dehydrated and added to the container, stirred evenly, 100g of polyphenyl polymethylene polyisocyanate (NCO% content 30%) is added to the container, mixed and heated to 75°C, stirred and reacted for 1.5h, then 12g of modified polyether compound, 3g of 1,4-butanediol, 0.5g of catalyst dimorpholinyl ethyl ether and 20g of ethyl acetate are added, and the stirring reaction is continued for 2h. Test the viscosity and NCO%, and after the viscosity and NCO% are qualified, discharge, seal, and package to obtain a one-component moisture-curing polyurethane adhesive. The NCO content of the one-component moisture-curing polyurethane adhesive is 11.0%, and the viscosity at 25°C is 2550mPa.s.

[0065] The preparation method of high-strength environmentally friendly bamboo-wood composite particleboard is as follows:

[0066] Step 1: crush the bamboo material into bamboo raw materials with a particle size of 1-10mm using a crusher;

[0067] Step 2: crush the wood material into wood raw materials with a particle size of 0.2-5 mm using a crusher;

[0068] Step 3: Dry the bamboo raw material and the wood raw material separately to make their moisture content reach 5%.

[0069] Step 4: compound the bamboo raw material and the wood raw material in a mass ratio of 1:1, send them into a sizing machine, and apply the prepared polyurethane adhesive by spraying, wherein the amount of the polyurethane adhesive is 40kg / m3;

[0070] Step 5: Send the glued mixture to the paving machine for paving, and then undergo pre-pressing, hot pressing, cooling and shaping to obtain the high-strength environmentally friendly bamboo-wood composite particleboard with a thickness of 15 mm. The hot pressing temperature is 180°C, the hot pressing time is 25s / mm, and the hot pressing pressure is 2.5MPa.

[0071] Comparative Example 1:

[0072] The preparation process of polyurethane adhesive is as follows:

[0073] 40g of polyethylene glycol with a molecular weight of 1000 and 30g of polyethylene adipate with a molecular weight of 2000 were dehydrated and added to the container, stirred evenly, 100g of polyphenyl polymethylene polyisocyanate (NCO% content 30%) was added to the container, mixed and heated to 75°C, stirred and reacted for 1.5h, then 3g of 1,4-butanediol, 0.5g of catalyst bismorpholinyl ethyl ether and 20g of ethyl acetate were added, and the stirring reaction continued for 2h. The viscosity and NCO% were tested. After the viscosity and NCO% were qualified, the material was discharged, sealed, and packaged to obtain a one-component moisture-curing polyurethane adhesive. The NCO content of the one-component moisture-curing polyurethane adhesive was 11.4%, and the viscosity at 25°C was 2550mPa.s.

[0074] The preparation method of high-strength environmentally friendly bamboo-wood composite particleboard is as follows:

[0075] Step 1: crush the bamboo material into bamboo raw materials with a particle size of 1-10mm using a crusher;

[0076] Step 2: crush the wood material into wood raw materials with a particle size of 0.2-5 mm using a crusher;

[0077] Step 3: Dry the bamboo raw material and the wood raw material separately to make their moisture content reach 5%.

[0078] Step 4: Take the bamboo raw material and the wood raw material in a mass ratio of 1:1, send them into a sizing machine, and apply the prepared polyurethane adhesive by spraying. The amount of the polyurethane adhesive is 40kg / m 3 ;

[0079] Step 5: Send the glued mixture to the paving machine for paving, and then undergo pre-pressing, hot pressing, cooling and shaping to obtain the high-strength environmentally friendly bamboo-wood composite particleboard with a thickness of 15 mm. The hot pressing temperature is 180°C, the hot pressing time is 25s / mm, and the hot pressing pressure is 2.5MPa.

[0080] Comparative Example 2:

[0081] The modified polyether compound prepared in Example 1 was used to prepare the polyurethane adhesive of Comparative Example 2, as follows:

[0082] 40g of polyethylene glycol with a molecular weight of 1000 and 30g of polyethylene adipate with a molecular weight of 2000 are dehydrated and added to the container, stirred evenly, 100g of polyphenyl polymethylene polyisocyanate (NCO% content 30%) is added to the container, mixed and heated to 75°C, stirred and reacted for 1.5h, then 15g of modified polyether compound, 3g of 1,4-butanediol, 0.5g of catalyst dimorpholinyl ethyl ether and 20g of ethyl acetate are added, and the stirring reaction is continued for 2h. Test the viscosity and NCO%, and after the viscosity and NCO% are qualified, discharge, seal, and package to obtain a one-component moisture-curing polyurethane adhesive. The NCO content of the one-component moisture-curing polyurethane adhesive is 11.0%, and the viscosity at 25°C is 2600mPa.s.

[0083] The preparation method of high-strength environmentally friendly bamboo-wood composite particleboard is as follows:

[0084] Step 1: crush the bamboo material into bamboo raw materials with a particle size of 1-10mm using a crusher;

[0085] Step 2: crush the wood material into wood raw materials with a particle size of 0.2-5 mm using a crusher;

[0086] Step 3: Dry the bamboo raw material and the wood raw material separately to make their moisture content reach 5%.

[0087] Step 4: compound the bamboo raw material and the wood raw material in a mass ratio of 1:1, send them into a sizing machine, and apply the prepared polyurethane adhesive by spraying, wherein the amount of the polyurethane adhesive is 40kg / m3;

[0088] Step 5: Send the glued mixture to the paving machine for paving, and then undergo pre-pressing, hot pressing, cooling and shaping to obtain the high-strength environmentally friendly bamboo-wood composite particleboard with a thickness of 15 mm. The hot pressing temperature is 180°C, the hot pressing time is 25s / mm, and the hot pressing pressure is 2.5MPa.

[0089] Performance Testing:

[0090] The edges were trimmed with a circular saw and then sawn into small pieces of 50×50 mm and 300×50 mm. The elastic modulus, static bending strength, internal bonding strength, and formaldehyde content (perforation method) of the high-strength environmentally friendly bamboo-wood composite particleboard were tested in accordance with GB / T17657-2013 "Test methods for physical and chemical properties of wood-based panels and veneer wood-based panels". The oxygen index of the high-strength environmentally friendly bamboo-wood composite particleboard was tested in accordance with GB / T2406-93. The results are shown in Table 1.

[0091] Table 1:

[0092]

[0093] According to the experimental results of Table 1, the high-strength environmentally friendly bamboo-wood composite particleboard prepared by the present application does not contain formaldehyde and has high environmental protection. By comparing Example 1 with Comparative Example 1, it is explained that the modified polyether compound containing the structure of the titanate coupling agent and the P2O5 structure prepared by the present application is added to the moisture-curing polyurethane adhesive system and applied to the bamboo-wood composite particleboard, which can improve the internal bonding strength, static bending strength and elastic modulus of the bamboo-wood composite particleboard. At the same time, the flame retardancy of the bamboo-wood composite particleboard can also be improved. By comparing Example 1 with Comparative Example 2, it is explained that the amount of the modified polyether compound also has a certain degree of influence on the performance of the bamboo-wood composite particleboard. Excessive amount is not conducive to the improvement of the strength of the bamboo-wood composite particleboard.

[0094] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0095] The above contents are merely examples and explanations of the concept of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the defined scope, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a high-strength environmentally friendly bamboo-wood composite particleboard, characterized in that: The following steps are involved: Step 1: crush the bamboo material into bamboo raw materials with a particle size of 1-10mm using a crusher; Step 2: crush the wood material into wood raw materials with a particle size of 0.2-5 mm using a crusher; Step 3: Drying the bamboo raw material and the wood raw material respectively to make their moisture content reach 2-10%; Step 4: compound the bamboo raw material and the wood raw material in a mass ratio of 1:1, send them into a sizing machine, and apply polyurethane adhesive; Step 5: Send the glued mixture to a paving machine for paving, and then undergo pre-pressing, hot pressing, cooling and shaping to obtain the high-strength environmentally friendly bamboo-wood composite particleboard with a thickness of 12-16 mm; The raw materials for preparing the polyurethane adhesive are as follows: 40-50 parts of polyether diol, 20-30 parts of polyester diol, 6-12 parts of modified polyether compound, 1-3 parts of 1,4-butanediol, 100 parts of polyphenyl polymethylene polyisocyanate, 0.2-3 parts of catalyst, and 10-30 parts of ethyl acetate; The preparation process of the modified polyether compound is as follows: 1) Add 100-200 ml of solvent oil into a container, then add isooctyl alcohol and polyether N204, then add 0.5% of the reducing agent of the reaction raw materials, then add P2O5, after adding, raise the temperature to 50-60° C., react for 1-2 hours, then remove the solvent by reduced pressure distillation to obtain intermediate product 1; 2) Add 100-200 ml of solvent oil into a container, add tetraisopropyl titanate at the same time, stir evenly, then dropwise add the intermediate product 1 at room temperature, react at 80-90° C. for 1-3 hours after the dropwise addition is complete, and then distill under reduced pressure to obtain a modified polyether compound; The molar ratio of isooctyl alcohol, polyether N204 and P2O5 is 1:1:1, the mass ratio of the intermediate product 1 to tetraisopropyl titanate is 3:1-1:3, and the reducing agent is sodium phosphite and / or potassium phosphite.

2. The method for preparing a high-strength environmentally friendly bamboo-wood composite particleboard according to claim 1, characterized in that: The preparation process of the polyurethane adhesive is as follows: 40-50 parts of polyether diol and 20-30 parts of polyester diol are dehydrated and added to a container, and stirred evenly. 100 parts of polyphenyl polymethylene polyisocyanate are added to the container, mixed and heated to 70-80°C, stirred and reacted for 1-2 hours, and then 6-12 parts of modified polyether compound, 1-3 parts of 1,4-butanediol, 0.2-3 parts of catalyst and 10-30 parts of solvent are added, and the stirring reaction is continued for 1-3 hours. The viscosity and NCO% are tested. When the viscosity and NCO% are qualified, the material is discharged, sealed and packaged to obtain the polyurethane adhesive.

3. The method for preparing a high-strength environmentally friendly bamboo-wood composite particleboard according to claim 1, characterized in that: The hot pressing temperature is 160-190° C., the hot pressing time is 25-30 s / mm, and the hot pressing pressure is 2-3 MPa.

4. The method for preparing a high-strength environmentally friendly bamboo-wood composite particleboard according to claim 1, characterized in that: The NCO content of the polyurethane adhesive is 10-12%, the viscosity at 25°C is 2000-3000 mPa.s, and the amount of the polyurethane adhesive is 30-50 kg / m 3 .

Citation Information

Patent Citations

  • Manufacturing method for bamboo-wood composite super chipboard

    CN107756586A

  • Solvent-free single-component moisture-curable polyurethane adhesive for paper-plastic compounding and preparation method thereof

    CN112708386A

  • Preparation method of phosphorus-containing flame retardant

    CN113292596A

  • Single-component halogen-free flame-retardant silane modified polyurethane sealant and preparation method thereof

    CN114250055A

  • Adhesive and preparation method thereof

    CN116285852A

Cited By

  • Bamboo-wood composite shaving board and preparation method thereof

    CN120439414A