Waste paper reinforcing complexing agent and preparation method thereof

Through the synergistic effect of bio-based polymer emulsion, lignin nanofibers and nanoinorganic fillers, a waste paper reinforcement composite agent was prepared, which solved the problem of insufficient strength and waterproofing performance of waste paper and achieved efficient waste paper reinforcement and environmentally friendly treatment meets higher demands in application scenarios and sustainable development needs.

CN119083234APending Publication Date: 2024-12-06ZHEJIANG FANGAO BIOTECHNOLOGY CO LTD

Patent Information

Application Number
CN202411279587.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Traditional waste paper recycling and treatment methods are difficult to effectively improve the strength and waterproof performance of waste paper, and there are environmental pollution problems, which cannot meet the higher demands of application scenarios and sustainable development needs.

Method used

By using the synergistic effects of bio-based polymer emulsion, lignin nanofibers, nanoinorganic filler composites, environmentally friendly waterproofing compound and degradable crosslinking agent, the strength of waste paper is significantly improved by preparing a waste paper reinforcement compound agent. and moisture-proof performance, and use environmentally friendly materials and processes to reduce environmental pollution.

Benefits of technology

It significantly improves the mechanical properties and moisture-proof properties of waste paper, extends the service life of paper products, and at the same time improves performance while reducing environmental pollution, meeting the requirements of sustainable development.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of waste paper recycling, and provides a waste paper reinforcing complexing agent which comprises the following components in parts by weight: 40-50 parts of bio-based polymer emulsion, 20-30 parts of lignin nanofibers, 15-25 parts of a nano inorganic filler compound, 10-15 parts of an environment-friendly waterproof agent compound and 8-12 parts of a degradable cross-linking agent. The diameter of the lignin nanofiber is 10-50nm, and the length of the lignin nanofiber is 1.5-2mu m. Through the synergistic effect of the bio-based polymer emulsion, the lignin nanofibers, the nano inorganic filler compound and other components, the strength of the waste paper is remarkably improved, a hydrophobic layer can be formed on the surface of the waste paper through the environment-friendly waterproof agent compound, the moisture resistance of the waste paper is effectively improved, the service life of a paper product is prolonged, and the environment-friendly waterproof agent compound is suitable for popularization and application. By adopting environment-friendly materials and processes, the environmental pollution can be reduced while the performance of the waste paper reinforcing complexing agent in various aspects can be improved, and the sustainable development is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waste paper recycling, in particular to a waste paper reinforcing composite agent and a preparation method thereof. Background Art

[0002] With the development of the global economy and the improvement of people's living standards, the consumption of paper is increasing. At the same time, the overexploitation of forest resources and the increasingly severe environmental problems have made people's demand for sustainable development more and more urgent. In this context, waste paper recycling has emerged as an important way of resource recycling.

[0003] Traditional waste paper recycling methods often fail to effectively improve the strength and moisture resistance of waste paper. Commonly used enhancers have limited effects and cannot meet higher-demand application scenarios. At the same time, existing waterproofing methods have problems such as lack of long-lasting waterproofing effects and impact on paper performance. In addition, the materials and processes used in traditional waste paper processing may cause significant pollution to the environment and do not meet the requirements of sustainable development. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a waste paper reinforcing composite agent and a preparation method thereof, which solves the problems of limited strength improvement, poor waterproof effect and environmental pollution in the existing waste paper treatment methods.

[0005] To achieve the above objectives, the present invention is implemented through the following technical scheme: a waste paper reinforcement composite agent and a preparation method thereof, comprising the following components in parts by weight: 40-50 parts of a bio-based polymer emulsion, 20-30 parts of lignin nanofibers, 15-25 parts of a nano-inorganic filler composite, 10-15 parts of an environmentally friendly waterproofing agent composite and 8-12 parts of a degradable cross-linking agent.

[0006] Preferably, the bio-based polymer emulsion is selected from one or more of acrylic emulsion and polyurethane emulsion.

[0007] Preferably, the lignin nanofibers have a diameter of 10-50 nm and a length of 1.5-2 μm.

[0008] Preferably, the nano inorganic filler composite is prepared by mixing nano silicon dioxide, nano aluminum hydroxide and nano montmorillonite in a ratio of 6:5:4.

[0009] Preferably, the environmentally friendly waterproofing agent composite is prepared by mixing beeswax, γ-aminopropyltriethoxysilane and tea tree essential oil in a ratio of 4:3:2.

[0010] Preferably, the degradable cross-linking agent is selected from one of tributyl citrate, polylactic acid diglycidyl ether or epoxidized soybean oil.

[0011] Preferably, a method for preparing a waste paper reinforcing composite agent comprises the following steps: S1. Add the bio-based polymer emulsion to the reactor and stir at a temperature of 45-55 ° C at a stirring speed of 150-200 rpm for 20-30 minutes to make it fully uniform; S2. Slowly add lignin nanofibers to the reactor and stir at a temperature of 55-65°C at a stirring speed of 200-250 rpm for 40-50 minutes to ensure that the lignin nanofibers are evenly dispersed in the emulsion; S3. The nano-inorganic filler composite was added to the reactor and stirred at a temperature of 60-70 ° C at a stirring speed of 180-220 rpm for 30-40 minutes to fully mix the nano-inorganic filler with other components; S4. After the components of the environmentally friendly waterproofing agent composite are uniformly mixed in proportion, they are slowly added to the reactor and stirred at a temperature of 65-75 ° C in the range of 150-180 rpm for 30-40 minutes; S5. Finally, a degradable cross-linking agent is added, and the mixture is stirred at a temperature of 60-70° C. at a stirring speed of 120-150 rpm for 20-30 minutes, and cooled to room temperature to obtain a waste paper reinforcement composite.

[0012] Preferably, during the preparation process of S1-S5, the reactor should be kept under a nitrogen atmosphere to prevent the components from being oxidized and ensure the stable performance of the composite agent.

[0013] Preferably, in S3, ultrasound is used to assist in dispersing the nano-inorganic filler composite before adding the nano-inorganic filler composite.

[0014] The present invention provides a waste paper reinforcing composite agent and a preparation method thereof, which has the following beneficial effects: 1. The present invention significantly improves the strength of waste paper through the synergistic effect of components such as bio-based polymer emulsion, lignin nanofibers and nano-inorganic filler composites. The lignin nanofibers can be intertwined and entangled with waste paper fibers to form a complex three-dimensional network structure, thereby enhancing the mechanical properties of waste paper. Combined with the adsorption and reinforcement effects of the nano-inorganic filler composite, the stability and strength of the composite can be further improved.

[0015] 2. The environmentally friendly waterproofing agent compound of the present invention is prepared by mixing beeswax, γ-aminopropyltriethoxysilane and tea tree essential oil in proportion, which can form a hydrophobic layer on the surface of waste paper, effectively improve the moisture-proof performance of the waste paper, and extend the service life of paper products.

[0016] 3. The present invention adopts environmentally friendly materials and processes, which can improve the performance of waste paper reinforcement composite agents in various aspects while reducing pollution to the environment, which is conducive to sustainable development. DETAILED DESCRIPTION

[0017] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0018] Embodiment 1: The embodiment of the present invention provides a waste paper reinforcement composite agent, comprising the following components in parts by weight: 45 parts of bio-based polymer emulsion, 25 parts of lignin nanofibers, 20 parts of nano inorganic filler composite, 12 parts of environmentally friendly waterproofing agent composite and 10 parts of degradable cross-linking agent.

[0019] The bio-based polymer emulsion is acrylic emulsion, which has good adhesion and flexibility and can effectively enhance the strength of waste paper.

[0020] The diameter of lignin nanofibers is 20-30nm and the length is 1.6-1.8μm. The lignin nanofibers are specifically prepared from straw by a chemical mechanical method. The preparation steps are: first, the raw materials are crushed and screened to obtain relatively pure lignin raw materials; the lignin raw materials are immersed in a sodium hydroxide solution and reacted at 60°C for 30 minutes to degrade the macromolecular structure of the lignin, making it easier to mechanically process, while improving the reaction activity and processability of the lignin; grinding to obtain lignin slurry, pressurizing the lignin slurry through a high-pressure pump, and passing it at high speed in a narrow gap to generate strong shear force and impact force, so that the lignin fibers are gradually refined and separated to form nanometer-scale fibers. When mixed with waste paper fibers, these nanofibers can be intertwined and entangled with each other to form a complex three-dimensional network structure, thereby enhancing the mechanical properties of the waste paper and improving its strength.

[0021] The nano inorganic filler composite material is prepared by mixing nano silicon dioxide, nano aluminum hydroxide and nano montmorillonite in a ratio of 6:5:4, has adsorption and reinforcing effects, and can improve the stability and strength of the composite agent.

[0022] The environmentally friendly waterproofing agent composite is prepared by mixing beeswax, γ-aminopropyltriethoxysilane and tea tree essential oil in a ratio of 4:3:2. It can form a hydrophobic layer on the surface of waste paper and effectively improve the moisture-proof performance of the waste paper.

[0023] The degradable cross-linking agent is tributyl citrate, which can promote the cross-linking reaction between the components, improve the performance and stability of the composite agent, and is degradable in the natural environment, meeting environmental protection requirements.

[0024] A method for preparing a waste paper reinforcing composite agent comprises the following steps: S1: Add the acrylic emulsion into the reaction kettle, stir at 50°C and 180 rpm for 25 minutes to make it fully uniform; S2: slowly add lignin nanofibers into the reactor, stir at 60°C and 220 rpm for 45 minutes to ensure that the lignin nanofibers are evenly dispersed in the emulsion; S3: Before adding the nano-inorganic filler composite, ultrasonic-assisted dispersion of the nano-inorganic filler composite can effectively break up the agglomeration of the nano-filler and make it evenly dispersed in the system, which is beneficial to improving the interfacial bonding force and enhancing the overall performance of the waste paper reinforcement composite. Then, the nano-inorganic filler composite is added to the reactor and stirred at a temperature of 65°C and a stirring speed of 200 rpm for 35 minutes to fully mix the nano-inorganic filler with other components.

[0025] S4: After mixing the components of the environmentally friendly waterproofing agent composite uniformly according to a certain proportion, slowly add them into the reaction kettle, and stir them at a temperature of 70° C. and a stirring speed of 160 rpm for 35 minutes.

[0026] S5: Finally, tributyl citrate was added, and the mixture was stirred at 65° C. and 130 rpm for 25 minutes. After cooling to room temperature, the waste paper reinforcing composite agent was obtained. During the entire preparation process, the reactor was kept under a nitrogen atmosphere.

[0027] Embodiment 2: The embodiment of the present invention provides a waste paper reinforcement composite agent, comprising the following components in parts by weight: bio-based polymer emulsion: 40 parts of polyurethane emulsion, lignin nanofiber: 30-40nm in diameter and 1.7-1.9μm in length, 22 parts, nano inorganic filler composite: 18 parts of nano silicon dioxide, nano aluminum hydroxide and nano montmorillonite mixed in a ratio of 6:5:4, an environmentally friendly waterproofing agent composite: 10 parts of beeswax, γ-aminopropyl triethoxysilane and tea tree essential oil mixed in a ratio of 4:3:2, a degradable cross-linking agent: 8 parts of polylactic acid diglycidyl ether, wherein the raw material for preparing the lignin nanofiber is waste wood, and the preparation method refers to Example 1.

[0028] A method for preparing a waste paper reinforcing composite agent comprises the following steps: S1: Add the polyurethane emulsion into the reaction kettle, stir at 45°C and 160 rpm for 20 minutes to make it fully uniform; S2: slowly add lignin nanofibers into the reactor, stir at 200 rpm for 40 minutes at 55°C to ensure that the lignin nanofibers are evenly dispersed in the emulsion; S3: before adding the nano inorganic filler composite, the nano inorganic filler composite is dispersed by ultrasonic assistance, and then the nano inorganic filler composite is added into the reaction kettle, and stirred at a temperature of 60° C. and a stirring speed of 180 rpm for 30 minutes to fully mix the nano inorganic filler with other components; S4: After mixing the components of the environmentally friendly waterproofing agent composite uniformly according to a certain proportion, slowly add the mixture into the reaction kettle, and stir at a temperature of 65° C. and a stirring speed of 150 rpm for 30 minutes; S5: Finally, polylactic acid diglycidyl ether was added, and the mixture was stirred at 60° C. and 120 rpm for 20 minutes. After cooling to room temperature, the waste paper reinforcing composite was obtained. During the entire preparation process, the reactor was kept under a nitrogen atmosphere.

[0029] Embodiment three: The embodiment of the present invention provides a waste paper strengthening composite agent, comprising the following components in parts by weight: Bio-based polymer emulsion: a mixed emulsion of 25 parts of acrylic emulsion and 25 parts of polyurethane emulsion, lignin nanofiber: 30 parts with a diameter of 40-50nm and a length of 1.8-2μm, nano-inorganic filler composite: 25 parts of nano-silicon dioxide, nano-aluminum hydroxide and nano-montmorillonite mixed in a ratio of 6:5:4, environmentally friendly waterproofing agent composite: 15 parts of beeswax, γ-aminopropyltriethoxysilane and tea tree essential oil mixed in a ratio of 4:3:2, degradable cross-linking agent: 12 parts of epoxidized soybean oil, wherein the raw material for preparing the lignin nanofiber is waste wood, and the preparation method refers to Example 1.

[0030] A method for preparing a waste paper reinforcing composite agent comprises the following steps: S1: Add the mixed emulsion of acrylic emulsion and polyurethane emulsion into a reaction kettle, and stir at a temperature of 55° C. and a stirring speed of 200 rpm for 30 minutes to make it fully uniform; S2: slowly add lignin nanofibers into the reactor, stir at 65°C and 250 rpm for 50 minutes to ensure that the lignin nanofibers are evenly dispersed in the emulsion; S3: before adding the nano inorganic filler composite, the nano inorganic filler composite is dispersed by ultrasonic assistance, and then the nano inorganic filler composite is added into the reaction kettle, and stirred at a temperature of 70° C. and a stirring speed of 220 rpm for 40 minutes to fully mix the nano inorganic filler with other components; S4: After mixing the components of the environmentally friendly waterproofing agent composite uniformly according to a certain proportion, slowly add them into the reaction kettle, and stir at a temperature of 75° C. and a stirring speed of 180 rpm for 40 minutes; S5: Finally, epoxidized soybean oil was added, and the mixture was stirred at 70° C. and 150 rpm for 30 minutes. After cooling to room temperature, the waste paper reinforcing composite was obtained. During the entire preparation process, the reactor was kept under a nitrogen atmosphere.

[0031] Comparative Example 1: Composition: 45 parts of ordinary polymer emulsion, 20 parts of nano silicon dioxide, 12 parts of ordinary waterproofing agent, and 10 parts of conventional cross-linking agent.

[0032] Preparation method: S1: Add the common polymer emulsion into the reaction kettle and stir at a temperature of 50°C and a stirring speed of 180 rpm for 25 minutes; S2: Add nano-silicon dioxide into the reaction kettle and stir at a temperature of 65°C and a stirring speed of 200 rpm for 35 minutes; S3: Add a common waterproofing agent into the reaction kettle, and stir at a temperature of 70°C and a stirring speed of 160 rpm for 35 minutes; S4: Finally, add a conventional cross-linking agent, stir at 65° C. and 130 rpm for 25 minutes, and cool to room temperature.

[0033] Comparative Example 2: Ingredients: 30 parts of bio-based polymer emulsion (acrylate emulsion), 15 parts of lignin nanofibers (diameter 20-30nm, length 1.6-1.8μm), the preparation method refers to Example 1, 15 parts of nano-inorganic filler composite (nano-silicon dioxide, nano-aluminum hydroxide and nano-montmorillonite mixed in a ratio of 3:2:1), 8 parts of environmentally friendly waterproofing agent composite (beeswax, γ-aminopropyltriethoxysilane and tea tree essential oil mixed in a ratio of 3:2:1), 6 parts of degradable cross-linking agent (tributyl citrate).

[0034] Preparation method: S1: Add the acrylic emulsion into the reaction kettle and stir at a temperature of 45°C and a stirring speed of 150 rpm for 20 minutes; S2: slowly add lignin nanofibers into the reactor, and stir at 55°C and 200 rpm for 40 minutes; S3: adding the nano inorganic filler composite into the reaction kettle, stirring at a temperature of 60° C. and a stirring speed of 180 rpm for 30 minutes; S4: After mixing the components of the environmentally friendly waterproofing agent composite uniformly according to a certain proportion, slowly add them into the reaction kettle, and stir them at a temperature of 65° C. and a stirring speed of 150 rpm for 30 minutes.

[0035] S5: Finally, tributyl citrate was added, and the mixture was stirred at 60° C. and 120 rpm for 20 minutes, and then cooled to room temperature.

[0036] The tensile strength (unit: MPa), water absorption (unit: %) and degradation time (unit: month) of the above examples and comparative examples were tested, and the test results are shown in the following table: Tensile strength (MPa) Water absorption (%) Degradation time (months) Embodiment 1 25 3.0 6 Embodiment 2 22 4.0 8 Embodiment 3 24 3.5 7 Comparative Example 1 14 8.5 Non-degradable Comparative Example 2 16 7.0 12 Through the analysis of the components, preparation methods and national standard test results of the three embodiments and two comparative examples, it can be seen that the waste paper reinforcement composite using bio-based polymer emulsion, lignin nanofiber, a specific proportion of nano-inorganic filler composite, an environmentally friendly waterproofing agent composite and a degradable cross-linking agent has obvious advantages in strength performance, moisture-proof performance and environmental protection performance. Nano-scale lignin fiber, reasonable formula ratio and the use of degradable materials play a key role in improving the performance of the composite.

[0037] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A waste paper reinforcing compound, characterized in that: The invention comprises the following components in parts by weight: 40-50 parts of bio-based polymer emulsion, 20-30 parts of lignin nanofiber, 15-25 parts of nano inorganic filler compound, 10-15 parts of environment-friendly waterproofing agent compound and 8-12 parts of degradable cross-linking agent.

2. The waste paper reinforcing composite agent according to claim 1, characterized in that: The bio-based polymer emulsion is selected from one or more of acrylic emulsion and polyurethane emulsion.

3. The waste paper reinforcing composite agent according to claim 1, characterized in that: The lignin nanofiber has a diameter of 10-50 nm and a length of 1.5-2 μm.

4. The waste paper reinforcing composite agent according to claim 1, characterized in that: The nano inorganic filler composite is prepared by mixing nano silicon dioxide, nano aluminum hydroxide and nano montmorillonite in a ratio of 6:5:

4.

5. The waste paper reinforcing composite agent according to claim 1, characterized in that: The environmentally friendly waterproofing agent compound is prepared by mixing beeswax, gamma-aminopropyl triethoxysilane and tea tree essential oil in a ratio of 4:3:

2.

6. The waste paper strengthening composite agent according to claim 1, characterized in that: The degradable cross-linking agent is selected from one of tributyl citrate, polylactic acid diglycidyl ether or epoxidized soybean oil.

7. A method for preparing a waste paper reinforcing composite agent, using the waste paper reinforcing composite agent as claimed in any one of claims 1 to 6, characterized in that: The following steps are involved: S1. Add the bio-based polymer emulsion to the reactor and stir at a temperature of 45-55 ° C at a stirring speed of 150-200 rpm for 20-30 minutes to make it fully uniform; S2. Slowly add lignin nanofibers to the reactor and stir at a temperature of 55-65°C at a stirring speed of 200-250 rpm for 40-50 minutes to ensure that the lignin nanofibers are evenly dispersed in the emulsion; S3. The nano-inorganic filler composite was added to the reactor and stirred at a temperature of 60-70 ° C at a stirring speed of 180-220 rpm for 30-40 minutes to fully mix the nano-inorganic filler with other components; S4. After the components of the environmentally friendly waterproofing agent composite are uniformly mixed in proportion, they are slowly added to the reactor and stirred at a temperature of 65-75 ° C in the range of 150-180 rpm for 30-40 minutes; S5. Finally, a degradable cross-linking agent is added, and the mixture is stirred at a temperature of 60-70° C. at a stirring speed of 120-150 rpm for 20-30 minutes, and cooled to room temperature to obtain a waste paper reinforcement composite.

8. The method for preparing a waste paper reinforcing composite agent according to claim 7, characterized in that: During the preparation of S1-S5, the reactor should be kept under a nitrogen atmosphere to prevent the components from being oxidized and ensure the stability of the performance of the composite.

9. The method for preparing a waste paper reinforcing composite agent according to claim 7, characterized in that: In S3, ultrasonic wave is used to assist in dispersing the nano inorganic filler composite before adding the nano inorganic filler composite.

Citation Information

Patent Citations

  • Corrugating base paper

    CN106676945A

  • Modified composite fiber material as well as preparation method and application thereof

    CN110158348A

Cited By

  • Production process of recycled waste paper papermaking board

    CN120158948A