Active lime additive and preparation method thereof
By using active lime additives of specific compositions, the problems of slow changes in concrete strength and difficult construction in low temperature and low humidity environments are solved, which significantly improves the early strength, durability and permeability of concrete and improves construction properties.
Patent Information
- Application Number
- CN202411585527.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-08
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In low temperature and low humidity environments, the hydration reaction rate of traditional concrete slows down, resulting in slow changes in concrete strength, impact on construction progress and quality, and easy to cause problems such as freeze-thaw cycle failure, dry cracking and reduced permeability.
It consists of artificial stone, ceramics, natural stone, activated lime, ore powder, sodium aluminum silicate, trimethylolpropane, alkyl alcohol polyoxyethylene ether, sodium anthraquinone-1-sulfonate and benzoyl peroxide. The activated lime additive is decomposed and fired through the feeding system to obtain the activated lime additive, which improves the strength, durability, permeability and construction properties of the concrete.
It significantly improves the early strength, durability, permeability and frost resistance of concrete, improves construction properties, reduces the damage and dry cracks of freeze-thaw cycles, and improves the density and flowability of concrete.
Smart Images

Figure CN119080419A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of active lime additives, in particular to an active lime additive and a preparation method thereof. Background Art
[0002] Active lime is often used as an additive in the preparation of concrete because of its high water activity, low bulk density, high porosity and large specific surface area. It is used to improve the strength of concrete, especially its early strength. Ingredients such as calcium oxide and calcium hydroxide in active lime participate in the hydration reaction of concrete, promote the formation of a solid structure, or significantly increase the compressive strength of concrete. At the same time, active lime can also fill small pores in concrete, reduce the leakage rate and water loss rate of concrete, and extend the service life of concrete.
[0003] When faced with low temperature and low humidity environments such as plateaus, the hydration reaction rate of cement in traditional concrete slows down significantly, resulting in slow changes in concrete strength, affecting construction progress and concrete quality; at the same time, in low temperature and low humidity environments, the concrete mixture is viscous and has poor fluidity, making construction operations difficult; after construction, in long-term low temperature and low humidity environments, freeze-thaw cycle damage, cracking, and decreased impermeability are prone to occur, resulting in reduced strength and durability.
[0004] Therefore, it is of great significance to study an active lime additive and a preparation method to solve the above-mentioned problems in the construction and application of concrete. Summary of the invention
[0005] The object of the present invention is to provide an active lime additive and a preparation method thereof to solve the problems raised in the above background technology.
[0006] To achieve the above object, the present invention provides the following technical solution: an active lime additive, which is made of the following components: by weight, 20-40 parts of a mixed component A, 20-40 parts of a mixed component B, 20-40 parts of a mixed component C and 20-40 parts of a mixed component D, wherein: The mixed component A comprises the following components: by weight, 15-30 parts of artificial stone, 15-30 parts of ceramic and 25-40 parts of natural stone; The mixed component B comprises the following components: by weight, 20-35 parts of active lime, 10-20 parts of mineral powder and 10-20 parts of sodium aluminum silicate; The mixed component C comprises the following components: by weight, 20-30 parts of anthraquinone-1-sodium sulfonate, 15-40 parts of trimethylolpropane, 15-40 parts of alkyl alcohol polyoxyethylene ether and 20-30 parts of benzoyl peroxide; The mixed component D comprises the following components: 10-20 parts of zeolite powder and 10-20 parts of silica fume, by weight.
[0007] In a preferred embodiment, the mixed component A comprises the following components: 25 parts of artificial stone, 25 parts of ceramic and 25 parts of natural stone, by weight; the mixed component B comprises the following components: 35 parts of active lime, 10 parts of mineral powder and 20 parts of sodium aluminum silicate, by weight; the mixed component C comprises the following components: 30 parts of trimethylolpropane, 30 parts of alkyl alcohol polyoxyethylene ether, 20 parts of benzoyl peroxide and 20 parts of sodium anthraquinone-1-sulfonate, by weight; and the mixed component D comprises the following components: 10 parts of zeolite powder and 10 parts of silica fume, by weight.
[0008] In a preferred embodiment, the mixed component A comprises the following components: 15 parts of artificial stone, 15 parts of ceramic and 30 parts of natural stone, by weight; the mixed component B comprises the following components: 35 parts of active lime, 20 parts of mineral powder and 10 parts of sodium aluminum silicate, by weight; the mixed component C comprises the following components: 25 parts of trimethylolpropane, 35 parts of alkyl alcohol polyoxyethylene ether, 20 parts of benzoyl peroxide and 20 parts of sodium anthraquinone-1-sulfonate, by weight; and the mixed component D comprises the following components: 20 parts of zeolite powder and 10 parts of silica fume, by weight.
[0009] In a preferred embodiment, the mixed component A comprises the following components: 20 parts of artificial stone, 20 parts of ceramic and 30 parts of natural stone, by weight; the mixed component B comprises the following components: 35 parts of active lime, 15 parts of mineral powder and 15 parts of sodium aluminum silicate, by weight; the mixed component C comprises the following components: 25 parts of trimethylolpropane, 15 parts of alkyl alcohol polyoxyethylene ether, 30 parts of benzoyl peroxide and 30 parts of sodium anthraquinone-1-sulfonate, by weight; and the mixed component D comprises the following components: 10 parts of zeolite powder and 20 parts of silica fume, by weight.
[0010] In a preferred embodiment, the mixed component A comprises the following components: 30 parts of artificial stone, 20 parts of ceramic and 25 parts of natural stone, by weight; the mixed component B comprises the following components: 35 parts of active lime, 20 parts of mineral powder and 20 parts of sodium aluminum silicate, by weight; the mixed component C comprises the following components: 20 parts of trimethylolpropane, 30 parts of alkyl alcohol polyoxyethylene ether, 30 parts of benzoyl peroxide and 20 parts of sodium anthraquinone-1-sulfonate, by weight; and the mixed component D comprises the following components: 10 parts of zeolite powder and 20 parts of silica fume, by weight.
[0011] A method for preparing an active lime additive comprises the following steps: Step 1, preparing raw materials: preparing mixed component A, mixed component B, mixed component C and mixed component D respectively and feeding them into the feeding system; Step 2, decomposition and calcination: the materials in the feeding system are preheated by the multi-stage cyclone preheating system and then sent to the decomposition furnace to be calcined into active lime. The main control temperature of the decomposition furnace is 850-950℃; the calcination time is 3-5 seconds; Step 3: Product cooling: After cooling in a multi-stage cyclone cooler, the active lime additive is obtained.
[0012] Furthermore, the specific process for preparing the mixed component B in the step 1 is to weigh 20-35 parts of active lime, 10-20 parts of mineral powder and 10-20 parts of sodium aluminum silicate by weight, add a certain amount of deionized water into a stirred reactor and stir thoroughly, let it stand for 48-72 hours at 70°C±5°C and 85%-95% humidity, and grind it after drying at 85-98°C.
[0013] Furthermore, the specific process for preparing the mixed component C in step 1 is to weigh 15-40 parts of trimethylolpropane, 15-40 parts of alkyl alcohol polyoxyethylene ether, 20-30 parts of benzoyl peroxide and 20-30 parts of sodium anthraquinone-1-sulfonate by weight, add a certain amount of deionized water, and mix well to obtain a mixed solution.
[0014] Furthermore, the specific process for preparing the mixed component D in step 1 is as follows: pouring deionized water into 10-20 parts of zeolite powder, stirring evenly to obtain zeolite powder slurry, ball-milling the zeolite powder slurry and 10-20 parts of silica fume, and then dispersing and sieving at a temperature of 85-98°C.
[0015] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides an active lime additive and a preparation method thereof. The components work together to significantly improve the strength, durability, impermeability, frost resistance and workability of concrete. Artificial stone, ceramic and natural stone, as inorganic mineral materials, have good hardness and stability, and increase the basic strength and durability of concrete. Mineral materials can form a dense microstructure in concrete, reduce porosity and improve the compactness of concrete. Components such as calcium oxide and calcium hydroxide in active lime participate in the hydration reaction of concrete, promote the formation of a solid structure and increase the strength of concrete. Mineral powder and sodium aluminum silicate can fill the tiny pores in concrete, improve the pore structure of concrete, and improve its compactness and impermeability.
[0016] Surfactants such as trimethylolpropane and alkyl alcohol polyoxyethylene ether can accelerate the hydration reaction of cement, especially under low temperature conditions, and help improve the early strength of concrete.
[0017] Anthraquinone-1-sulfonate sodium forms a tiny mesh structure in concrete or fills the pores of concrete through its special chemical structure, thereby reducing the space for water to freeze and expand at low temperatures, and reducing the destructive force of concrete caused by freezing and expansion. It improves the compactness of concrete, reduces permeability, and makes it more difficult for water to penetrate into the interior of concrete, thereby further enhancing its frost resistance. In a low-humidity environment, the water on the surface of concrete tends to evaporate quickly, causing the surface of the concrete to dry and crack. Anthraquinone-1-sulfonate sodium has a certain water retention performance, which can slow down the evaporation rate of water on the surface of concrete to a certain extent, thereby reducing the occurrence of dry cracking. Anthraquinone-1-sulfonate sodium, as a concrete additive, promotes the hydration reaction process of cement by chemically reacting with certain components in cement. At low temperatures, the hydration reaction rate of cement will slow down, and the addition of additives will accelerate this process to a certain extent, so that concrete can quickly reach a certain strength at low temperatures. Sodium anthraquinone-1-sulfonate forms a protective film on the surface of concrete, which can block the impact of rapid changes in external humidity on the internal structure of concrete, maintain the relative stability of the internal humidity of concrete, and thus reduce stress concentration and damage caused by humidity changes. When constructed in a low-temperature and low-humidity environment, concrete is prone to problems such as sticky mixtures and poor fluidity. The addition of sodium anthraquinone-1-sulfonate improves the physical properties and chemical effects of concrete, improves its construction performance at low temperatures, and enables concrete to maintain good fluidity and plasticity at low temperatures.
[0018] Chemical additives such as benzoyl peroxide react with cement components to form a more stable chemical structure, improving the durability of concrete. Zeolite powder and silica fume have fine particle structures that can fill smaller pores in concrete, further improving the density of concrete.
[0019] Mineral admixtures such as silica fume can produce volcanic ash reaction in concrete, generate more hydration products, and enhance the strength and durability of concrete. Appropriate amount of mineral admixture improves the workability of concrete, increases fluidity, and reduces bleeding and segregation. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is a flow chart of the present invention; Figure 2 The present invention is a detailed flow chart of a method for preparing an active lime additive. DETAILED DESCRIPTION
[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Embodiment 1:
[0022] See also Figure 1 The present invention provides an active lime additive, which comprises the following components: by weight, 20 parts of a mixed component A, 20 parts of a mixed component B, 20 parts of a mixed component C and 20 parts of a mixed component D, wherein the mixed component A comprises the following components: by weight, 15 parts of artificial stone, 15 parts of ceramics and 25 parts of natural stone, the mixed component B comprises the following components: by weight, 20 parts of active lime, 10 parts of mineral powder and 10 parts of sodium aluminum silicate, the mixed component C comprises the following components: by weight, 15 parts of trimethylolpropane, 15 parts of alkyl alcohol polyoxyethylene ether, 20 parts of benzoyl peroxide and 20 parts of sodium anthraquinone-1-sulfonate, and the mixed component D comprises the following components: by weight, 10 parts of zeolite powder and 10 parts of silica fume. RO-(CH2CH2O) of alkyl alcohol polyoxyethylene ether n H and R are alkyl chains, n is the degree of polymerization of ethylene oxide, and the alkyl alcohol polyoxyethylene ether with n>15 is selected in this embodiment.
[0023] The present invention provides a method for preparing an additive of active lime, comprising the following steps: Step 1, prepare raw materials: prepare mixed component A, mixed component B, mixed component C and mixed component D respectively and put them into the feeding system; the specific process for preparing mixed component B is to weigh 20 parts of active lime, 10 parts of mineral powder and 10 parts of sodium aluminum silicate by weight, add a certain amount of deionized water into a stirred reactor and stir thoroughly, stand for 48-72 hours at 70℃±5℃ and humidity 85%-95%, dry at 85-98℃ and grind to obtain. The specific process for preparing mixed component C is to weigh 15 parts of trimethylolpropane, 15 parts of alkyl alcohol polyoxyethylene ether, 20 parts of benzoyl peroxide and 20 parts of anthraquinone-1-sulfonic acid sodium by weight, add a certain amount of deionized water, and mix evenly to obtain a mixed solution. The specific process for preparing the mixed component D is as follows: pouring deionized water into 10 parts of zeolite powder, stirring evenly to obtain a zeolite powder slurry, ball-milling the zeolite powder slurry and 10 parts of silica fume, and then dispersing and sieving at a temperature of 85-98° C. to obtain a modified active lime mineral admixture.
[0024] Step 2, decomposition and calcination: the materials in the feeding system are preheated by the multi-stage cyclone preheating system and then sent to the decomposition furnace to be calcined into active lime additive. The main control temperature of the decomposition furnace is 850-950℃; the calcination time is 3-5 seconds; Step 3: Product cooling: After cooling in a multi-stage cyclone cooler, the active lime additive is obtained. Embodiment 2:
[0025] In this embodiment, the active lime additive includes the following components: by weight, 40 parts of mixed component A, 40 parts of mixed component B, 40 parts of mixed component C and 40 parts of mixed component D, the mixed component A includes the following components: by weight, 25 parts of artificial stone, 25 parts of ceramic and 25 parts of natural stone, the mixed component B includes the following components: by weight, 35 parts of active lime, 10 parts of mineral powder and 20 parts of sodium aluminum silicate, the mixed component C includes the following components: by weight, 30 parts of trimethylolpropane, 30 parts of alkyl alcohol polyoxyethylene ether, 20 parts of benzoyl peroxide and 20 parts of sodium anthraquinone-1-sulfonate, and the mixed component D includes the following components: by weight, 10 parts of zeolite powder and 10 parts of silica fume.
[0026] The specific preparation process is as follows: Step 1, preparing raw materials: preparing mixed component A, mixed component B, mixed component C and mixed component D respectively and feeding them into the feeding system; The specific process for preparing mixed component B is to weigh 35 parts of active lime, 10 parts of mineral powder and 20 parts of sodium aluminum silicate by weight, add a certain amount of deionized water into a stirred reactor and stir thoroughly, let it stand for 48-72 hours at 70℃±5℃ and humidity 85%-95%, and grind it after drying at 85-98℃.
[0027] The specific process for preparing the mixed component C is as follows: 30 parts of trimethylolpropane, 30 parts of alkyl alcohol polyoxyethylene ether, 20 parts of benzoyl peroxide and 20 parts of sodium anthraquinone-1-sulfonate are weighed by weight, a certain amount of deionized water is added, and the mixture is mixed uniformly to obtain a mixed solution.
[0028] The specific process for preparing the mixed component D is as follows: pouring deionized water into 10 parts of zeolite powder, stirring evenly to obtain a zeolite powder slurry, ball-milling the zeolite powder slurry and 10 parts of silica fume, and then dispersing and sieving at a temperature of 85-98° C. to obtain a modified active lime mineral admixture.
[0029] Step 2, decomposition and calcination: the materials in the feeding system are preheated by the multi-stage cyclone preheating system and then sent to the decomposition furnace to be calcined into active lime additive. The main control temperature of the decomposition furnace is 850-950℃; the calcination time is 3-5 seconds; Step 3: Product cooling: After cooling in a multi-stage cyclone cooler, the active lime additive is obtained. Embodiment 3:
[0030] In this embodiment, the active lime additive includes the following components: by weight, 30 parts of mixed component A, 25 parts of mixed component B, 30 parts of mixed component C and 25 parts of mixed component D. The mixed component A includes the following components: by weight, 15 parts of artificial stone, 15 parts of ceramic and 30 parts of natural stone. The mixed component B includes the following components: by weight, 35 parts of active lime, 20 parts of mineral powder and 10 parts of sodium aluminum silicate. The mixed component C includes the following components: by weight, 25 parts of trimethylolpropane, 35 parts of alkyl alcohol polyoxyethylene ether, 20 parts of benzoyl peroxide and 20 parts of sodium anthraquinone-1-sulfonate. The mixed component D includes the following components: by weight, 20 parts of zeolite powder and 10 parts of silica fume.
[0031] The specific preparation process is as follows: Step 1, preparing raw materials: preparing mixed component A, mixed component B, mixed component C and mixed component D respectively and feeding them into the feeding system; The specific process for preparing mixed component B is to weigh 35 parts of active lime, 20 parts of mineral powder and 10 parts of sodium aluminum silicate by weight, add a certain amount of deionized water into a stirred reactor and stir thoroughly, let it stand for 48-72 hours at 70℃±5℃ and humidity 85%-95%, and grind it after drying at 85-98℃.
[0032] The specific process for preparing the mixed component C is as follows: 25 parts of trimethylolpropane, 35 parts of alkyl alcohol polyoxyethylene ether, 20 parts of benzoyl peroxide and 20 parts of sodium anthraquinone-1-sulfonate are weighed by weight, a certain amount of deionized water is added, and the mixture is mixed evenly to obtain a mixed solution.
[0033] The specific process for preparing the mixed component D is as follows: pouring deionized water into 120 parts of zeolite powder, stirring evenly to obtain a zeolite powder slurry, ball-milling the zeolite powder slurry and 10 parts of silica fume, and then dispersing and sieving at a temperature of 85-98° C. to obtain a modified active lime mineral admixture.
[0034] Step 2, decomposition and calcination: the materials in the feeding system are preheated by the multi-stage cyclone preheating system and then sent to the decomposition furnace to be calcined into active lime additive. The main control temperature of the decomposition furnace is 850-950℃; the calcination time is 3-5 seconds; Step 3: Product cooling: After cooling in a multi-stage cyclone cooler, the active lime additive is obtained. Embodiment 4:
[0035] In this embodiment, the active lime additive includes the following components: by weight, 30 parts of mixed component A, 35 parts of mixed component B, 25 parts of mixed component C and 28 parts of mixed component D. The mixed component A includes the following components: by weight, 20 parts of artificial stone, 20 parts of ceramic and 30 parts of natural stone. The mixed component B includes the following components: by weight, 35 parts of active lime, 15 parts of mineral powder and 15 parts of sodium aluminum silicate. The mixed component C includes the following components: by weight, 25 parts of trimethylolpropane, 15 parts of alkyl alcohol polyoxyethylene ether, 30 parts of benzoyl peroxide and 30 parts of sodium anthraquinone-1-sulfonate. The mixed component D includes the following components: by weight, 10 parts of zeolite powder and 20 parts of silica fume.
[0036] The specific preparation process is as follows: Step 1, preparing raw materials: preparing mixed component A, mixed component B, mixed component C and mixed component D respectively and feeding them into the feeding system; The specific process for preparing mixed component B is to weigh 35 parts of active lime, 15 parts of mineral powder and 15 parts of sodium aluminum silicate by weight, add a certain amount of deionized water into a stirred reactor and stir thoroughly, let it stand for 48-72 hours at 70℃±5℃ and humidity 85%-95%, and grind it after drying at 85-98℃.
[0037] The specific process for preparing the mixed component C is as follows: 25 parts of trimethylolpropane, 15 parts of alkyl alcohol polyoxyethylene ether, 30 parts of benzoyl peroxide and 30 parts of sodium anthraquinone-1-sulfonate are weighed by weight, a certain amount of deionized water is added, and the mixture is mixed uniformly to obtain a mixed solution.
[0038] The specific process for preparing the mixed component D is as follows: pouring deionized water into 10 parts of zeolite powder, stirring evenly to obtain a zeolite powder slurry, ball-milling the zeolite powder slurry and 20 parts of silica fume, and then dispersing and sieving at a temperature of 85-98° C. to obtain a modified active lime mineral admixture.
[0039] Step 2, decomposition and calcination: the materials in the feeding system are preheated by the multi-stage cyclone preheating system and then sent to the decomposition furnace to be calcined into active lime additive. The main control temperature of the decomposition furnace is 850-950℃; the calcination time is 3-5 seconds; Step 3: Product cooling: After cooling in a multi-stage cyclone cooler, the active lime additive is obtained. Embodiment 5:
[0040] In this embodiment, the active lime additive includes the following components: by weight, 22 parts of mixed component A, 26 parts of mixed component B, 28 parts of mixed component C and 33 parts of mixed component D. The mixed component A includes the following components: by weight, 30 parts of artificial stone, 20 parts of ceramic and 25 parts of natural stone. The mixed component B includes the following components: by weight, 35 parts of active lime, 20 parts of mineral powder and 20 parts of sodium aluminum silicate. The mixed component C includes the following components: by weight, 20 parts of trimethylolpropane, 30 parts of alkyl alcohol polyoxyethylene ether, 30 parts of benzoyl peroxide and 20 parts of sodium anthraquinone-1-sulfonate. The mixed component D includes the following components: by weight, 10 parts of zeolite powder and 20 parts of silica fume.
[0041] The specific preparation process is as follows: Step 1, preparing raw materials: preparing mixed component A, mixed component B, mixed component C and mixed component D respectively and feeding them into the feeding system; The specific process for preparing mixed component B is to weigh 35 parts of active lime, 20 parts of mineral powder and 20 parts of sodium aluminum silicate by weight, add a certain amount of deionized water into a stirred reactor and stir thoroughly, let it stand for 48-72 hours at 70℃±5℃ and humidity 85%-95%, and grind it after drying at 85-98℃.
[0042] The specific process for preparing the mixed component C is as follows: 20 parts of trimethylolpropane, 30 parts of alkyl alcohol polyoxyethylene ether, 30 parts of benzoyl peroxide and 20 parts of sodium anthraquinone-1-sulfonate are weighed by weight, a certain amount of deionized water is added, and the mixture is mixed uniformly to obtain a mixed solution.
[0043] The specific process for preparing the mixed component D is as follows: pouring deionized water into 10 parts of zeolite powder, stirring evenly to obtain a zeolite powder slurry, ball-milling the zeolite powder slurry and 20 parts of silica fume, and then dispersing and sieving at a temperature of 85-98° C. to obtain a modified active lime mineral admixture.
[0044] Step 2, decomposition and calcination: the materials in the feeding system are preheated by the multi-stage cyclone preheating system and then sent to the decomposition furnace to be calcined into active lime additive. The main control temperature of the decomposition furnace is 850-950℃; the calcination time is 3-5 seconds; Step 3: Product cooling: After cooling in a multi-stage cyclone cooler, the active lime additive is obtained.
[0045] Comparative Example 1: In this comparative example, the mixed component C is not added to the composition of the active lime additive, and the other components and the preparation process are the same as those in Example 1.
[0046] Comparative Example 2: In this comparative example, sodium anthraquinone-1-sulfonate was not added to the mixed component C of the active lime additive, and other components and preparation process were the same as those in Example 1.
[0047] The active lime additives prepared in Example 1 to Example 5 and Comparative Example 1 to Comparative Example 2 were used together with water, cement, sand and recycled aggregate to make cubic concrete test blocks of 150 mm×150 mm×150 mm, which were numbered SC1, SC2, SC3, SC4, SC5, PC1 and PC2, respectively. Ordinary concrete was used to make cubic concrete test blocks of 180 mm×180 mm×180 mm, which were numbered NC.
[0048] The test conditions are described as follows: The test environment includes environment 1: outdoor temperature 20℃, humidity 70%; environment 2: outdoor temperature -10℃, humidity 30%.
[0049] Test indicator 1, compressive strength, refers to the maximum pressure that concrete can withstand per unit area under standard conditions, which reflects the mechanical strength characteristics of concrete. The unit is megapascal (MPa). Test method: The compressive strength determination is based on the methods, equipment, specimen preparation and maintenance of concrete mechanical properties tests specified in the "Standard for Test Methods for Mechanical Properties of Ordinary Concrete" (GB / T 50081-2019), and provides a test method for concrete compressive strength.
[0050] Test index 2, impermeability, is indirectly reflected by the water seepage height. The lower the water seepage height, the stronger the concrete's ability to resist water penetration, that is, the better the impermeability. Test method: Use sealing materials to seal the specimen to prevent water from leaking from the side. The sealing method can be to roll on melted paraffin, cement and butter mixture or other reliable sealing methods.
[0051] Install the sealed specimen on the impermeability tester to ensure that the specimen and the impermeability tester are well sealed. Start the impermeability tester and apply a constant water pressure of 1.2MPa to the specimen. The pressurization process should be rapid and stable, and the time to reach the preset pressure is used as the starting time of the test record. During the test, observe the water seepage at the end face of the specimen regularly. When the end face of the specimen begins to seep water, record the time when the seepage occurs and the corresponding seepage height (the seepage height is the height of the specimen at this time). If water seeps out from the periphery of the specimen during the test, it means that the seal is poor, and the seal should be re-performed and the test should be restarted. Set the test time to 24 hours according to the test requirements. After the time is reached, terminate the test and remove the specimen. If there is no water seepage in the specimen within the set time, it is recorded as no water seepage. Measurement and calculation of water seepage height: Place the tested specimen on a press and split it in half along the longitudinal section to observe the water seepage profile. Use a waterproof pen or ink to draw the water seepage profile on the split surface. Note that the handwriting should not be too thick to avoid affecting the measurement accuracy. Place a trapezoidal plate (or transparent glass plate) on the split surface of the specimen, and use a steel ruler to measure the water seepage height of multiple measuring points at equal intervals along the water seepage profile (usually measure 10 points and be accurate to 0.1mm). The arithmetic mean of the water seepage height of all measuring points is taken as the average water seepage height of the specimen. If multiple groups of tests are conducted, the average water seepage height of multiple groups of specimens needs to be calculated to evaluate the overall anti-seepage performance of the concrete.
[0052] Test indicator 3, the frost resistance of concrete, refers to the ability of concrete to resist freeze-thaw cycles in low temperature environments. Under low temperature conditions, the water in concrete will freeze and expand in volume, which may cause stress inside the concrete, leading to cracking and damage. Therefore, frost resistance is an important indicator for evaluating the durability of concrete in cold areas. The mass loss rate is an important parameter for evaluating the frost resistance of concrete. It reflects the degree of surface erosion of concrete during the freeze-thaw cycle, thereby indirectly reflecting the frost resistance of concrete. The lower the mass loss rate, the less erosion of concrete during the freeze-thaw cycle, and the better the frost resistance. The detection process of mass loss rate is as follows: prepare concrete specimens in accordance with relevant standards and maintain them under standard conditions. Place the specimens in a freeze-thaw cycle tester and test them according to the predetermined number of freeze-thaw cycles. Each freeze-thaw cycle includes a certain period of freezing and thawing. Before and after the freeze-thaw cycle, use a precision balance to measure the mass of the specimens, and record the initial mass and the mass after the freeze-thaw cycle. The mass loss rate was calculated according to the formula “mass loss rate = (initial mass - mass after freeze-thaw) / initial mass × 100%”.
[0053] Test indicator 3, fluidity. Fluidity is an important indicator to measure the plasticity and fluidity of concrete mixtures during the construction process, and slump is an intuitive and commonly used quantitative indicator to reflect the fluidity of concrete. Slump refers to the degree to which the concrete mixture can collapse freely and fill the formwork under the action of its own weight or mechanical vibration. The larger the slump, the better the fluidity of the concrete, and the easier it is to pour and vibrate; conversely, the smaller the slump, the worse the fluidity of the concrete, and the difficulty of pouring and vibrating will also increase. Determination method: Prepare tools and materials: Slump cone: Use a trumpet-shaped metal cylinder with an upper diameter of 100mm, a lower diameter of 200mm, and a height of 300mm. Tamping rod: a round steel rod with a diameter of about 16mm and a length of 600mm. Other auxiliary tools: spatula, ruler, shovel, etc. Determination steps: Before the measurement, wet the inner wall and bottom of the slump cone with a wet cloth to prevent concrete from sticking. Use a small shovel to evenly load the concrete mixture into the cone in three layers. Use a tamping rod to tamp each layer from the outside to the center 25 times in the spiral direction. The tamping should be evenly distributed on the cross section. When tamping the bottom layer, the tamping rod should penetrate the entire depth; when tamping the second and top layers, the tamping rod should penetrate the current layer to the surface of the next layer; after tamping each layer, use a rubber hammer to gently tap the cylinder wall to remove the bubbles generated during tamping. After tamping, scrape off the excess concrete with a trowel, and smooth the surface with a trowel so that the concrete surface is flush with the plane of the cone mouth. Lift the slump cone vertically upward carefully and steadily without tilting. The lifting process should be completed within 5 to 10 seconds. The entire process from the beginning of loading to lifting the cylinder should be carried out uninterruptedly and should be completed within 150 seconds. Place the slump cone next to the concrete sample, place a ruler on the top of the cone facing the mixture, and use a steel ruler to measure the height difference between the highest point of the concrete specimen and the upper edge of the cone after collapse, which is the slump value of the concrete mixture. During the measurement process, maintain the uniformity of the concrete mixture to avoid segregation. The slump cone should be kept vertical when loading to avoid tilting that will cause inaccurate measurement results. The speed of lifting the slump cone should be uniform and stable to avoid too fast or too slow to affect the measurement results. After the measurement is completed, clean up the slump cone and tools in time to keep the equipment clean.
[0054] Table 1 Performance index test of each test block under environmental conditions (D / day) Sample Slump% / <1D 3D Strength 7D Strength 28D Strength 90D strength 180D strength Water seepage height / mm Mass loss rate% 3D-7D intensity change rate NC 7.11 12.3 20.1 26.2 34.2 45.4 126 2.35 1.95 SC1 8.36 15.6 27.9 35.9 40.6 57.8 88 1.12 3.075 SC2 8.27 14.2 25.7 37.1 41.1 58.1 86 0.92 2.875 SC3 8.29 14.2 25.2 30.5 48.1 52.9 89 0.91 2.75 SC4 8.31 15.2 25.4 32.1 48.4 52.4 91 1.05 2.55 SC5 8.32 14.4 23.1 34.1 48.6 51.6 87 0.99 2.175 PC1 7.64 13.3 22.6 28.2 37.8 47.2 115 1.53 2.325 PC2 7.52 13.8 23.1 28.8 38.4 47.8 112 1.48 2.325 As can be seen from Table 1, compared with ordinary concrete (NC): the compressive strength of all concrete specimens (SC1-SC5) with active lime additives at various ages (3 days, 7 days, 28 days, etc.) is significantly higher than that of ordinary concrete (NC). At the age of 3 days, the compressive strength of SC1 is 15.6MPa, while that of NC is only 12.3MPa; at the age of 28 days, the strength of the SC series is generally above 30MPa, while that of NC is only 26.2MPa. This shows that the active lime additive significantly improves the early strength of concrete and improves the later strength to a large extent.
[0055] As can be seen from the table, the strength growth rate of concrete with active lime additives between 3 days and 7 days is generally higher, such as the strength change rate of SC1 is 3.075%, which is much higher than 1.95% of NC. This shows that the additive promotes the rapid development of early strength of concrete and helps to speed up the construction progress.
[0056] All concrete blocks with active lime additives showed significantly lower water penetration heights than those of NC. Lower water penetration heights mean that these concretes have better anti-seepage properties and can more effectively prevent water penetration, thereby improving the durability and service life of concrete.
[0057] The mass loss rate is an important indicator for evaluating the frost resistance of concrete. As can be seen from the table, the mass loss rate of concrete with active lime additives after freeze-thaw cycles is generally lower, indicating that these concretes have better resistance to freeze-thaw cycles and can maintain structural integrity under harsh climatic conditions.
[0058] In addition, the slump of concrete with active lime additives is generally slightly higher than that of normal concrete (NC), indicating that these concretes have better fluidity and plasticity, which is beneficial to the pouring and vibration operations during construction.
[0059] Table 2 Performance index test of each test block under environmental conditions (D / day) Sample Slump% / <1D 3D Strength 7D Strength 28D Strength 90D strength 180D strength Water seepage height / mm Mass loss rate% 3D-7D intensity change rate NC 6.77 10.3 15.8 18.4 23.2 28.6 129 3.11 1.38 SC1 7.98 13.1 22.1 25.2 27.6 36.4 90 2.00 2.24 SC2 7.90 11.9 20.3 26.0 27.9 36.6 88 1.82 2.09 SC3 7.92 11.9 19.9 21.4 32.7 33.3 91 1.81 1.99 SC4 7.94 12.8 20.1 22.5 32.9 33.0 93 1.94 1.825 SC5 7.95 12.1 19.2 23.9 33.0 32.5 89 1.89 1.785 PC1 7.29 11.2 17.8 19.8 25.7 29.7 118 2.37 1.66 PC2 7.17 11.6 18.2 20.2 26.1 30.1 115 2.33 1.66 As can be seen from Table 2, under low temperature conditions (outdoor temperature -10°C, humidity 30%), the compressive strength of all concrete specimens (SC1-SC5) with active lime additives at various ages (3 days, 7 days, 28 days, etc.) remained at a certain level, although it was lower than that in normal temperature environments (Table 1), but it was still significantly higher than that of ordinary concrete (NC) without additives. This shows that active lime additives can still effectively improve the strength of concrete under low temperature conditions.
[0060] In low temperature environment, the strength growth rate of concrete is generally lower than that in normal temperature environment. However, the strength growth rate of concrete specimens with active lime additives between 3 days and 7 days is still higher than that of ordinary concrete (NC), such as the strength change rate of SC1 is 2.24%, while that of NC is only 1.38125%. This shows that additives can still promote the growth of concrete strength in low temperature environment, but the effect is limited by temperature.
[0061] Under low temperature conditions, the water seepage height of concrete specimens with active lime additives was still significantly lower than that of normal concrete (NC), indicating that these concretes also have good anti-seepage properties at low temperatures. This helps prevent water penetration and reduce the damage to concrete caused by freeze-thaw cycles.
[0062] The mass loss rate can be used to indirectly evaluate the frost resistance of concrete. Although the mass loss rate of all concrete specimens increased under low temperature conditions, the mass loss rate of concrete specimens with active lime additives was still low, indicating that these concretes have better frost resistance at low temperatures than ordinary concrete.
[0063] In low temperature environment, the slump of concrete generally decreases, but the slump of concrete specimens with active lime additives still remains at a certain level, higher than that of ordinary concrete (NC). This shows that additives help improve the workability of concrete in low temperature environment, making it easier to construct.
[0064] The data in Table 2 reflect the positive effect of active lime additives on concrete performance in low temperature environments. Although low temperature environments have a significant impact on concrete performance, additives can still improve the strength, durability and workability of concrete to a certain extent.
[0065] In addition, it can be seen from Tables 1 and 2 that the compressive strength of concrete samples with mixed component C (such as SC1-SC5) at all ages is significantly higher than that of the control samples without mixed component C (such as comparative examples PC1 and PC2). This shows that mixed component C plays an important role in improving the strength of concrete.
[0066] Especially for the early strength (such as 3-day and 7-day strength), the contribution of mixed component C is particularly obvious. This is because the chemical components in mixed component C can accelerate the hydration reaction of cement and promote the formation of early strength.
[0067] Water seepage height and mass loss rate are important indicators for evaluating the durability of concrete. As can be seen from Tables 1 and 2, the water seepage height and mass loss rate of concrete samples with mixed component C added are generally lower, indicating that their durability is better than that of samples without mixed component C. The ingredients of mixed component C include trimethylolpropane, whose chemical formula is C6H 14 O3, alkyl alcohol polyoxyethylene ether: The structure can be expressed as RO-(CH2CH2O)nH, where R represents the alkyl chain, n>15, represents the degree of polymerization of ethylene oxide. Benzoyl peroxide. Sodium anthraquinone-1-sulfonate is the sodium salt form of anthraquinone-1-sulfonic acid. The above ingredients in mixed component C form a more compact structure inside the concrete, reducing water penetration and concrete erosion. Among them, the effects of sodium anthraquinone-1-sulfonate on the performance of concrete samples are as follows: By comparing the data of the examples and comparative examples (such as Example 1 and Comparative Example 1, Example 1 and Comparative Example 2), it can be clearly seen that the compressive strength of the concrete samples added with sodium anthraquinone-1-sulfonate is higher than that of the samples without or only partially added with sodium anthraquinone-1-sulfonate at all ages. This shows that sodium anthraquinone-1-sulfonate has a significant contribution to improving the strength of concrete.
[0068] Sodium anthraquinone-1-sulfonate enhances the strength of concrete by promoting cement hydration reaction and filling concrete pores. In terms of water seepage height and mass loss rate, concrete samples with the addition of sodium anthraquinone-1-sulfonate show better durability. Sodium anthraquinone-1-sulfonate improves the impermeability and frost resistance of concrete by forming a protective layer and reducing the internal stress concentration of concrete, and reduces the evaporation of water on the concrete surface, reducing the occurrence of cracking.
[0069] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An active lime additive, characterized in that: It is made of the following components: by weight, 20-40 parts of mixed component A, 20-40 parts of mixed component B, 20-40 parts of mixed component C and 20-40 parts of mixed component D, wherein: The mixed component A comprises the following components: by weight, 15-30 parts of artificial stone, 15-30 parts of ceramic and 25-40 parts of natural stone; The mixed component B comprises the following components: 20-35 parts of active lime, 10-20 parts of mineral powder and 10-20 parts of sodium aluminum silicate, by weight; The mixed component C comprises the following components: by weight, 20-30 parts of anthraquinone-1-sodium sulfonate, 15-40 parts of trimethylolpropane, 15-40 parts of alkyl alcohol polyoxyethylene ether and 20-30 parts of benzoyl peroxide; The mixed component D comprises the following components: 10-20 parts of zeolite powder and 10-20 parts of silica fume, by weight.
2. An active lime additive according to claim 1, characterized in that: The mixed component A comprises the following components: 25 parts of artificial stone, 25 parts of ceramic and 25 parts of natural stone, by weight; the mixed component B comprises the following components: 35 parts of active lime, 10 parts of mineral powder and 20 parts of sodium aluminum silicate, by weight; the mixed component C comprises the following components: 30 parts of trimethylolpropane, 30 parts of alkyl alcohol polyoxyethylene ether, 20 parts of benzoyl peroxide and 20 parts of sodium anthraquinone-1-sulfonate, by weight; and the mixed component D comprises the following components: 10 parts of zeolite powder and 10 parts of silica fume, by weight.
3. An active lime additive according to claim 1, characterized in that: The mixed component A comprises the following components: 15 parts of artificial stone, 15 parts of ceramic and 30 parts of natural stone, by weight; the mixed component B comprises the following components: 35 parts of active lime, 20 parts of mineral powder and 10 parts of sodium aluminum silicate, by weight; the mixed component C comprises the following components: 25 parts of trimethylolpropane, 35 parts of alkyl alcohol polyoxyethylene ether, 20 parts of benzoyl peroxide and 20 parts of sodium anthraquinone-1-sulfonate, by weight; and the mixed component D comprises the following components: 20 parts of zeolite powder and 10 parts of silica fume, by weight.
4. An active lime additive according to claim 1, characterized in that: The mixed component A comprises the following components: 20 parts of artificial stone, 20 parts of ceramics and 30 parts of natural stone, by weight; the mixed component B comprises the following components: 35 parts of active lime, 15 parts of mineral powder and 15 parts of sodium aluminum silicate, by weight; the mixed component C comprises the following components: 25 parts of trimethylolpropane, 15 parts of alkyl alcohol polyoxyethylene ether, 30 parts of benzoyl peroxide and 30 parts of sodium anthraquinone-1-sulfonate, by weight; and the mixed component D comprises the following components: 10 parts of zeolite powder and 20 parts of silica fume, by weight.
5. An active lime additive according to claim 1, characterized in that: The mixed component A comprises the following components: 30 parts of artificial stone, 20 parts of ceramics and 25 parts of natural stone, by weight; the mixed component B comprises the following components: 35 parts of active lime, 20 parts of mineral powder and 20 parts of sodium aluminum silicate, by weight; the mixed component C comprises the following components: 20 parts of trimethylolpropane, 30 parts of alkyl alcohol polyoxyethylene ether, 30 parts of benzoyl peroxide and 20 parts of sodium anthraquinone-1-sulfonate, by weight; and the mixed component D comprises the following components: 10 parts of zeolite powder and 20 parts of silica fume, by weight.
6. A method for preparing an active lime additive according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1, preparing raw materials: preparing mixed component A, mixed component B, mixed component C and mixed component D respectively and feeding them into the feeding system; Step 2, decomposition and calcination: the material in the feeding system is preheated by the multi-stage cyclone preheating system and then sent to the decomposition furnace to be calcined into active lime. The main control temperature of the decomposition furnace is 850-950℃; the calcination time is 3-5 seconds; Step 3: Product cooling: After cooling in a multi-stage cyclone cooler, the active lime additive is obtained.
7. The method for preparing an active lime additive according to claim 6, characterized in that: The specific process for preparing the mixed component B in the step 1 is to weigh 20-35 parts of active lime, 10-20 parts of mineral powder and 10-20 parts of sodium aluminum silicate by weight, add a certain amount of deionized water into a stirred reactor and stir thoroughly, let it stand for 48-72 hours at 70°C±5°C and 85%-95% humidity, and grind it after drying at 85-98°C.
8. The method for preparing an active lime additive according to claim 6, characterized in that: The specific process for preparing the mixed component C in the step 1 is to weigh 15-40 parts of trimethylolpropane, 15-40 parts of alkyl alcohol polyoxyethylene ether, 20-30 parts of benzoyl peroxide and 20-30 parts of anthraquinone-1-sodium sulfonate by weight, add a certain amount of deionized water, and mix them evenly to obtain a mixed solution.
9. The method for preparing an active lime additive according to claim 6, characterized in that: The specific process for preparing the mixed component D in step 1 is to pour deionized water into 10-20 parts of zeolite powder, stir evenly to obtain zeolite powder slurry, ball-mill the zeolite powder slurry and 10-20 parts of silica fume, and then disperse and sieve at a temperature of 85-98°C.
Citation Information
Patent Citations
High-dosage fly ash concrete and preparation method thereof
CN113636794A