Continuous macro preparation device and method for flexible and elastic ceramic superfine fiber material

Through the combination of feeding and liquid dispensing system, multi-jet uniform electrospinning system and low-temperature calcining system, the problems of continuity and structural regulation in the production of ceramic microfiber materials are solved, and efficient preparation of ceramic fiber materials is achieved, which improves mechanical properties and Flexible and elastic.

CN119083040AActive Publication Date: 2024-12-06DONGHUA UNIV

Patent Information

Application Number
CN202411182140.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The prior art is difficult to realize the continuous macro production of flexible elastic ceramic microfiber materials, and there is a lack of continuous production of preparation methods, low conversion of hybrid fibers in spinning liquid, difficult to regulate the structural form, and slow removal of polymer components in the calcining device. Problem, cannot meet the actual application requirements.

Method used

Provide a continuous macro preparation device including a feeding and liquid dispensing system, a multi-jet uniform electrospinning system and a low-temperature calcination system. Through online monitoring and vacuum concentration configuration of the spinning liquid, using multi-jet electrospinning and low-temperature calcination technology, Achieve precise regulation of fibers and rapid removal of polymer templates.

Benefits of technology

It realizes efficient and stable molding of ceramic fiber materials, improves mechanical properties, and obtains ceramic microfiber materials with flexible elastic properties, solving the problems of low production efficiency of fiber materials and difficult structural form regulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119083040A_ABST
    Figure CN119083040A_ABST
Patent Text Reader

Abstract

The invention relates to a continuous macro preparation device and method for a flexible and elastic ceramic superfine fiber material. The continuous macro preparation device sequentially comprises a feeding and liquid preparation system, a multi-jet uniform electrostatic spinning system, a low-temperature calcination system and a winding system. Mixing the raw materials, dispersing at low temperature, and concentrating in vacuum to obtain sol; enabling the sol and the polymer to flow into a polymer mixing device, mixing, and removing bubbles; enabling the mixed sol to flow into an inorganic component content control device, and performing negative pressure suction to obtain a spinning solution; the spinning solution flows into a multi-jet-flow electrostatic spinning module, the temperature, humidity and multidirectional differential speed during spinning are regulated and controlled, and a fiber membrane material or a fiber flocculus material is obtained; the fiber material is sequentially conveyed to a drying area, a microwave pretreatment area, a polymer removal area, an oxygen-deficient atmosphere heat treatment area and a cooling area to be subjected to multi-temperature-area calcination, and the soft and elastic ceramic superfine fiber material is obtained; and rolling and packaging are conducted, and continuous macro-quantity manufacturing of the flexible and elastic ceramic superfine fiber material is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ceramic fiber material preparation, and in particular to a device and method for continuous large-scale preparation of flexible and elastic ceramic ultrafine fiber materials. Background Art

[0002] Ceramic fiber has the advantages of high temperature resistance, fire retardancy, and good chemical stability. It is an important material in the fields of aerospace, energy and environment. The main methods for preparing ceramic fibers include centrifugal spinning, melt blowing and dry spinning. The fibers prepared by these methods are usually thicker in diameter and not flexible. At present, electrospinning is the main way to prepare ceramic ultrafine fibers. However, this method has the following problems:

[0003] (1) The preparation method of pre-flexible elastic ceramic fiber materials is usually not continuous, and it is impossible to achieve liquid preparation, spinning and calcination at the same time. The required production cycle is long and the production efficiency is low.

[0004] (2) In order to ensure the spinnability of the solution, high molecular weight polymers are often selected as spinning aids and added to the inorganic sol, resulting in a low hybrid fiber conversion rate of the spinning solution and a low content of inorganic components in the hybrid fibers.

[0005] (3) A single electrospinning nozzle can only form a single jet, and the electric field interference between multiple nozzles is large, making it impossible to spin stably.

[0006] (4) Existing electrospinning equipment is difficult to precisely control the structural morphology of the fibers and can only prepare fiber membrane materials, but cannot obtain bulk materials in one step.

[0007] (5) The existing calcination equipment has the problem of slow removal of polymer components and easy residue, and the grain size cannot be controlled, resulting in the fiber material having no flexibility.

[0008] (6) The mechanical properties of ceramic ultrafine fiber materials prepared by existing technologies still cannot meet the needs of practical applications, and fiber flake materials cannot be obtained in one step, making continuous production difficult.

[0009] Therefore, how to achieve continuous mass production of various types of flexible and elastic ceramic ultrafine fiber materials has become a difficult problem that needs to be solved urgently.

[0010] In response to the above problems, researchers have conducted relevant research in this field. Patent 202111376349.1 discloses a large-scale continuous manufacturing device for flexible ceramic nanofibers, including configuring a linear inorganic polymer sol spinning solution through a batch preparation device, using an electrospinning nozzle to quickly electrospin the spinning solution into fibers, and low-temperature calcining the gel nanofibers to obtain flexible ceramic nanofibers. However, the electrospinning mechanism of the device is only a single nozzle, which limits the increase in the production rate of fiber materials. Patent 201810442177.5 discloses an electrospinning device and method for batch preparation of uniform nanofibers. The spinning solution forms multiple Taylor cones on the auxiliary Taylor cone assembly. The generated Taylor cones are stretched into filaments under the action of the electrostatic field of the high-voltage electrostatic generator and are received on the negative electrode receiving mechanism to form nanofibers. However, this method does not accurately control the morphological structure of the fiber, and can only prepare fiber membrane materials formed by stacking straight fibers, and cannot achieve one-step molding of fiber body materials. Patent CN202210756271.4 discloses a device and method for continuously producing flexible oxide nanofiber membranes. The spinning module electrospins the precursor liquid, continuously collects the spun fibers on a high-temperature ceramic fiber cloth, and then directly transports them to a heating device through a conveyor belt for rapid sintering, thereby continuously preparing flexible oxide nanofiber materials. However, the sintering device in the device does not pretreat the polymer template in the oxide fiber, resulting in a slow decomposition rate of the polymer template and a long time consumption.

[0011] Therefore, the development of a continuous large-scale preparation device and method for flexible and elastic ceramic ultrafine fiber materials is expected to solve the above-mentioned bottleneck problem and is of great significance. Summary of the invention

[0012] The purpose of the present invention is to overcome the above-mentioned problems existing in the prior art and to provide a continuous large-scale preparation device and method for flexible and elastic ceramic ultrafine fiber materials.

[0013] The purpose of the present invention can be achieved by the following technical solutions:

[0014] One of the technical solutions of the present invention is to provide a continuous large-scale preparation device for flexible and elastic ceramic ultrafine fiber materials, which comprises a feeding and liquid preparation system, a multi-jet uniform electrospinning system, a low-temperature calcination system, and a winding system in sequence;

[0015] The feeding and liquid preparation system comprises a mixing device, a polymer mixing device, and an inorganic component content control device which are connected in series via a liquid delivery pipeline in sequence;

[0016] The multi-jet uniform electrospinning system comprises a temperature and humidity control device, a multi-jet electrospinning module and a solvent vapor removal device electrically connected to the temperature and humidity control device and connected to the inorganic component content control device, and a static elimination and insulation device connected to the multi-jet electrospinning module;

[0017] The low-temperature calcination system includes a multi-zone temperature control device, a drying zone, a microwave pretreatment zone, a polymer removal zone, an oxygen-deficient atmosphere heat treatment zone, and a cooling zone which are sequentially connected to the multi-zone temperature control device and are independently separated.

[0018] In some specific embodiments, the mixing device includes a primary tank body, an in-situ infrared analyzer, a viscosity detector, a primary feeding port, and a vacuum concentration component arranged on the primary tank body, a gelation inhibition component wrapped around the body and bottom of the primary tank body, a primary stratification stirring component arranged in the primary tank body, and a primary flow control valve arranged on the liquid delivery pipe at the outlet of the mixing device.

[0019] As a more preferred embodiment, the first-level layered stirring assembly includes a stirring blade and a motor, the structure of the stirring blade is selected from any one of paddle type, turbine type, propeller type, anchor type, frame type, ribbon type, and screw type, the material of the stirring blade includes stainless steel, carbon steel, carbon steel lined with rubber, carbon steel lined with fiberglass, the rotation speed of the stirring roller is 50 to 5000 rpm, the number of stirring layers is 1 to 5 layers, the number of stirring rollers is 1 to 5, the material of the stirring roller includes stainless steel, carbon steel, rubber, cast iron, polyurethane, the spacing between the stirring rollers is 5 to 20 cm, and the equivalent diameter is 3 to 10 cm.

[0020] In some specific embodiments, the vacuum concentration mechanism includes a vacuum concentrator, a heat exchanger, a condensed water tank, and a vacuum pump.

[0021] As a more preferred embodiment, the outer diameter of the primary can is 30 to 100 cm, the thickness is 2 to 35 cm, the height is 60 to 160 cm, and the material includes stainless steel, titanium alloy, glass, quartz glass, polytetrafluoroethylene, and nickel-chromium-molybdenum alloy.

[0022] In some specific embodiments, the gelation inhibition component includes a cold air component, a low-temperature pipe connected to the cold air component and surrounding the body and bottom of the first-level tank body, and an insulation layer arranged on the outside of the low-temperature pipe, and the low-temperature pipe is provided with a plurality of jet ports that penetrate the bottom of the first-level tank body.

[0023] As a more preferred embodiment, the number of the air jets is 5-20, the diameter of the air jets is 1-5 cm, and the materials include stainless steel, galvanized steel, aluminum alloy, polyethylene, and polytetrafluoroethylene.

[0024] As a more preferred embodiment, the low-temperature pipe has a thickness of 0.2 to 2 cm and an outer diameter of 2 to 10 cm, and the low-temperature material includes stainless steel, low-temperature carbon steel, and alloy steel.

[0025] More preferably, the thickness of the thermal insulation layer is 2 to 5 cm, and the material of the thermal insulation layer 1053 includes glass fiber, polyurethane foam, rock wool, and aluminum silicate fiber.

[0026] In some specific embodiments, the polymer mixing device includes a secondary tank body connected to the primary tank body, a secondary feeding port, an ultrasonic component, and a bubble removal component arranged on the secondary tank body, a secondary stratification stirring component arranged in the secondary tank body, and a secondary flow control valve arranged on the liquid delivery pipe at the outlet of the secondary tank body.

[0027] As a more preferred embodiment, the secondary layered stirring assembly includes a stirring blade and a motor, the structure of the stirring blade is selected from any one of paddle type, turbine type, propeller type, anchor type, frame type, ribbon type, and screw type, the material of the stirring blade includes stainless steel, carbon steel, carbon steel lined with rubber, carbon steel lined with fiberglass, the rotation speed of the stirring roller is 50 to 5000 rpm, the stirring layer is 1 to 3 layers, the number of stirring rollers is 1 to 3, the material of the stirring roller includes stainless steel, carbon steel, rubber, cast iron, polyurethane, the spacing between the stirring rollers is 5 to 20 cm, and the equivalent diameter is 3 to 10 cm.

[0028] More preferably, the outer diameter of the secondary tank body is 30 to 100 cm, the thickness ranges from 2 to 35 cm, the height is 30 to 120 cm, and the material includes stainless steel, titanium alloy, glass, quartz glass, polytetrafluoroethylene, polyvinyl chloride or nickel-chromium-molybdenum alloy.

[0029] In some specific embodiments, the ultrasonic component includes an ultrasonic signal generator, a transducer, and an amplitude transformer.

[0030] In some specific embodiments, the inorganic component content control device includes a tertiary tank body connected to the secondary tank body, a negative pressure suction assembly and an inorganic component content monitor provided on the tertiary tank body, a tertiary stratification stirring assembly provided in the tertiary tank body, and a tertiary flow control valve provided on the liquid delivery pipeline at the outlet of the tertiary tank body.

[0031] As a more preferred embodiment, the outer diameter of the three-stage tank body is 30 to 100 cm, the thickness ranges from 2 to 35 cm, the height is 30 to 120 cm, and the materials include stainless steel, titanium alloy, glass, quartz glass, polytetrafluoroethylene, polyvinyl chloride, and nickel-chromium-molybdenum alloy.

[0032] As a more preferred embodiment, the three-stage layered stirring assembly includes a stirring blade and a motor. The structure of the stirring blade is selected from any one of paddle type, turbine type, propeller type, anchor type, frame type, ribbon type, and screw type. The material of the stirring blade includes but is not limited to stainless steel, carbon steel, carbon steel lined with rubber, carbon steel lined with fiberglass, the stirring roller speed is 50 to 5000 rpm, the stirring layer is 1 to 3 layers, the number of stirring rollers is 1 to 3, the material of the stirring roller includes but is not limited to stainless steel, carbon steel, rubber, cast iron, polyurethane, the spacing between the stirring rollers is 5 to 20 cm, and the equivalent diameter is 3 to 10 cm.

[0033] In some specific embodiments, the multi-jet electrospinning module includes a conveying assembly, a plurality of spinnerets located above the conveying assembly and connected to the liquid delivery pipeline, and a plurality of low-curvature liquid surface multi-jet nozzles provided at the bottom of the spinneret, wherein:

[0034] The conveying assembly comprises a conveying roller and a conveying belt arranged on the conveying roller;

[0035] The spinneret includes a thickness compensating spinneret arranged along the conveying direction of the conveying roller and a spinneret for ultrafine fibers vertically arranged between two adjacent thickness compensating spinnerets. The low-arc liquid surface multi-jet nozzle is arranged at the bottom of the thickness compensating spinneret and the spinneret for ultrafine fibers.

[0036] As a more preferred embodiment, the ultrafine fiber spinneret has a length of 80 to 320 cm, a width of 4 to 8 cm, a number of 4 to 16, a height of 4 to 8 cm, and is made of stainless steel, titanium alloy, nickel-based alloy, copper alloy, ceramic, tungsten carbide, and platinum;

[0037] The thickness compensating spinneret has a length of 20 to 120 cm, a width of 8 to 24 cm, a number of 4 to 16, a spinneret height of 4 to 8 cm, and materials including stainless steel, titanium alloy, nickel-based alloy, copper alloy, ceramic, tungsten carbide, and platinum.

[0038] In some specific embodiments, the low-curvature liquid surface multi-jet nozzle is arranged in an array, and the low-curvature liquid surface multi-jet nozzle includes a dumbbell-shaped liquid outlet channel that is wide at the top and bottom and narrow in the middle, a cantilever rod horizontally arranged inside the dumbbell-shaped liquid outlet channel, and a conductive wire vertically arranged on the cantilever rod and used to enhance the uniformity of the electric field.

[0039] As a more preferred embodiment, the inner diameters of the upper and lower ends of the outlet flow channel of the low-curvature liquid surface multi-jet nozzle are 1 to 4 mm, the inner diameter of the middle of the flow channel is 0.1 to 0.9 mm, the angle between the lower end flow channel and the extension line of the middle of the flow channel is 45 to 90°, and the nozzle length is 20 to 50 mm; the angle between the low-curvature liquid surface and the nozzle is 10 to 30°, and the number of jets from a single nozzle is 2 to 30;

[0040] The number of nozzles of the ultrafine fiber spinneret is 40 to 80, the nozzle spacing is 20 to 40 mm, and the number of nozzles arranged in one row on the ultrafine fiber spinneret is 1;

[0041] The number of nozzles of the thickness compensation spinneret is 20 to 40, the nozzle spacing is 40 to 60 mm, the number of liquid-discharging nozzles is 10 to 20, the number of non-liquid-discharging nozzles is 10 to 20, and the number of nozzles arranged in 2 to 4 rows on the thickness compensation spinneret is 2 to 4 rows.

[0042] The array arrangement of the low-curvature liquid surface multi-jet nozzles is selected from any one of a linear array, a rectangular array, a circular array, a spiral array, a triangular array, a honeycomb array, a random array, a staggered array, a spherical array, and a cubic array;

[0043] The height of the conductive wire is 15-45 mm, the structure of the conductive wire is selected from any one of a needle shape, a plate shape, a ring shape, and a column shape, and the material includes stainless steel, copper, aluminum or titanium.

[0044] In some specific embodiments, the temperature and humidity control device includes a microprocessor, a temperature and humidity detector electrically connected to the microprocessor and connected to the liquid delivery pipe, a bidirectional temperature control pipe connected to the spinneret for ultrafine fibers, a humidifier, and a temperature-control hollow plate connected to the bidirectional temperature control pipe and located under the conveyor belt.

[0045] As a more preferred embodiment, the air flow temperature range of the bidirectional temperature control pipe is -20 to 90°C, the pipe thickness is 0.3 to 3cm, the outer diameter is 2 to 10cm, the temperature range of the temperature control hollow plate is -10 to 80°C, the thickness is 3 to 5cm, the length is 5 to 10cm, the number is 3 to 10, the plate spacing is 2 to 10cm, and the materials include stainless steel, carbon steel, galvanized steel, and aluminum alloy.

[0046] As a more preferred embodiment, the humidity adjustment range of the humidifier is 10 to 99%.

[0047] In some specific embodiments, the solvent vapor removal device includes a shell connected to a liquid delivery pipe, a main suction duct arranged in the inner cavity of the shell, a secondary suction duct located on the outer wall of the shell, and a gradient distributed honeycomb partition arranged in the main suction duct and the secondary suction duct along the axial direction of the suction duct.

[0048] As a more preferred embodiment, the thickness of the main suction duct is 0.5-2 cm, the diameter is 5-20 cm, the number is 1-3, and the material includes galvanized steel plate, stainless steel, aluminum alloy, PVC plastic;

[0049] The secondary air suction duct has a thickness of 0.5-2 cm, a diameter of 2-10 cm, a number of 2-6, and is made of galvanized steel, stainless steel, aluminum alloy, or PVC plastic.

[0050] The diameter of the gradient distribution honeycomb partition is 2-20 cm.

[0051] In some specific embodiments, the static electricity elimination and insulation device includes a nozzle insulation base arranged between the spinneret and the low-curvature liquid surface multi-jet nozzle, an insulating plate arranged at both ends of the bottom of the spinneret, an anti-static voltage roller arranged on the conveyor belt, and an inner insulating layer and an outer insulating tube arranged relatively inside and outside the low-curvature liquid surface multi-jet nozzle.

[0052] As a more preferred embodiment, the number of the static voltage removing rollers is 3 to 10;

[0053] The materials of the nozzle insulation base, the inner insulation layer, the outer insulation tube, the insulation plate and the anti-static voltage roller include polyoxymethylene, polypropylene, polyethylene, polycarbonate, poly(p-phenylene terephthalamide), polyvinyl chloride or polyetheretherketone.

[0054] In some specific embodiments, the multi-temperature zone temperature control device includes a central processing unit, a temperature sensor electrically connected to the central processing unit, an analog-to-digital converter, a heating element combination distributor, and a heating roller located below the drying zone, microwave pretreatment zone, polymer removal zone, and oxygen-deficient atmosphere heat treatment zone.

[0055] In some specific embodiments, the drying zone is provided with a first heating element electrically connected to the multi-zone temperature control device, the microwave pretreatment zone is provided with a microwave generator, a microwave reflector, a second heating element electrically connected to the multi-zone temperature control device, and a waveguide connected to the microwave generator, the polymer removal zone is provided with a third heating element electrically connected to the multi-zone temperature control device, the oxygen-deficient atmosphere heat treatment zone is provided with an atmosphere concentration controller, a fourth heating element electrically connected to the multi-zone temperature control device, and a dual-cavity supply device electrically connected to the atmosphere concentration controller, and the cooling zone is provided with a fifth heating element electrically connected to the multi-zone temperature control device.

[0056] In some specific embodiments, the winding system includes a winding support and a winding roller disposed on the winding support.

[0057] More preferably, the winding roller is made of aluminum alloy, stainless steel, polypropylene, polyethylene, or carbon fiber, and has a diameter of 30 to 100 cm.

[0058] The second technical solution of the present invention is to provide a method for continuous and large-scale preparation of flexible and elastic ceramic ultrafine fiber materials. The continuous and large-scale preparation device of flexible and elastic ceramic ultrafine fiber materials according to one of the above technical solutions comprises the following steps:

[0059] S1, putting the raw materials into a mixing device for mixing, low-temperature dispersion, vacuum concentration, and removing the solvent to obtain a sol;

[0060] S2, the sol and polymer obtained in step S1 are flowed into a polymer mixing device for mixing and degassing;

[0061] S3, the mixed sol obtained by the treatment in step S2 flows into the inorganic component content control device, and is sucked by negative pressure to obtain a spinning solution;

[0062] S4, flowing the spinning solution obtained in step S3 into a multi-jet electrospinning module, regulating the temperature, humidity, and multi-directional differential velocity during spinning, to obtain a fiber membrane material or a fiber flake material;

[0063] S5, sequentially conveying the fiber material obtained in step S4 to a drying zone, a microwave pretreatment zone, a polymer removal zone, an oxygen-deficient atmosphere heat treatment zone, and a cooling zone for multi-temperature zone calcination to obtain a flexible and elastic ceramic ultrafine fiber material;

[0064] S6. The flexible and elastic ceramic ultrafine fiber material obtained in step S5 is rolled up and packaged through a rolling system.

[0065] In some specific embodiments, in step S1, inorganic salts, solvents, and catalysts are put into a primary tank body, and the primary layered stirring component is turned on for stirring, while the in-situ infrared analyzer and the viscosity detector are turned on for monitoring respectively, the gelation inhibition component is turned on to allow the low-temperature inert atmosphere to flow around the outer wall of the primary tank body and into the primary tank body, and the vacuum concentration component is turned on for vacuum concentration, wherein the inert atmosphere is selected from any one or more of nitrogen, helium, neon, argon, krypton or xenon, the temperature of the inert atmosphere is 5 to 25°C, and the vacuum degree range is: -0.01 to -0.1 MPa.

[0066] More preferably, the inorganic salt is selected from any one or more of silicon salts, titanium salts, zirconium salts or aluminum salts, wherein:

[0067] The silicon salt is selected from any one or more of tetraethyl orthosilicate, tetra-n-propoxysilane, tetraethoxysilane or methyltriethoxysilane;

[0068] The titanium salt is selected from any one or more of isopropyl titanate, butyl titanate, titanium n-propoxide, titanium isopropoxide, titanium n-butoxide, titanium isobutoxide or titanium n-octoxide;

[0069] The zirconium salt is selected from any one or more of zirconium n-propoxide, zirconium isopropoxide, zirconium n-butoxide, zirconium isobutoxide or zirconium n-octoxide;

[0070] The aluminum salt is selected from any one or more of aluminum isopropoxide, aluminum n-butoxide, aluminum isobutoxide, aluminum n-propoxide or aluminum ethoxide;

[0071] The inorganic salt component accounts for 20 to 70 wt % of the spinning solution.

[0072] More preferably, the solvent is selected from any one or more of deionized water, alcohol solvent or non-polar solvent, wherein:

[0073] The alcohol solvent is selected from any one or more of methanol, ethanol, isopropanol, butanol, pentanol, hexanol, ethylene glycol, propylene glycol, benzyl alcohol, allyl alcohol or octanol;

[0074] The non-polar solvent is selected from any one or more of carbon tetrachloride, benzene, toluene, dichloromethane, chloroform, ether, diphenyl ether, ethyl acetate, acetone, tetrahydrofuran, N-methylpyrrolidone or N,N-dimethylformamide.

[0075] More preferably, the catalyst is selected from any one or more of oxalic acid, acetic acid, phosphoric acid, hydrofluoric acid or trifluoroacetic acid.

[0076] More preferably, the spinning solution can be kept in an ungelled state for 200 to 400 hours.

[0077] In some specific embodiments, in step S2, the sol and polymer obtained by the treatment in step S1 flow into the secondary tank, and while the secondary stratification stirring component is turned on for stirring, the ultrasonic component is turned on to mix the sol and the polymer, and the bubble removal component is turned on to remove bubbles during mixing, and the ultrasonic output frequency range of the ultrasonic component is 20 to 130 kHz.

[0078] More preferably, the molecular weight of the polymer is in the range of 1-50W, and the polymer is selected from any one or more of polyvinyl alcohol, hydroxypropyl methylcellulose, polyethylene oxide, polyvinyl pyrrolidone, polyacrylonitrile, polylactic acid, and polymethyl methacrylate.

[0079] In some specific embodiments, in step S3, the mixed sol obtained by processing in step S2 flows into a three-stage tank body, and while the three-stage stratified stirring component is turned on for mixing, the negative pressure suction component is turned on to make the inside of the three-stage tank body a low pressure or negative pressure state to remove the solvent, and the inorganic component content monitor is turned on for monitoring.

[0080] More preferably, the suction pressure range of the negative pressure suction component is 0-5MPa.

[0081] More preferably, the viscosity of the spinning solution is 0.1 to 1000 mPa·s.

[0082] In some specific embodiments, in step S4, the spinning solution obtained in step S3 is sprayed out through the low-curvature liquid surface multi-jet nozzle of the spinneret to a conveyor belt for deposition and forming, the solvent vapor removal device and the static elimination and insulation device are turned on, the temperature and humidity control device is turned on to adjust the temperature at the low-curvature liquid surface multi-jet nozzle to 10-30°C, the temperature at the conveyor belt is adjusted to 20-50°C, the humidity of the spinning environment is 10-99%, the movement speed of the spinneret for ultrafine fibers is 0.4-0.6m / min, the movement speed of the thickness compensation spinneret is 0.4-0.6m / min, and the conveying speed of the conveying roller is 0.2-0.5m / min.

[0083] In some specific embodiments, in step S5, the temperature of the drying zone is 180-220°C, the temperature of the microwave pretreatment zone is 350-450°C, the frequency is 300-300000 MHz, the temperature of the polymer removal zone is 550-600°C, the temperature of the oxygen-deficient atmosphere heat treatment zone is 700-1200°C, the oxygen concentration is less than 20%, the temperature of the cooling zone is 160-200°C, and the heating temperature of the heating rod is 20-1300°C.

[0084] The preparation method provided by the present invention is to prepare a flexible and elastic ceramic ultrafine fiber material by real-time configuration of the spinning raw material through a spinning solution, multi-jet electrospinning and continuous low-temperature calcination. It is an efficient and stable molding method for ceramic fiber materials, which greatly improves the mechanical properties of ceramic fiber materials and realizes continuous and large-scale production of flexible and elastic ceramic ultrafine fiber materials, wherein:

[0085] (1) In the process of preparing the spinning solution: the hydrolysis-polycondensation reaction rate of the inorganic alcohol salt in the large-capacity reaction device is monitored and analyzed online by in-situ infrared analysis equipment, and the sol state is detected in real time in combination with the viscosity online monitoring equipment, thereby realizing the online real-time preparation of the sol; a vacuum concentration component is used to remove the solvent to promote the forward reaction; a cold air device is used to generate a low-temperature inert gas, so that the cold air flows around the outer wall of the first-stage tank, and an insulation layer is configured on the outer layer to reduce temperature changes. At the same time, the cold air enters the first-stage tank to increase the sol flow rate, accelerate the diffusion of each component, and inhibit the gelation of the sol, thereby ensuring the long-term stable and controllable preparation of the polymer / sol spinning solution.

[0086] (2) In the multi-jet electrospinning process of the spinning solution: the spinning environment is controlled by using a temperature and humidity control device in the nozzle area and the receiving area to achieve precise control of the fiber morphology and structure; a solvent vapor rapid removal device is set, and a honeycomb partition is set in the main suction duct to reduce the impact of the airflow on the jet, thereby achieving environmentally friendly and efficient treatment of the solvent; the fiber is made to perform multi-directional differential motion in the jet deposition direction, the spinneret movement direction, and the conveying mechanism movement direction, thereby regulating the degree of fiber entanglement and ensuring the controllable forming of the fiber membrane material and the fiber flake material.

[0087] (3) During the low-temperature calcination of the ceramic ultrafine fiber material, the microwave pretreatment zone is used to break down the long polymer macromolecule chains into short small molecular chains under the dual effects of the electromagnetic field and the thermal flow field, which is conducive to the rapid and complete removal of the polymer template; the oxygen concentration at the grain boundary is reduced by the oxygen-deficient atmosphere heat treatment zone, which slows down the grain growth, reduces the pore defects in the fiber, and promotes the densification of the fiber, thereby obtaining a ceramic ultrafine fiber material with soft / elastic properties.

[0088] In summary, the preparation method proposed by the present invention has the following improvements:

[0089] (1) Stable storage of inorganic sol: The low-temperature inert atmosphere flows around the outer wall of the primary tank and enters the interior of the primary tank, accelerating the diffusion of each component, thereby inhibiting the instability and gelation of the sol.

[0090] (2) Control of the inorganic component content of the spinning solution: The prepared spinning solution is subjected to negative pressure suction to control the overlapping concentration of the polymer concentration, and the solution is monitored in real time using an inorganic component content monitor to obtain a polymer / inorganic colloid spinning solution with controllable inorganic component content.

[0091] (3) Uniform and stable spinning of multi-jet electrospinning module: By setting a low-curvature liquid surface multi-jet nozzle, the number of jets at the nozzle is increased, and a spinneret for ultrafine fibers and a thickness compensation spinneret equipped with multiple low-curvature liquid surface multi-jet nozzles are configured to allow the fibers to be evenly deposited on the conveyor belt.

[0092] (4) Regulation of single fiber morphology: By controlling the temperature and humidity in the nozzle area and the receiving area respectively, fibers with different degrees of curling can be obtained.

[0093] (5) Preparation of various types of fiber materials: Through a multi-jet electrospinning module, straight fibers or curly fibers are subjected to differential motion in the direction of jet deposition, spinneret movement, and conveyor belt movement, thereby regulating the degree of entanglement between fibers and obtaining fiber membrane materials or fiber flake materials.

[0094] (6) Rapid removal of polymer templates: By setting up a microwave pretreatment zone in the low-temperature calcination system, under the dual effects of the electromagnetic field and the thermal flow field, the long polymer molecular chains are broken down into small molecular short chains that are easy to remove, thereby promoting the rapid and complete removal of the polymer template.

[0095] (7) Preparation of flexible and elastic ceramic ultrafine fiber materials: The fibers are calcined in an oxygen-deficient atmosphere in an oxygen-deficient atmosphere heat treatment zone to reduce the oxygen concentration at the grain boundaries, thereby inhibiting the growth of grains and promoting the densification of the fibers. The grains inside the fibers are small, the grain boundaries are numerous, and the pore defects are few, which is beneficial to the transmission and dissipation of stress inside the fibers. The ceramic ultrafine fiber materials exhibit good flexibility. BRIEF DESCRIPTION OF THE DRAWINGS

[0096] Figure 1 It is a structural schematic diagram of the present invention.

[0097] Figure 2 Schematic diagram of a single nozzle with multiple jets at a low-arc liquid surface.

[0098] The following are marked in the figure:

[0099] 1-mixing device, 101-in-situ infrared analyzer, 102-viscosity detector, 1031-first-level feeding port, 1032-first-level tank, 104-vacuum concentration component, 1041-vacuum concentrator, 1042-heat exchanger, 1043-condensed water tank, 1044-vacuum pump, 105-gelation inhibition component, 1051-cold air component, 1052-low temperature pipe, 1053-insulation layer, 1054-jet nozzle, 106-first-level layered stirring component, 107-first-level flow control valve, 2-polymer mixing device, 2011-secondary feeding port, 20 12-secondary tank, 202-ultrasonic component, 2021-ultrasonic signal generator, 2022-transducer, 2023-amplifier, 203-bubble removal component, 204-secondary stratified stirring component, 205-secondary flow control valve, 3-inorganic component content control device, 301-third-level stratified stirring component, 302-negative pressure suction component, 303-inorganic component content monitor, 304-third-level flow control valve, 4-multi-jet electrospinning module, 401-low-curvature liquid surface multi-jet nozzle, 4011-dumbbell-shaped flow channel, 4012-conductive wire, 4013- Cantilever rod, 4021-spinneret for ultrafine fiber, 4022-thickness compensation spinneret, 4023-transmission component, 5-temperature and humidity control device, 501-temperature and humidity detector, 502-microprocessor, 503-bidirectional temperature control pipeline, 504-temperature control hollow plate, 505-wetting device, 6-solvent vapor rapid removal device, 601-main suction duct, 602-secondary suction duct, 603-gradient distribution honeycomb partition, 7-static elimination and insulation device, 701-nozzle insulation base, 702-insulation board, 703-static voltage roller, 704-inner insulation layer, 7 05-external insulation tube, 8-multi-temperature zone temperature control device, 801-heating element combination distributor, 802-temperature sensor, 803-analog-to-digital converter, 804-central processing unit, 805-heating rod, 9-drying zone, 10-microwave pretreatment zone, 1001-microwave generator, 1002-waveguide, 1003-microwave reflector, 11-polymer removal zone, 12-oxygen-poor atmosphere heat treatment zone, 1201-double air cavity supply equipment, 1202-atmosphere concentration controller, 13-cooling zone, 1401-winding roller, 1402-winding bracket, 15-liquid delivery pipeline. DETAILED DESCRIPTION

[0100] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0101] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0102] In conjunction with the accompanying drawings, some embodiments of the present invention are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments may be combined with each other.

[0103] In the following embodiments, if there is no special description of functional components or structures, it means that they are all conventional components or conventional structures used in the art to achieve corresponding functions. If there is no special description of raw materials or processing techniques, it means that they are all conventional commercially available raw material products or conventional processing techniques in the art.

[0104] Embodiment 1:

[0105] like Figure 1 As shown, a continuous large-scale preparation device for flexible and elastic ceramic ultrafine fiber materials includes a feeding and liquid preparation system, a multi-jet uniform electrospinning system, a low-temperature calcination system, and a winding system.

[0106] The feeding and liquid dispensing system comprises a mixing device 1, a polymer mixing device 2, and an inorganic component content control device 3 which are connected in series via a liquid delivery pipeline 15 in sequence;

[0107] The multi-jet uniform electrospinning system comprises a temperature and humidity control device 5, a multi-jet electrospinning module 4 and a solvent vapor removal device 6 electrically connected to the temperature and humidity control device 5 and connected to the inorganic component content control device 3, and a static elimination and insulation device 7 connected to the multi-jet electrospinning module 4;

[0108] The low-temperature calcination system includes a multi-zone temperature control device 8, a drying zone 9, a microwave pretreatment zone 10, a polymer removal zone 11, an oxygen-deficient atmosphere heat treatment zone 12, and a cooling zone 13 which are sequentially connected to the multi-zone temperature control device 8 and are independently separated.

[0109] in:

[0110] In the feeding and liquid dispensing system, the mixing device 1 includes a primary tank 1032, an in-situ infrared analyzer 101, a viscosity detector 102, a primary feeding port 1031, a vacuum concentration component 104, a gelation inhibition component 105 wrapped around the primary tank 1032 and the bottom, a primary layered stirring component 106 disposed in the primary tank 1032, and a primary flow control valve 107 disposed on the liquid delivery pipeline () at the outlet of the mixing device 1. The vacuum concentration component 104 includes a vacuum concentrator 1041, a heat exchanger 1042, a condensed water tank 1043, and a vacuum pump 1044. The gelation inhibition component 105 includes a cold air component 1051, a low-temperature pipe 1052 connected to the cold air component 1051 and surrounding the body and bottom of the first-level tank body 1032, and a thermal insulation layer 1053 arranged on the outside of the low-temperature pipe 1052. The low-temperature pipe 1052 is provided with a plurality of jet ports 1054 that penetrate the bottom of the first-level tank body 1032. The hydrolysis-polycondensation reaction rate of the inorganic alcohol salt in the primary tank 1032 is monitored and analyzed online by the in-situ infrared analyzer 101, and the sol state is detected in real time in combination with the viscosity detector 102, thereby realizing online real-time configuration of the sol; the vacuum concentration component 104 is used to remove the solvent to promote the forward reaction; the cold air component 1051 is used to generate low-temperature inert gas, so that the cold air flows around the outer wall of the primary tank, and an insulation layer is configured on the outer layer to reduce temperature changes. At the same time, the cold air enters the primary tank 1032 to increase the sol flow rate, accelerate the diffusion of each component, and inhibit the gelation of the sol, thereby ensuring the long-term stable and controllable preparation of the polymer / sol spinning solution.

[0111] As a preferred technical solution, the first-level layered stirring assembly 106 includes a stirring blade and a motor. The structure of the stirring blade is selected from any one of paddle type, turbine type, propulsion type, anchor type, frame type, spiral belt type, and screw type. The material of the stirring blade includes stainless steel, carbon steel, carbon steel lined with rubber, and carbon steel lined with fiberglass. The speed of the stirring roller is 50 to 5000 rpm, the number of stirring layers is 1 to 5, the number of stirring rollers is 1 to 5, and the material of the stirring roller includes stainless steel, carbon steel, rubber, cast iron, and polyurethane. The spacing between the stirring rollers is 5 to 20 cm, and the equivalent diameter is 3 to 10 cm. The outer diameter of the first-level can 1032 is 30 to 100 cm, the thickness is 2 to 35 cm, and the height is 60 to 160 cm. The material includes stainless steel, titanium alloy, glass, quartz glass, polytetrafluoroethylene, and nickel-chromium-molybdenum alloy. The number of the jet ports 1054 is 5-20, the diameter of the jet ports 1054 is 1-5 cm, and the materials include stainless steel, galvanized steel, aluminum alloy, polyethylene, and polytetrafluoroethylene. The thickness of the cryogenic tube 1052 is 0.2-2 cm, the outer diameter is 2-10 cm, and the materials of the cryogenic tube 1052 include stainless steel, low-temperature carbon steel, and alloy steel. The thickness of the thermal insulation layer 1053 is 2-5 cm, and the materials of the thermal insulation layer 1053 include glass fiber, polyurethane foam, rock wool, and aluminum silicate fiber.

[0112] The polymer mixing device 2 includes a secondary tank 2012 connected to the primary tank 1032, a secondary feeding port 2011, an ultrasonic component 202, and a bubble removal component 203 provided on the secondary tank 2012, a secondary layered stirring component 204 provided in the secondary tank 2012, and a secondary flow control valve 205 provided on the liquid delivery pipeline 15 at the outlet of the secondary tank 2012. The ultrasonic component 202 includes an ultrasonic signal generator 2021, a transducer 2022, and an amplitude transformer 2023.

[0113] As a preferred technical solution, the secondary layered stirring assembly 204 includes a stirring blade and a motor, the structure of the stirring blade is selected from any one of paddle type, turbine type, propulsion type, anchor type, frame type, spiral belt type, and screw type, the material of the stirring blade includes stainless steel, carbon steel, carbon steel lined with rubber, and carbon steel lined with fiberglass, the speed of the stirring roller is 50-5000rpm, the stirring layer is 1-3 layers, the number of stirring rollers is 1-3, the material of the stirring roller includes stainless steel, carbon steel, rubber, cast iron, and polyurethane, the spacing between the stirring rollers is 5-20cm, and the equivalent diameter is 3-10cm. The outer diameter of the secondary tank body 2012 is 30-100cm, the thickness ranges from 2-35cm, and the height is 30-120cm, and the material includes stainless steel, titanium alloy, glass, quartz glass, polytetrafluoroethylene, polyvinyl chloride, or nickel-chromium-molybdenum alloy.

[0114] The inorganic component content control device 3 includes a tertiary tank 305 connected to the secondary tank 2012, a negative pressure suction assembly 302 and an inorganic component content monitor 303 provided on the tertiary tank 305, a tertiary layered stirring assembly 301 provided in the tertiary tank 305, and a tertiary flow control valve 304 provided on the liquid delivery pipeline 15 at the outlet of the tertiary tank 305. The configured spinning solution is subjected to negative pressure suction to control the overlapping concentration of the polymer concentration, and the solution is monitored in real time using the inorganic component content monitor 303 to obtain a polymer / inorganic colloid spinning solution with controllable inorganic component content.

[0115] As a preferred technical solution, the outer diameter of the three-stage tank 305 is 30-100 cm, the thickness ranges from 2-35 cm, and the height is 30-120 cm. The materials include stainless steel, titanium alloy, glass, quartz glass, polytetrafluoroethylene, polyvinyl chloride, and nickel-chromium-molybdenum alloy. The three-stage layered stirring assembly 301 includes stirring blades and a motor. The structure of the stirring blades is selected from any one of paddle type, turbine type, propulsion type, anchor type, frame type, spiral belt type, and screw type. The material of the stirring blades includes but is not limited to stainless steel, carbon steel, carbon steel lined with rubber, and carbon steel lined with glass fiber reinforced plastic. The stirring roller speed is 50-5000 rpm, the stirring layer is 1-3 layers, the number of stirring rollers is 1-3, the material of the stirring rollers includes but is not limited to stainless steel, carbon steel, rubber, cast iron, and polyurethane. The spacing between the stirring rollers is 5-20 cm, and the equivalent diameter is 3-10 cm.

[0116] In the multi-jet uniform electrospinning system, the multi-jet electrospinning module 4 includes a transmission component 4023, a plurality of spinnerets located above the transmission component 4023 and connected to the liquid delivery pipeline 15, and a plurality of low-curvature liquid surface multi-jet nozzles 401 provided at the bottom of the spinneret, wherein:

[0117] The conveying assembly 4023 includes a conveying roller and a conveying belt arranged on the conveying roller;

[0118] The spinneret includes a thickness compensation spinneret 4022 arranged along the conveying direction of the conveying roller, and a superfine fiber spinneret 4021 vertically arranged between two adjacent thickness compensation spinnerets 4022, and the low-curvature liquid surface multi-jet nozzle 401 is arranged at the bottom of the thickness compensation spinneret 4022 and the superfine fiber spinneret 4021. The low-curvature liquid surface multi-jet nozzle 401 is arranged in an array, and the low-curvature liquid surface multi-jet nozzle 401 includes a dumbbell-shaped liquid outlet flow channel 4011 that is wide at the top and bottom and narrow in the middle, a cantilever rod 4013 horizontally arranged inside the dumbbell-shaped liquid outlet flow channel 4011, and a conductive filament 4012 vertically arranged on the cantilever rod 4013 and used for uniform electric field enhancement. By setting the low-curvature liquid surface multi-jet nozzle 401, the number of jets from the nozzle is increased, so that the fibers are evenly deposited on the conveyor belt.

[0119] The temperature and humidity control device 5 includes a microprocessor 502, a temperature and humidity detector 501 electrically connected to the microprocessor 502 and connected to the liquid delivery pipe 15, a bidirectional temperature control pipe 503 connected to the ultrafine fiber spinneret 4021, a humidifier 505, and a temperature control hollow plate 504 connected to the bidirectional temperature control pipe 503 and located under the conveyor belt. The temperature and humidity of the nozzle area and the receiving area are respectively controlled by the bidirectional temperature control pipe 503 and the humidifier 505, so as to obtain fibers with different curling degrees.

[0120] The solvent vapor removal device 6 includes a shell connected to the liquid delivery pipe 15, a main suction pipe 601 arranged in the inner cavity of the shell, a secondary suction pipe 602 located on the outer wall of the shell, and a gradient distributed honeycomb partition 603 arranged in the main suction pipe 601 and the secondary suction pipe 602 along the axial direction of the suction pipe.

[0121] The static electricity elimination and insulation device 7 includes a nozzle insulation base 701 arranged between the spinneret and the low-curvature liquid surface multi-jet nozzle 401, an insulation plate 702 arranged at both ends of the bottom of the spinneret, an anti-static voltage roller 703 arranged on the conveyor belt, and an inner insulation layer 704 and an outer insulation tube 705 arranged relatively inside and outside the low-curvature liquid surface multi-jet nozzle 401.

[0122] The spinning environment is controlled by the temperature and humidity control device 5 in the nozzle area and the receiving area, so that the fiber morphology structure can be precisely controlled. A solvent vapor rapid removal device 6 is provided, and a honeycomb partition 603 is provided in the main suction duct 601 and the secondary suction duct 602 to reduce the influence of the airflow on the jet, thereby realizing environmentally friendly and efficient treatment of the solvent. The fiber is made to perform multi-directional differential motion in different directions of jet deposition, spinneret movement direction, and conveying mechanism movement, so as to control the degree of fiber entanglement and ensure the controllable forming of fiber membrane materials and fiber flake materials.

[0123] As an optimal technical solution, the inner diameters of the upper and lower ends of the liquid outlet channel of the low-curvature liquid surface multi-jet nozzle 401 are 1 to 4 mm, the inner diameter of the middle part of the channel is 0.1 to 0.9 mm, the angle between the lower end channel and the extension line of the middle part of the channel is 45 to 90°, and the nozzle length is 20 to 50 mm; the angle between the low-curvature liquid surface and the nozzle is 10 to 30°, and the number of jets from a single nozzle is 2 to 30; the length of the ultrafine fiber spinneret 4021 is 80 to 320 cm, the width is 4 to 8 cm, the number is 4 to 16, and the height is 4 to 8 cm. The materials include stainless steel, titanium alloy, nickel-based alloy, copper alloy, ceramic, tungsten carbide, and platinum. The number of nozzles of the ultrafine fiber spinneret 4021 is 40 to 80, the nozzle spacing is 20 to 40 mm, and the number of nozzles arranged on the ultrafine fiber spinneret 4021 is 1 row. The thickness compensation spinneret 4022 has a length of 20 to 120 cm, a width of 8 to 24 cm, a number of 4 to 16, and a height of 4 to 8 cm. The material includes stainless steel, titanium alloy, nickel-based alloy, copper alloy, ceramic, tungsten carbide, and platinum. The thickness compensation spinneret 4022 has 20 to 40 nozzles, a nozzle spacing of 40 to 60 mm, 10 to 20 nozzles that discharge liquid, 10 to 20 nozzles that do not discharge liquid, and 2 to 4 nozzles on the thickness compensation spinneret 4022. The array arrangement of the low-curvature liquid surface multi-jet nozzle 401 is selected from any one of a linear array, a rectangular array, a circular array, a spiral array, a triangular array, a honeycomb array, a random array, a staggered array, a spherical array, and a cubic array. The height of the conductive wire 4012 is 15-45mm, and the structure of the conductive wire 4012 is selected from any one of needle-shaped, plate-shaped, ring-shaped, and column-shaped, and the material includes stainless steel, copper, aluminum, or titanium. The air flow temperature range of the bidirectional temperature control pipe 503 is -20 to 90°C, the pipe thickness is 0.3 to 3cm, and the outer diameter is 2 to 10cm. The temperature range of the temperature control hollow plate is -10 to 80°C, the thickness is 3 to 5cm, the length is 5 to 10cm, the number is 3 to 10, the plate spacing is 2 to 10cm, and the material includes stainless steel, carbon steel, galvanized steel, and aluminum alloy. The humidity adjustment range of the humidifier 505 is 10 to 99%. The thickness of the main suction pipe 601 is 0.5-2cm, the diameter is 5-20cm, the number is 1-3, and the material includes galvanized steel plate, stainless steel, aluminum alloy, and PVC plastic. The thickness of the secondary air suction duct 602 is 0.5-2 cm, the diameter is 2-10 cm, the number is 2-6, and the materials include galvanized steel plate, stainless steel, aluminum alloy, and PVC plastic. The diameter of the gradient distribution honeycomb partition 603 is 2-20 cm. There are 3 to 10 static voltage removal rollers 703. The materials of the nozzle insulation base 701, the inner insulation layer 704, the outer insulation tube 705, the insulation plate 702 and the static voltage removal roller 703 include polyoxymethylene, polypropylene, polyethylene, polycarbonate, poly(p-phenylene terephthalamide), polyvinyl chloride or polyetheretherketone.

[0124] In the low-temperature calcination system part, the multi-temperature zone temperature control device 8 includes a heating element combination distributor 801, a temperature sensor 802, an analog-to-digital converter 803, a central processing unit 804 and a heating rod 805 arranged below the drying zone 9, the microwave pretreatment zone 10, the polymer removal zone 11, and the oxygen-deficient atmosphere heat treatment zone 12. The drying zone 9 is provided with a first heating element electrically connected to the heating element combination distributor 801, the microwave pretreatment zone 10 is provided with a microwave generator 1001 electrically connected to the central processing unit 804, a microwave reflector 1003, a second heating element electrically connected to the heating element combination distributor 801, and a waveguide 1002 connected to the microwave generator 1001, the polymer removal zone 11 is provided with a third heating element electrically connected to the heating element combination distributor 801, the oxygen-deficient atmosphere heat treatment zone 12 is provided with an atmosphere concentration controller 1202 electrically connected to the central processing unit 804, a fourth heating element electrically connected to the heating element combination distributor 801, and a dual-cavity supply device 1201 electrically connected to the atmosphere concentration controller 1202, and the cooling zone 13 is provided with a fifth heating element electrically connected to the heating element combination distributor 801.

[0125] The microwave pretreatment zone 10 is used to break down the polymer macromolecular long chains into small molecular short chains under the dual effects of the electromagnetic field and the heat flow field, which is helpful for the rapid and complete removal of the polymer template. The oxygen concentration at the grain boundary is reduced by the oxygen-deficient atmosphere heat treatment zone 12, which slows down the grain growth, reduces the hole defects in the fiber, and promotes the densification of the fiber, thereby obtaining a ceramic ultrafine fiber material with soft / elastic properties.

[0126] The winding system includes a winding support and a winding roller 1401 disposed on the winding support 1402 .

[0127] As a preferred technical solution, the material of the winding roller 1401 includes aluminum alloy, stainless steel, polypropylene, polyethylene, carbon fiber, and the diameter is 30 to 100 cm.

[0128] Embodiment 2:

[0129] Based on the continuous large-scale preparation device of a flexible and elastic ceramic ultrafine fiber material in Example 1, this embodiment provides a continuous large-scale preparation method of a flexible and elastic ceramic ultrafine fiber membrane material, comprising the following steps:

[0130] The first step: turn on the primary stratified stirring component 106, set the rotation speed of the primary stratified stirring roller to 5000rpm, feed 12kg of tetraethoxysilane, 2kg of deionized water, 3.5kg of ethanol, and 15g of hydrochloric acid into the primary tank 1032 from the primary feeding port 1031 at one time, turn on the in-situ infrared analyzer 101 to detect the hydrolysis-polycondensation reaction rate of the alcohol salt, turn on the viscosity detector 102 to detect the sol state in real time, turn on the vacuum concentration component 104 to set the vacuum degree to -0.098MPa, turn on the gelation inhibition component 105 to adjust the cold air temperature, so that 20°C low-temperature helium flows around the outer wall of the primary tank 1032, and flows into the primary tank 1032 from the jet port 1054 to accelerate the diffusion of each component, and the prepared silica sol can be stably stored for 400 hours without gelation.

[0131] Open the secondary stratification stirring component 204 and set the rotation speed of the secondary stratification stirring roller to 4900rpm, open the primary flow control valve 107 to allow the configured silica sol to flow into the secondary tank 2012, feed 100,000 molecular weight polyvinyl alcohol into the secondary tank 2012 through the secondary feeding port 2011, turn on the ultrasonic component 22 and the bubble removal component 203 so that the output frequency is 80kHz, so that the polymer is fully dissolved in the sol.

[0132] Open the secondary flow control valve 205 to allow the mixed liquid to flow into the tertiary tank 305, open the tertiary stratification stirring assembly 301 and set the rotation speed of the tertiary stratification stirring roller to 4500rpm, turn on the negative pressure suction assembly 302, set the pressure of the suction pump to 3MPa, remove a large amount of solvent and discharge it, and turn on the inorganic component content monitor 303.

[0133] Step 2: Make the spinning liquid flow into the ultrafine fiber spinneret 4021, the thickness compensation spinneret 4022 and the low-curvature liquid surface multi-jet nozzle 401 in sequence through the liquid delivery pipe 15. The inner diameters of the upper and lower ends of the flow channel in the nozzle are 2 mm, the inner diameter of the middle part of the flow channel is 0.5 mm, the angle between the lower end flow channel and the extension line of the middle part of the flow channel is 45°, and the nozzle length is 45 mm. The height of the conductive wire 4012 is 35 mm, the angle between the low-arc liquid surface and the nozzle is 30°, the number of single nozzle jets is 20, the length of the ultrafine fiber spinneret 4021 is 200 cm, the length of the thickness compensating spinneret 4022 is 120 cm, the height of the spinnerets is 6 cm, the number of nozzles on the ultrafine fiber spinneret 4021 is 65, and the nozzle spacing is 26 mm, the number of nozzles on the thickness compensating spinneret 4022 is 40, and the nozzle spacing is 25 mm, of which 20 are liquid-discharging nozzles and 20 are non-liquid-discharging nozzles.

[0134] The conveying roller, the ultrafine fiber spinneret 4021 and the thickness compensation spinneret 4022 move along their axes, i.e. in different directions. The spinneret movement speed is 0.55 m / min, the conveying roller movement speed is 0.45 m / min, the temperature and humidity control device 5 is turned on, and the relative ambient humidity of the spinning area is adjusted to 38%, the nozzle area temperature is 18°C, and the receiving area temperature is 23°C.

[0135] The solvent vapor rapid removal device 6 is turned on to remove the solvent in the spinning zone, so that the jet is deposited evenly and stably. The number of the static-eliminating voltage rollers 703 is 5.

[0136] Step 3: Send the hybrid fiber membrane into the low-temperature calcination system, turn on the multi-temperature zone temperature control device 8, set the temperature of the drying zone 9 to 180°C, the temperature of the microwave pretreatment zone 10 to 400°C, the temperature of the polymer removal zone 11 to 600°C, the temperature of the oxygen-deficient atmosphere heat treatment zone 12 to 800°C, the oxygen concentration is less than 20%, the temperature of the cooling zone 13 to 200°C, the frequency of the microwave generator 1001 is set to 300000MHz, and the hybrid fiber membrane after cooling is rolled and packaged to finally obtain a flexible silica fiber membrane with a production capacity of 54m 2 / h.

[0137] Embodiment 3:

[0138] Based on the continuous large-scale preparation device of a flexible and elastic ceramic ultrafine fiber material in Example 1, this embodiment provides a continuous large-scale preparation method of a flexible and elastic ceramic ultrafine fiber membrane material, comprising the following steps:

[0139] The first step: open the primary layered stirring component 106, set the rotation speed of the primary layered stirring roller to 5000rpm, feed 4kg of zirconium n-propoxide, 0.3kg of deionized water, 15kg of ethanol, and 2.5kg of acetic acid into the primary tank body 1032 from the primary feeding port 1031 at one time, open the in-situ infrared analyzer 101 to detect the hydrolysis-polycondensation reaction rate of the alcohol salt, open the viscosity detector 102 to detect the sol state in real time, open the vacuum concentration component 104 to set the vacuum degree to -0.099MPa, open the gelation inhibition component 105 to adjust the cold air temperature, so that 25°C low-temperature nitrogen flows around the outer wall of the primary tank body 1032, and flows into the primary tank body 1032 from the jet port 1054 to accelerate the diffusion of each component, and the prepared zirconium sol can be stably stored for 350 hours without gelation.

[0140] Open the secondary stratification stirring component 204 and set the speed of the secondary stratification stirring roller to 4700rpm, open the primary flow control valve 107 to allow the configured zirconium sol to flow into the secondary tank 2012, feed 150,000 molecular weight polyvinyl alcohol into the secondary tank 2012 through the secondary feeding port 2011, turn on the ultrasonic component 22 and the bubble removal component 203 so that the output frequency is 130kHz, so that the polymer is fully dissolved in the sol.

[0141] Open the secondary flow control valve 205 to allow the mixed liquid to flow into the tertiary tank 305, open the tertiary stratification stirring assembly 301 and set the rotation speed of the tertiary stratification stirring roller to 4500rpm, turn on the negative pressure suction assembly 302, set the pressure of the suction pump to 5MPa, remove a large amount of solvent and discharge it, and turn on the inorganic component content monitor 303.

[0142] Step 2: The spinning solution is sequentially flowed into the ultrafine fiber spinneret 4021, the thickness compensation spinneret 4022 and the low-curvature liquid surface multi-jet nozzle 401 through the liquid delivery pipe 15. The inner diameters of the upper and lower ends of the flow channel in the nozzle are 3 mm, the inner diameter of the middle of the flow channel is 0.8 mm, the angle between the lower end flow channel and the extension line of the middle of the flow channel is 55°, and the nozzle length is 40 mm. The height of the conductive wire 4012 is 45 mm, the angle between the low-curvature liquid surface and the nozzle is 15°, and the number of single nozzle jets is 30. The length of the ultrafine fiber spinneret 4021 is 320 cm, the length of the thickness compensating spinneret 4022 is 100 cm, the height of the spinnerets is 8 cm, the number of nozzles on the ultrafine fiber spinneret 4021 is 80, the nozzle spacing is 35 mm, the number of nozzles on the thickness compensating spinneret 4022 is 20, the nozzle spacing is 45 mm, among which there are 10 liquid-discharging nozzles and 10 non-liquid-discharging nozzles.

[0143] The conveying roller, the ultrafine fiber spinneret 4021 and the thickness compensation spinneret 4022 move along their axes, i.e. in different directions. The spinneret movement speed is 0.45 m / min, the conveying roller movement speed is 0.3 m / min, the temperature and humidity control device 5 is turned on, and the relative ambient humidity of the spinning area is adjusted to 40%, the nozzle area temperature is 20°C, and the receiving area temperature is 26°C.

[0144] The solvent vapor rapid removal device 6 is turned on to remove the solvent in the spinning zone, so that the jet is deposited evenly and stably. The number of the static-eliminating voltage rollers 703 is 6.

[0145] Step 3: Send the hybrid fiber membrane into the low-temperature calcination system, turn on the multi-temperature zone temperature control device 8, set the temperature of the drying zone 9 to 200°C, the temperature of the microwave pretreatment zone 10 to 450°C, the temperature of the polymer removal zone 11 to 550°C, the temperature of the oxygen-deficient atmosphere heat treatment zone 12 to 800°C, the oxygen concentration is less than 20%, the temperature of the cooling zone 13 to 200°C, the frequency of the microwave generator 1001 to 250000MHz, and the hybrid fiber membrane after cooling is rolled up and packaged to finally obtain a flexible zirconium dioxide fiber membrane with a production capacity of 36m 2 / h.

[0146] Embodiment 4:

[0147] Based on the continuous macro-scale preparation device of a flexible and elastic ceramic ultrafine fiber material in Example 1, this embodiment provides a continuous macro-scale preparation method of a flexible and elastic ceramic ultrafine fiber flake material, comprising the following steps:

[0148] The first step: open the primary layered stirring component 106, set the rotation speed of the primary layered stirring roller to 5000rpm, feed 5kg of aluminum isopropoxide, 2kg of aluminum oxide, 2.5kg of tetraethoxysilane, 3kg of deionized water, 10kg of ethanol, and 30g of oxalic acid into the primary tank 1032 from the primary feeding port 1031 at one time, open the in-situ infrared analyzer 101 to detect the hydrolysis-polycondensation reaction rate of the alcohol salt, open the viscosity detector 102 to detect the sol state in real time, open the vacuum concentration component 104 to set the vacuum degree to -0.075MPa, open the gelation inhibition component 105 to adjust the cold air temperature, so that 16°C low-temperature neon gas flows around the outer wall of the primary tank 1032, and flows into the primary tank 1032 from the air jet 1054 to accelerate the diffusion of each component, and the prepared mullite sol can be stably stored for 450 hours without gelation.

[0149] Open the secondary stratification stirring component 204 and set the rotation speed of the secondary stratification stirring roller to 4500rpm, open the primary flow control valve 107 to allow the configured mullite sol to flow into the secondary tank 2012, feed 40,000 molecular weight polyethylene oxide into the secondary tank 2012 through the secondary feeding port 2011, turn on the ultrasonic component 22 and the bubble removal component 203 so that the output frequency is 100kHz, so that the polymer is fully dissolved in the sol.

[0150] Open the secondary flow control valve 205 to allow the mixed liquid to flow into the tertiary tank 305, open the tertiary stratification stirring assembly 301 and set the rotation speed of the tertiary stratification stirring roller to 4000rpm, turn on the negative pressure suction assembly 302, set the pressure of the suction pump to 5MPa, and remove a large amount of solvent and discharge it.

[0151] Step 2: The spinning solution is made to flow into the ultrafine fiber spinneret 4021, the thickness compensation spinneret 4022 and the low-curvature liquid surface multi-jet nozzle 401 in sequence through the liquid delivery pipe 15. The inner diameters of the upper and lower ends of the flow channel in the nozzle are 2.8 mm, the inner diameter of the middle of the flow channel is 0.6 mm, the angle between the lower end flow channel and the extension line of the middle of the flow channel is 90°, the nozzle length is 47 mm, the height of the conductive wire 4012 is 40 mm, and the angle between the low-curvature liquid surface and the nozzle is 20°. The number of single nozzle jets is 27. The length of the ultrafine fiber spinneret 4021 is 240 cm, the length of the thickness compensation spinneret 4022 is 85 cm, the spinneret height is 7 cm, the number of nozzles on the ultrafine fiber spinneret 4021 is 80, and the nozzle spacing is 25 mm. The number of nozzles on the thickness compensation spinneret 4022 is 20, and the nozzle spacing is 40 mm, of which there are 10 liquid-discharging nozzles and 10 non-liquid-discharging nozzles.

[0152] The conveying roller, the ultrafine fiber spinneret 4021 and the thickness compensation spinneret 4022 move along their axes, i.e. in different directions. The spinneret movement speed is 0.45 m / min, the conveying roller movement speed is 0.35 m / min, the temperature and humidity precision control device 5 is turned on, and the relative ambient humidity of the spinning area is adjusted to 42%, the nozzle area temperature is 19°C, and the receiving area temperature is 40°C.

[0153] The solvent vapor rapid removal device 6 is turned on to remove the solvent in the spinning zone, so that the jet is deposited evenly and stably. The number of the static-eliminating voltage rollers 703 is 5.

[0154] Step 3: The hybrid fiber flakes are sent into the low-temperature calcination system, the multi-temperature zone temperature control device 8 is turned on, the temperature of the drying zone 9 is set to 200°C, the temperature of the microwave pretreatment zone 10 is set to 450°C, the temperature of the polymer removal zone 11 is set to 600°C, the temperature of the oxygen-deficient atmosphere heat treatment zone 12 is 1200°C, the oxygen concentration is less than 20%, the temperature of the cooling zone 13 is 180°C, the frequency of the microwave generator 1001 is set to 200000MHz, the hybrid fiber flakes after cooling are rolled and packaged, and finally flexible mullite fiber flakes are obtained, with a production capacity of 42m 2 / h.

[0155] Embodiment 5:

[0156] Based on the continuous macro-scale preparation device of a flexible and elastic ceramic ultrafine fiber material in Example 1, this embodiment provides a continuous macro-scale preparation method of a flexible and elastic ceramic ultrafine fiber flake material, comprising the following steps:

[0157] The first step: open the primary layered stirring component 106, set the rotation speed of the primary layered stirring roller to 4900rpm, feed 9kg of isopropyl titanate, 0.45kg of deionized water, 1kg of ethanol, and 7.5kg of acetic acid into the primary tank body 1032 from the primary feeding port 1031 at one time, open the in-situ infrared analyzer 101 to detect the hydrolysis-polycondensation reaction rate of the alcohol salt, open the viscosity detector 102 to detect the sol state in real time, open the vacuum concentration component 104 to set the vacuum degree to -0.08MPa, open the gelation inhibition component 105 to allow 22°C low-temperature argon gas to flow around the outer wall of the primary tank body 1032, and flow into the primary tank body 1032 from the jet port 1054 to accelerate the diffusion of each component, and the prepared titanium sol can be stably stored for 400 hours without gelation.

[0158] Open the secondary stratification stirring component 204 and set the rotation speed of the secondary stratification stirring roller to 5000 rpm, open the primary flow control valve 107 to allow the configured titanium sol to flow into the secondary tank body 2012, feed 90,000 molecular weight polyvinyl pyrrolidone into the secondary tank body 2012 through the secondary feeding port 2011, turn on the ultrasonic component 22 and the bubble removal component 203 so that the output frequency is 110 kHz, so that the polymer is fully dissolved in the sol.

[0159] Open the secondary flow control valve 205 to allow the mixed liquid to flow into the tertiary tank 305, open the tertiary stratification stirring assembly 301 and set the rotation speed of the tertiary stratification stirring roller to 5000rpm, turn on the negative pressure suction assembly 302, set the pressure of the suction pump to 4MPa, and remove a large amount of solvent and discharge it.

[0160] Step 2: Make the spinning liquid flow into the ultrafine fiber spinneret 4021, the thickness compensation spinneret 4022 and the low-curvature liquid surface multi-jet nozzle 401 in sequence through the liquid delivery pipe 15. The inner diameters of the upper and lower ends of the flow channel in the nozzle are 4 mm, the inner diameter of the middle part of the flow channel is 0.9 mm, the angle between the lower end flow channel and the extension line of the middle part of the flow channel is 80°, and the nozzle length is 50 mm. The height of the conductive wire 4012 is 43 mm, the angle between the low-arc liquid surface and the nozzle is 25°, the number of single nozzle jets is 23, the length of the ultrafine fiber spinneret 4021 is 300 cm, the length of the thickness compensating spinneret 4022 is 115 cm, the height of the spinnerets is 6 cm, the number of nozzles on the ultrafine fiber spinneret 4021 is 70, and the nozzle spacing is 40 mm, the number of nozzles on the thickness compensating spinneret 4022 is 25, and the nozzle spacing is 45 mm, of which 15 are liquid-discharging nozzles and 10 are non-liquid-discharging nozzles.

[0161] The conveying roller, the ultrafine fiber spinneret 4021 and the thickness compensation spinneret 4022 move along their axes, i.e. in different directions. The spinneret movement speed is 0.55 m / min, the conveying roller movement speed is 0.4 m / min, the temperature and humidity precision control device 5 is turned on, and the relative ambient humidity of the spinning area is adjusted to 40%, the nozzle area temperature is 23°C, and the receiving area temperature is 39°C.

[0162] The solvent vapor rapid removal device 6 is turned on to remove the solvent in the spinning zone, so that the jet is deposited evenly and stably. The number of the static-eliminating voltage rollers 703 is 7.

[0163] Step 3: The hybrid fiber flakes are sent into the low-temperature calcination system, the multi-temperature zone temperature control device 8 is turned on, the temperature of the drying zone 9 is set to 200°C, the temperature of the microwave pretreatment zone 10 is set to 400°C, the temperature of the polymer removal zone 11 is set to 570°C, the temperature of the oxygen-deficient atmosphere heat treatment zone 12 is 1000°C, the oxygen concentration is less than 20%, the temperature of the cooling zone 13 is 160°C, the microwave generator frequency 1001 is set to 300000MHz, the hybrid fiber flakes after cooling are rolled and packaged, and finally flexible titanium dioxide fiber flakes are obtained, with a production capacity of 48m 2 / h.

[0164] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A continuous and large-scale preparation device for flexible and elastic ceramic ultrafine fiber materials, characterized in that: It includes feeding and liquid preparation system, multi-jet uniform electrospinning system, low-temperature calcination system and winding system. The feeding and liquid preparation system comprises a mixing device (1), a polymer mixing device (2), and an inorganic component content control device (3) which are sequentially connected in series via a liquid delivery pipeline (15); The multi-jet uniform electrospinning system comprises a temperature and humidity control device (5), a multi-jet electrospinning module (4) and a solvent vapor removal device (6) electrically connected to the temperature and humidity control device (5) and connected to the inorganic component content control device (3), and a static elimination and insulation device (7) connected to the multi-jet electrospinning module (4); The low-temperature calcination system comprises a multi-zone temperature control device (8), a drying zone (9) which is sequentially connected to the multi-zone temperature control device (8) and is independently separated, a microwave pretreatment zone (10), a polymer removal zone (11), an oxygen-deficient atmosphere heat treatment zone (12), and a temperature reduction zone (13).

2. The continuous large-scale preparation device of a flexible and elastic ceramic ultrafine fiber material according to claim 1 is characterized in that: The mixing device (1) comprises a primary tank body (1032), an in-situ infrared analyzer (101) arranged on the primary tank body (1032), a viscosity detector (102), a primary feeding port (1031), a vacuum concentration component (104), a gelation inhibition component (105) wrapped around the primary tank body (1032) and the bottom, a primary layering stirring component (106) arranged in the primary tank body (1032), and a primary flow control valve (107) arranged on the liquid delivery pipeline (15) at the outlet of the mixing device (1); The gelation suppression component (105) includes a cold air component (1051), a low-temperature pipe (1052) connected to the cold air component (1051) and surrounding the body and bottom of the first-level tank body (1032), and a thermal insulation layer (1053) arranged on the outside of the low-temperature pipe (1052); the low-temperature pipe (1052) is provided with a plurality of jet ports (1054) that penetrate the bottom of the first-level tank body (1032).

3. The continuous large-scale preparation device of a flexible and elastic ceramic ultrafine fiber material according to claim 2 is characterized in that: The polymer mixing device (2) comprises a secondary tank body (2012) connected to the primary tank body (1032), a secondary feeding port (2011) arranged on the secondary tank body (2012), an ultrasonic component (202), a bubble removal component (203), a secondary stratification stirring component (204) arranged in the secondary tank body (2012), and a secondary flow control valve (205) arranged on the liquid delivery pipe (15) at the outlet of the secondary tank body (2012).

4. The continuous large-scale preparation device of the flexible and elastic ceramic ultrafine fiber material according to claim 3 is characterized in that: The inorganic component content control device (3) includes a tertiary tank body (305) connected to the secondary tank body (2012), a negative pressure suction component (302) and an inorganic component content monitor (303) arranged on the tertiary tank body (305), a tertiary stratification stirring component (301) arranged in the tertiary tank body (305), and a tertiary flow control valve (304) arranged on the liquid delivery pipeline (15) at the outlet of the tertiary tank body (305).

5. The continuous large-scale preparation device of a flexible and elastic ceramic ultrafine fiber material according to claim 1 is characterized in that: The multi-jet electrospinning module (4) comprises a transmission component (4023), a plurality of spinnerets located above the transmission component (4023) and connected to the liquid delivery pipeline (15), and a plurality of low-curvature liquid surface multi-jet nozzles (401) arranged at the bottom of the spinnerets, wherein: The conveying assembly (4023) comprises a conveying roller and a conveying belt arranged on the conveying roller; The spinneret comprises a thickness compensating spinneret (4022) arranged along the conveying direction of the conveying roller, and a spinneret (4021) for ultrafine fibers vertically arranged between two adjacent thickness compensating spinnerets (4022), and the low-arc liquid surface multi-jet nozzle (401) is arranged at the bottom of the thickness compensating spinneret (4022) and the spinneret (4021) for ultrafine fibers.

6. The continuous large-scale preparation device of the flexible elastic ceramic ultrafine fiber material according to claim 5 is characterized in that: The low-curvature liquid surface multi-jet nozzles (401) are arranged in an array, and the low-curvature liquid surface multi-jet nozzles (401) include a dumbbell-shaped liquid outlet channel (4011) that is wider at the top and bottom and narrower in the middle, a cantilever rod (4013) arranged horizontally inside the dumbbell-shaped liquid outlet channel (4011), and a conductive wire (4012) vertically arranged on the cantilever rod (4013) and used for uniform electric field intensification; The temperature and humidity control device (5) comprises a microprocessor (502), a temperature and humidity detector (501) electrically connected to the microprocessor (502) and connected to the liquid delivery pipeline (15), a bidirectional temperature control pipeline (503) connected to the ultrafine fiber spinneret (4021), a humidifier (505), and a temperature control hollow plate (504) connected to the bidirectional temperature control pipeline (503) and located under the conveyor belt; The solvent vapor removal device (6) comprises a shell connected to a liquid delivery pipe (15), a main air suction pipe (601) arranged in the inner cavity of the shell, a secondary air suction pipe (602) located on the outer wall of the shell, and a gradient distribution honeycomb partition (603) arranged in the main air suction pipe (601) and the secondary air suction pipe (602) along the axial direction of the air suction pipe; The static electricity elimination and insulation device (7) comprises a nozzle insulation base (701) arranged between the spinneret and the low-curvature liquid surface multi-jet nozzle (401), an insulation plate (702) arranged at both ends of the bottom of the spinneret, a static electricity elimination roller (703) arranged on the conveyor belt, an inner insulation layer (704) and an outer insulation tube (705) arranged relatively inside and outside the low-curvature liquid surface multi-jet nozzle (401).

7. The continuous large-scale preparation device of flexible and elastic ceramic ultrafine fiber material according to claim 1 is characterized in that: The multi-temperature zone temperature control device (8) comprises a central processing unit (804), a temperature sensor (802) electrically connected to the central processing unit (804), an analog-to-digital converter (803), a heating element combination distributor (801), and a heating roller (805) disposed below the drying zone (9), the microwave pretreatment zone (10), the polymer removal zone (11), and the oxygen-deficient atmosphere heat treatment zone (12); The drying zone (9) is provided with a first heating element electrically connected to the multi-zone temperature control device (8); the microwave pretreatment zone (10) is provided with a microwave generator (1001), a microwave reflector (1003), a second heating element electrically connected to the multi-zone temperature control device (8), and a waveguide (1002) connected to the microwave generator (1001); the polymer removal zone (11) is provided with a third heating element electrically connected to the multi-zone temperature control device (8); the oxygen-deficient atmosphere heat treatment zone (12) is provided with an atmosphere concentration controller (1202), a fourth heating element electrically connected to the multi-zone temperature control device (8), and a dual-cavity supply device (1201) electrically connected to the atmosphere concentration controller (1202); and the cooling zone (13) is provided with a fifth heating element electrically connected to the multi-zone temperature control device (8).

8. The continuous large-scale preparation device of flexible elastic ceramic ultrafine fiber material according to claim 7 is characterized in that: The winding system comprises a winding support (1402) and a winding roller (1401) arranged on the winding support (1402).

9. A method for continuous and large-scale preparation of flexible and elastic ceramic ultrafine fiber materials, characterized in that: The continuous large-scale preparation device of the flexible elastic ceramic ultrafine fiber material according to any one of claims 1 to 8 comprises the following steps: S1, putting the raw materials into a mixing device (1) for mixing, low-temperature dispersion, vacuum concentration, and removing the solvent to obtain a sol; S2, the sol and polymer obtained in step S1 flow into the polymer mixing device (2) for mixing and degassing; S3, the mixed sol obtained in step S2 flows into the inorganic component content control device (3), and is sucked by negative pressure to obtain a spinning solution; S4, the spinning solution obtained in step S3 is flowed into a multi-jet electrospinning module (4), and the temperature, humidity, and multi-directional differential velocity during spinning are adjusted to obtain a fiber membrane material or a fiber flake material; S5, the fiber material obtained in step S4 is sequentially transferred to a drying zone (9), a microwave pretreatment zone (10), a polymer removal zone (11), an oxygen-deficient atmosphere heat treatment zone (12), and a cooling zone (13) for multi-temperature zone calcination to obtain a flexible and elastic ceramic ultrafine fiber material; S6. The flexible and elastic ceramic ultrafine fiber material obtained in step S5 is rolled up and packaged through a rolling system.

10. The continuous and large-scale preparation method of the flexible and elastic ceramic ultrafine fiber material according to claim 9, characterized in that: In step S1, inorganic salt, solvent and catalyst are put into the primary tank (1032), the primary layer stirring component (106) is turned on for stirring, and the in-situ infrared analyzer (101) and the viscosity detector (102) are turned on for monitoring respectively, the gelation inhibition component (105) is turned on to allow the low-temperature inert atmosphere to flow around the outer wall of the primary tank (1032) and flow into the primary tank (1032), and the vacuum concentration component (104) is turned on for vacuum concentration, wherein the inert atmosphere is selected from any one or more of nitrogen, helium, neon, argon, krypton or xenon, the temperature of the inert atmosphere is 5 to 25°C, and the vacuum degree range is: -0.01 to -0.1 MPa; In step S2, the sol and polymer obtained in step S1 are flowed into the secondary tank (2012), the secondary layered stirring component (204) is turned on for stirring, the ultrasonic component (202) is turned on to mix the sol and the polymer, and the bubble removal component (203) is turned on to remove bubbles during mixing, and the ultrasonic output frequency range of the ultrasonic component (202) is 20 to 130 kHz; In step S3, the mixed sol obtained in step S2 is flowed into the tertiary tank (305), and the tertiary layer stirring assembly (301) is turned on for mixing, and the negative pressure suction assembly (302) is turned on to make the inside of the tertiary tank (305) a low pressure or negative pressure state to remove the solvent, and the inorganic component content monitor (303) is turned on for monitoring; In step S4, the spinning solution obtained in step S3 is sprayed onto a conveyor belt through a low-curvature liquid surface multi-jet nozzle (401) of a spinneret for deposition and forming, the solvent vapor removal device (6) and the static elimination and insulation device (7) are turned on, the temperature and humidity control device (5) is turned on to adjust the temperature at the low-curvature liquid surface multi-jet nozzle (401) to 10-30° C., the temperature at the conveyor belt is adjusted to 20-50° C., the humidity of the spinning environment is 10-99%, the movement speed of the ultrafine fiber spinneret (4021) is 0.4-0.6 m / min, the movement speed of the thickness compensation spinneret (4022) is 0.4-0.6 m / min, and the conveying speed of the conveyor roller is 0.2-0.5 m / min; In step S5, the temperature of the drying zone (9) is 180-220°C, the temperature of the microwave pretreatment zone (10) is 350-450°C, the frequency is 300-300000 MHz, the temperature of the polymer removal zone (11) is 550-600°C, the temperature of the oxygen-deficient atmosphere heat treatment zone (12) is 700-1200°C, the oxygen concentration is less than 20%, the temperature of the cooling zone (13) is 160-200°C, and the heating temperature of the heating rod (805) is 20-1300°C.

Citation Information

Patent Citations

  • Multi-spraying-nozzle electrostatic spinning device with controllable spinning environment

    CN103409818A

  • Continuous production method of benzoin dimethyl ether and production device for method

    CN113461507A

  • Large-scale continuous manufacturing device for flexible ceramic nanofibers

    CN114369878A

  • Two-dimensional or three-dimensional oxide ceramic fiber and preparation method thereof

    CN117865648A

  • Reducing liquid mixing system

    CN218281418U

Cited By