Preparation method of wear-resistant billiard cloth fabric
By using special fibers and interwoven processes in billiards fabrics, the problem of rapid wear of billiards cloth is solved, significantly improving wear resistance and service life, and reducing exercise costs.
Patent Information
- Application Number
- CN202411229210.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-06
AI Technical Summary
The existing billiards fabric wears fast during use, resulting in a short life and increases exercise costs.
Using 66S and 50% special raw materials such as silk, KEVLAR fiber or fluorinated wool staple fiber, the warp and weft yarn are interwoven into twill tissue, and wool burning, washing and shrinking, steel needle wool wool, trimming and steaming To improve wear resistance.
It significantly improves the wear resistance of billiard cloth, extends service life, reduces operating costs, and ensures that the fabric is smooth and smooth, meeting sports needs.
Smart Images

Figure SMS_4 
Figure SMS_5
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of billiard cloth fabrics, and in particular to a method for preparing a wear-resistant billiard cloth fabric. Background Art
[0002] Billiards is a sport that has a good effect on the body and mind. Billiards is a sport that is both healthy and brain-boosting, and is a combination of physical strength and wisdom. Billiards does not involve strenuous physical exercise, so it can be played by men, women, young and old. Participating in billiards can also increase social interaction. Billiards can also encourage people to develop good behavioral habits and become a popular and civilized person. Therefore, billiards is very common throughout the world.
[0003] Billiards requires a variety of equipment and instruments, and the most important of these is the billiard table. In addition to the table itself, the billiard table also has the billiard cloth covering it. The billiard ball rolls back and forth on the billiard cloth, which causes a certain amount of wear and tear on the cloth. When the wear and tear accumulates to a certain extent, the cloth will be damaged. Once damaged, it needs to be replaced, and replacing the cloth also increases the cost of playing billiards.
[0004] Therefore, the billiard cloth fabric must have a certain thickness, and the surface must be flat and smooth, and at the same time it must have a certain wear resistance. However, conventional billiard cloth fabrics are very likely to be worn out and damaged due to problems with the use of raw materials. Summary of the invention
[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a method for preparing a wear-resistant fabric of billiard cloth.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing a wear-resistant billiard cloth fabric comprises the following steps:
[0008] S1. Grey cloth manufacturing:
[0009] 1) Spinning warp yarn with 80% (weight percentage) of 66S and other materials and 20% of special raw materials, first spinning single yarn with twist of 570 and twist direction S, and then plying with ply count of 38 / 2, ply twist of 610 and twist direction Z;
[0010] 2) 50% (weight percentage) of 66, 30% of 3D nylon, 20% of special raw materials, spun weft yarn 25 / 1, single yarn twist 520, twist direction S;
[0011] 3) interweaving the above warp yarns and weft yarns into a twill weave to obtain a grey cloth;
[0012] S2. Finishing of grey fabric:
[0013] The above grey cloth is post-finished to obtain the finished billiard cloth wear-resistant fabric. The post-finishing process is: singeing → washing and shrinking → opening width → drying → steel needle raising → cloth repairing → feeding and drying → steaming → finished product.
[0014] Preferably, the parameters of the grey cloth are: grey cloth warp density 425 / 10cm, grey cloth weft density 294 / 10cm, grey cloth width 175cm, grey cloth weight 645g / m, and the cloth edge is woven by square flat edge weaving method.
[0015] Preferably, the special raw material is Silk, KEVLAR fiber or fluorinated wool staple fiber.
[0016] CORDURA fabric: INVT CORDURA fabric is a functional fabric that is light, quick-drying, soft, and durable. It is not easy to change color after long-term use. Under the same weight, the durability of CORDURA fabric is 2 times that of standard nylon fabric, 3 times that of polyester fabric, and 10 times that of cotton canvas. The fiber fineness of silk ranges from 30 denier to 2000 denier and is widely used in a variety of products such as bags, footwear and functional clothing such as motorcycle jackets.
[0017] KEVLAR FIBER:
[0018] It is the brand name of an aramid fiber material product developed by Dupont in the United States. The original name of the material is "poly(p-phenylene terephthalamide)". Kevlar brand product materials are tough, wear-resistant, and both hard and soft.
[0019] KEVLAR has permanent heat resistance and flame retardancy, permanent antistatic property, permanent resistance to acid, alkali and organic solvent erosion, high strength, high wear resistance and high tear resistance. It will not produce any droplets or toxic gases when exposed to fire. When the fabric is burned by fire, the fabric surface will become thicker, the sealing will be enhanced and it will not crack.
[0020] KEVLAR is widely used in protective clothing and industrial textiles, such as bulletproof vests, bulletproof helmets, cut protection, sportswear, work protective clothing, elevator slings, tarpaulins, heat-resistant canvas, parachute fabrics, etc.
[0021] The preparation process of the fluorinated wool staple fiber is as follows:
[0022] Put the wool staple fibers into a reaction chamber, and introduce nitrogen containing 8% (volume percentage) fluorine into the bottom of the reaction chamber. After reacting for 60 seconds, pour in pure water and soak for 3-5 minutes, drain and dehydrate, and dry with hot air at 60-70°C to obtain fluorinated wool staple fibers.
[0023] Preferably, the parameters of the finished wear-resistant billiard cloth are: finished width ≥ 168 cm, finished weight ≥ 660 g / m, color: blue, and the finished product requires antistatic properties.
[0024] Preferably, the specific process and parameters of the S2 grey cloth finishing are as follows:
[0025] 1) Singeing: speed 100m / min, one pass on the front side, no burning on the back side;
[0026] 2) Washing and shrinkage: add 2% auxiliary agent, speed 80m / min, 40℃×120min;
[0027] 3) Steel needle raising: speed 12m / min, needle roller speed: 90 rpm, clockwise roller: 40r / min, counterclockwise roller: 45r / min, raising the reverse side 3 times;
[0028] 4) Loading: Add antistatic additives as required, the amount added is 30g / L;
[0029] 5) Steaming: Steam for 12 minutes, keep warm for 4 minutes, and cool for 10 minutes.
[0030] Furthermore, the antistatic auxiliary agent is ASA-302 antistatic finishing agent (Rizhao Nisi Environmental Protection Materials Co., Ltd.) or wool antistatic agent FK-312 (Jiangsu Jurong Chemical Co., Ltd.).
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] 1. The present invention makes a major adjustment to the raw materials for producing billiard cloth, uses some wear-resistant materials in the raw materials, greatly improves the wear resistance of the billiard cloth, prolongs the service life of the billiard cloth, reduces the operating cost of billiard sports, is conducive to the development and popularization of billiard sports, and at the same time, the product has also won many market orders for the enterprise, bringing better economic benefits to the enterprise.
[0033] 2. The present invention tests a variety of special materials with wear resistance and tension resistance (KEVLAR) or shrinkage-resistant fluorinated wool staple fibers at the same time, ensuring sufficient strength while ensuring wear resistance, ensuring that the prepared billiard cloth has extremely high wear resistance, greatly extending the service life of the billiard cloth, and reducing the operating cost of billiard sports. At the same time, it ensures that the prepared billiard cloth has moderate thickness, flat and smooth surface, and no obvious defects, which meets the requirements of billiard sports for billiard cloth. DETAILED DESCRIPTION
[0034] The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.
[0035] Embodiment 1:
[0036] This embodiment provides a method for preparing a billiard cloth material with extremely high wear resistance, and the specific steps are as follows:
[0037] Blended billiard fabric: finished product width ≥168cm, finished product weight ≥660g / m, color: blue, finished product requires antistatic properties.
[0038] 1. Use 80% of 66S and 20% of special raw materials to spin warp yarn. First spin single yarn with twist 570 and twist direction S, then plied, with ply count 38 / 2, ply twist 610 and twist direction Z.
[0039] 2. 50% 66, 30% 3D nylon, 20% special raw materials, spinning weft yarn 25 / 1, single yarn twist 520, twist direction S.
[0040] 3. The above warp yarns and weft yarns are interwoven into a twill structure. The warp density of the grey cloth is 425 / 10cm, the weft density of the grey cloth is 294 / 10cm, the width of the grey cloth is 175cm, the weight of the grey cloth is 645g / m, and the selvedge is woven using the square flat edge weaving method.
[0041] 4. The above grey cloth is post-finished, and the post-finishing process is as follows:
[0042] Singeing - washing and shrinking - opening - drying - steel needle raising - cloth repairing - feeding and drying - steaming - finished product.
[0043] 1) Singeing: Machine speed 100m / min, one pass on the front side, no burning on the back side.
[0044] 2) Washing and shrinkage: add 2% auxiliary agent, speed 80m / min, 40℃×120min.
[0045] 3) Steel needle raising: speed 12m / min, needle roller speed: 90 rpm, clockwise roller: 40r / min, counterclockwise roller: 45r / min, reverse side raising 3 times
[0046] 4) Loading: Add antistatic agent as required: 30g / l.
[0047] 5) Steaming: Steam for 12 minutes, keep warm for 4 minutes, and cool for 10 minutes.
[0048] The special raw materials used in this embodiment are Silk.
[0049] Embodiment 2:
[0050] The remaining steps are the same as those in Example 1, except that the special raw material used in this example is KEVLAR fiber.
[0051] Embodiment 3:
[0052] The remaining steps are the same as those in Example 1, except that the special raw material used in this example is fluorinated wool staple fiber.
[0053] The preparation process of the fluorinated wool staple fiber is as follows:
[0054] Put the wool staple fibers into a reaction chamber, and introduce nitrogen containing 8% (volume percentage) fluorine into the bottom of the reaction chamber. After reacting for 60 seconds, pour in pure water and soak for 3-5 minutes, drain and dehydrate, and dry with hot air at 60-70°C to obtain fluorinated wool staple fibers.
[0055] The technical indicators of the final product prepared in the above examples are as follows:
[0056] Ingredients: 66% wool, 14% nylon, 20% special raw materials;
[0057] Width: 170cm;
[0058] Weight per meter: 651g / m;
[0059] Pilling: Level 4-5;
[0060] Wear resistance times: >100,000 times, much higher than the standard requirement of ≥14,000 times.
[0061] Color fastness to light: Grade 3-4;
[0062] Water fastness: color change level 4-5, staining level 4;
[0063] Color fastness to perspiration: color change level 4, staining level 4;
[0064] Color fastness to ironing: color change level 4, cotton staining level 4;
[0065] Color fastness to dry rubbing: Grade 4;
[0066] Color fastness to wet rubbing: Grade 3-4;
[0067] Color fastness to dry cleaning: color change level 4, solvent change level 3-4;
[0068] The products of each embodiment differ slightly only in breaking strength, as shown in Table 1 below:
[0069] Table 1. Mechanical strength of billiard cloth wear-resistant fabric
[0070]
[0071]
[0072] In summary, the present invention provides a method for preparing a billiard cloth fabric with extremely high wear resistance. The prepared billiard cloth fabric has extremely high wear resistance, and the actual wear resistance times are greater than 100,000 times, which is much higher than the standard of ≥14,000 times, which greatly extends the service life of the billiard cloth and reduces the operating cost of billiard sports. At the same time, it is ensured that the prepared billiard cloth fabric meets the requirements of billiard sports for billiard cloth fabrics. Various physical and chemical indicators meet the "Combed Billiard Wool Tablecloth" standard, standard number: Q / 320582OQT1-2023-2023. The first-class product rate is 99.5%.
[0073] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a wear-resistant surface of billiard cloth, characterized in that: The following steps are involved: S1. Grey cloth manufacturing: 1) 80% of 66S and 20% of special raw materials are used to spin warp yarn. First, single yarn is spun with a twist of 570 and a twist direction of S, and then plying is performed with a ply count of 38 / 2, a ply twist of 610 and a twist direction of Z; 2) 50% 66, 30% 3D nylon, 20% special raw materials, spun weft yarn 25 / 1, single yarn twist 520, twist direction S; 3) interweaving the above warp yarns and weft yarns into a twill weave to obtain a grey cloth; S2. Finishing of grey fabric: The above grey cloth is post-finished to obtain the finished billiard cloth wear-resistant fabric. The post-finishing process is: singeing → washing and shrinking → opening width → drying → steel needle raising → cloth repairing → feeding and drying → steaming → finished product.
2. The method for preparing a wear-resistant surface material of billiard cloth according to claim 1, characterized in that: The parameters of the grey cloth are as follows: the grey cloth warp density is 425 / 10cm, the grey cloth weft density is 294 / 10cm, the grey cloth width is 175cm, the grey cloth weight is 645g / m, and the cloth edge is woven by a square flat edge weaving method.
3. The method for preparing a wear-resistant surface material of billiard cloth according to claim 1, characterized in that: The special raw materials in S1 are Silk or KEVLAR fiber.
4. The method for preparing a wear-resistant billiard cloth fabric according to claim 1, characterized in that: The special raw material in S1 is fluorinated wool staple fiber.
5. The method for preparing a wear-resistant surface material of billiard cloth according to claim 4, characterized in that: The preparation process of the fluorinated wool staple fiber is as follows: Put the wool staple fibers into a reaction chamber, and introduce nitrogen containing 8% (volume percentage) fluorine into the bottom of the reaction chamber. After reacting for 60 seconds, pour in pure water and soak for 3-5 minutes, drain and dehydrate, and dry with hot air at 60-70°C to obtain fluorinated wool staple fibers.
6. The method for preparing a wear-resistant surface material of billiard cloth according to claim 1, characterized in that: The parameters of the finished wear-resistant billiard cloth are: finished width ≥168cm, finished weight ≥660g / m, color: blue, and the finished product requires antistatic performance.
7. The method for preparing a wear-resistant billiard cloth fabric according to claim 1, characterized in that: The specific process and parameters of the S2 grey cloth finishing are as follows: 1) Singeing: speed 100m / min, one pass on the front side, no burning on the back side; 2) Washing and shrinkage: add 2% auxiliary agent, speed 80m / min, 40℃×120min; 3) Steel needle raising: speed 12m / min, needle roller speed: 90 rpm, clockwise roller: 40r / min, counterclockwise roller: 45r / min, raising the reverse side 3 times; 4) Loading: Add antistatic additives as required, the amount added is 30g / L; 5) Steaming: Steam for 12 minutes, keep warm for 4 minutes, and cool for 10 minutes.
8. The method for preparing a wear-resistant surface material of billiard cloth according to claim 7, characterized in that: The antistatic auxiliary agent is ASA-302 antistatic finishing agent or wool antistatic agent FK-312.
Citation Information
Patent Citations
Strong-strength wear-resistant machine-washable woolen business suit fabric and production method thereof
CN106884252A
Super wear-resistant worsted fancy suiting production process
CN106987971A
Preparation method of elastic woven fabric
CN108708014A
Wear-resistant breathable textile fabric
CN212289007U
Reducing shrinkage of wool and wool blend fabrics due to felting
US20130117978A1