Composite conductive film and preparation method thereof

By treating the base layer and plating surface of the composite conductive film to form a rough surface and preparing the plating layer on these surfaces, the problem of insufficient binding force of the composite conductive film is solved, the tensile strength and elongation of break are improved, and the use of the battery is extended Lifespan and reduce battery internal resistance.

CN119132701APending Publication Date: 2024-12-13ANHUI JIMAT NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411250852.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-12-13

AI Technical Summary

Technical Problem

The bonding force between the base film and the coating of the existing composite conductive film is limited, resulting in low overall tensile strength and easy to be torn off under external tension, reducing the elongation of breakage.

Method used

By treating the surfaces of the base layer and the first plating layer, a rough first concave and convex surface and a second concave and convex surface are formed to improve surface adhesion, and a magnetron sputtering method or vacuum evaporation method is used to prepare the following surfaces. The second plating layer enhances the bonding force between the base layer and the first plating layer and the first plating layer and the second plating layer.

Benefits of technology

It improves the overall tensile strength of the composite conductive film, avoids being torn off under external tension, extends the service life of the battery, reduces the internal resistance of the battery, and improves the performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119132701A_ABST
    Figure CN119132701A_ABST
Patent Text Reader

Abstract

The invention discloses a composite conductive film and a preparation method thereof. The composite conductive film comprises a substrate layer, a first plating layer and a second plating layer. In the first direction, the base layer comprises a first surface and a second surface opposite to the first surface, at least one of the first surface and the second surface is provided with a first concave-convex surface, and the first concave-convex surface is at least used for improving the surface adhesive force of the base layer; the first plating layers are arranged on the first surface and the second surface respectively, at least one of the surface, deviating from the substrate layer, of the first plating layer located on the first surface and the surface, deviating from the substrate layer, of the first plating layer located on the second surface is provided with a second concave-convex surface, and the second concave-convex surface is at least used for improving the surface adhesive force of the first plating layers; the second coating is arranged on the surface, away from the substrate layer, of the first coating. The problem of low overall tensile strength of the composite conductive film in the prior art can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of thin film preparation, and in particular to a composite conductive film and a preparation method thereof. Background Art

[0002] Conductive film refers to a thin film with conductive function. Due to its light weight, it has high practical application value and can be used in many places, such as in lithium-ion batteries.

[0003] At present, the composite conductive film includes a base film and coatings deposited on two surfaces of the base film, wherein the coatings may be a multi-layer structure. However, the bonding force between the base film and the coating, and between the coatings of the existing composite conductive film is limited. During the preparation process, the base film and the coating, and between the coatings, are easily separated, thereby reducing the overall tensile strength of the composite conductive film. When an external tensile force is applied to the composite conductive film, the composite conductive film is easily torn, which reduces the elongation at break of the composite conductive film to a certain extent. Summary of the invention

[0004] The main purpose of the present invention is to provide a composite conductive film and a preparation method thereof, so as to solve the problem of low overall tensile strength of the composite conductive film in the prior art.

[0005] According to one aspect of the present invention, there is provided a composite conductive film, comprising:

[0006] A base layer, along a first direction, the base layer comprises a first surface and a second surface opposite to the first surface, at least one of the first surface and the second surface has a first concavo-convex surface, and the first concavo-convex surface is at least used to improve the surface adhesion of the base layer;

[0007] A first coating, wherein the first coating is disposed on the first surface and the second surface respectively, and at least one of a surface of the first coating located on the first surface away from the base layer and a surface of the first coating located on the second surface away from the base layer has a second concavo-convex surface, and the second concavo-convex surface is at least used to improve the surface adhesion of the first coating;

[0008] A second plating layer is disposed on a surface of the first plating layer facing away from the base layer.

[0009] Furthermore, the second coating layer has a surface square resistance, and the square resistance change rate ρ of the surface square resistance satisfies the relationship: ρ<5×10 -2 .

[0010] Further, the roughness of the first concavo-convex surface is 0.18 μm to 0.22 μm; and / or,

[0011] The second concavo-convex surface has a roughness of 0.18 μm to 0.22 μm.

[0012] Furthermore, the first coating is a metal coating made of one or more of copper, aluminum, copper alloy, aluminum alloy, nickel alloy and titanium alloy; or,

[0013] The first coating is a non-metallic coating made of one or more of aluminum oxide and silicon nitride.

[0014] Further, along the first direction, the thickness of the metal plating layer is 10 nm to 1000 nm; or,

[0015] Along the first direction, the thickness of the non-metallic coating is 10 nm to 500 nm.

[0016] Furthermore, the second coating is made of one or more of copper, aluminum, copper alloy, aluminum alloy, nickel alloy and titanium alloy; and / or,

[0017] The base layer is made of one or more of polyethylene, polypropylene, ethylene-propylene copolymer, polyethylene terephthalate, polyethylene naphthalate, poly(p-phenylene terephthalamide), acrylonitrile-butadiene-styrene copolymer, poly(p-phenylene terephthalamide), polypropylene, polyoxymethylene, epoxy resin, phenolic resin, polytetrafluoroethylene, polyvinylidene fluoride, silicone rubber and polycarbonate.

[0018] Further, along the first direction, the thickness of the second coating layer is 10 nm to 1000 nm.

[0019] Further, along the first direction, the thickness of the base layer is 3 μm to 8 μm.

[0020] On the other hand, the present invention further provides a method for preparing a composite conductive film, the method for preparing a composite conductive film is used to prepare the above-mentioned composite conductive film, and the method for preparing a composite conductive film further comprises:

[0021] Step S1: preparing the base layer, and processing the first surface and / or the second surface of the base layer to obtain the first concave-convex surface, wherein the roughness of the first concave-convex surface is a first predetermined value;

[0022] Step S2: preparing the first coating on the first surface and the second surface, and processing the surface of the first coating on the first surface away from the base layer and / or the surface of the first coating on the second surface away from the base layer to obtain the second concave-convex surface, wherein the roughness of the second concave-convex surface is a second predetermined value;

[0023] Step S3: preparing the second coating layer on the surface of the first coating layer away from the base layer.

[0024] Further, in the step S1, the first surface and / or the second surface is treated by plasma treatment or corona treatment so that the first predetermined value is 0.18 μm to 0.22 μm, and the base layer is prepared by casting, extrusion or blow molding;

[0025] In the step S2, a plasma treatment method or a corona treatment method is used for the surface of the first coating layer facing away from the base layer so that the second predetermined value is 0.18 μm to 0.22 μm, and a magnetron sputtering method or a vacuum evaporation method or an ion plating method is used to prepare the first coating layer on the first surface and the second surface;

[0026] In the step S3, the second coating layer is prepared on the surface of the first coating layer away from the base layer by using magnetron sputtering, vacuum evaporation or ion plating.

[0027] Compared with the structure of the composite conductive film in the prior art, the present invention processes the surface of the base layer and the surface of the first coating so that the surface of the base layer and the surface of the first coating become rough and uneven. The roughness can effectively improve the adhesion of the surface of the base layer and the surface of the first coating, thereby improving the bonding strength between the base layer and the first coating, and between the first coating and the second coating, and then improving the overall tensile strength of the composite conductive film. When external tensile force is applied to the composite conductive film, the composite conductive film is not easily torn apart, thereby improving the elongation at break of the composite conductive film. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0029] Figure 1 A schematic diagram of the structure of a composite conductive film disclosed in an embodiment of the present invention;

[0030] Figure 2 The present invention is a flow chart of a method for preparing a composite conductive film disclosed in an embodiment of the present invention.

[0031] The above drawings include the following reference numerals:

[0032] 10. Base layer; 101. First surface; 102. Second surface; 20. First coating layer; 30. Second coating layer; 40. First concavo-convex surface; 50. Second concavo-convex surface. DETAILED DESCRIPTION

[0033] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0034] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0035] Unless otherwise specifically stated, the relative arrangement of the parts and steps described in these embodiments, numerical expressions and numerical values ​​do not limit the scope of the present invention. At the same time, it should be understood that, for ease of description, the sizes of the various parts shown in the accompanying drawings are not drawn according to the actual proportional relationship. The technology, methods and equipment known to ordinary technicians in the relevant field may not be discussed in detail, but in appropriate cases, the technology, methods and equipment should be regarded as a part of the authorization specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, so once a certain item is defined in an accompanying drawing, it does not need to be further discussed in subsequent drawings.

[0036] As mentioned in the background technology, the bonding force between the base film and the coating layer, and between the coating layers in the existing composite conductive film is limited, and separation is easy to occur during the preparation process, resulting in a decrease in the overall tensile strength of the composite conductive film. When an external tensile force is applied to the composite conductive film, the composite conductive film is easily torn apart, which reduces the elongation at break of the composite conductive film to a certain extent. Therefore, in order to improve the overall tensile strength of the composite conductive film, the inventor of the present invention has designed a new type of composite conductive film, and the composite conductive film of the present invention will be described in detail below.

[0037] See also Figure 1 to Figure 2 As shown, the present invention provides a composite conductive film, which includes a base layer 10, a first coating layer 20 and a second coating layer 30. It should be noted that the first direction of the present invention is to attach Figure 1 The direction indicated by the letter X.

[0038] Among them, along the first direction, the base layer 10 includes a first surface 101 and a second surface 102 opposite to the first surface 101, at least one of the first surface 101 and the second surface 102 has a first concave-convex surface 40, and the first concave-convex surface 40 is at least used to improve the surface adhesion of the base layer 10; the first coating 20 is respectively arranged on the first surface 101 and the second surface 102, at least one of the surface of the first coating 20 located on the first surface 101 away from the base layer 10 and the surface of the first coating 20 located on the second surface 102 away from the base layer 10 has a second concave-convex surface 50, and the second concave-convex surface 50 is at least used to improve the surface adhesion of the first coating 20; the second coating 30 is arranged on the surface of the first coating 20 away from the base layer 10.

[0039] In this embodiment, the base layer 10 includes a first surface 101 and a second surface 102. When the composite conductive film is actually processed, the first surface 101 and / or the second surface 102 can be processed by a plasma treatment method or a corona treatment method to form a first concave-convex surface 40 on the first surface 101 and / or the second surface 102. The first concave-convex surface 40 makes the first surface 101 and / or the second surface 102 rough and uneven, and the surface adhesion of the base layer 10 can be effectively improved by the roughness; then the first coating layer 20 is sputtered or plated on the first surface 101 and the second surface 102 by magnetron sputtering or vacuum evaporation or ion plating. In this process, since the first surface 101 and / or the second surface 102 become rough and uneven, when the first coating layer 20 is plated, the first coating layer 20 is plated on the first surface 101 and the second surface 102. When sputtering or plating is performed, the bonding force between the first plating layer 20 and the base layer 10 can be improved; then, a plasma treatment method or a corona treatment method is used to treat the surface of the first plating layer 20 located on the first surface 101 away from the base layer 10 and / or the surface of the first plating layer 20 located on the second surface 102 away from the base layer 10 to form a second concave-convex surface 50, and the second concave-convex surface 50 makes the surface of the first plating layer 20 away from the base layer 10 rough and uneven, and the surface adhesion of the first plating layer 20 can be effectively improved by the roughness; finally, the second plating layer 30 is sputtered or plated on the surface of the first plating layer 20 away from the base layer 10 by magnetron sputtering or vacuum evaporation or ion plating. In this process, since the surface of the first plating layer 20 away from the base layer 10 becomes rough and uneven, when the second plating layer 30 is sputtered or plated on the surface of the first plating layer 20 away from the base layer 10, the bonding force between the first plating layer 20 and the second plating layer 30 can be improved.

[0040] That is to say, the first concavo-convex surface 40 of the present invention can be arranged only on the first surface 101, the first concavo-convex surface 40 can also be arranged only on the second surface 102, or the first concavo-convex surface 40 can also be arranged on the first surface 101 and the second surface 102. Figure 1The figure shows the situation when the first concavo-convex surface 40 is arranged on the first surface 101; the second concavo-convex surface 50 of the present invention can be arranged only on the surface of the first coating 20 located on the first surface 101 away from the base layer 10, and the second concavo-convex surface 50 can also be arranged only on the surface of the first coating 20 located on the second surface 102 away from the base layer 10, and the second concavo-convex surface 50 can also be arranged on the surface of the first coating 20 located on the first surface 101 away from the base layer 10, and on the surface of the first coating 20 located on the second surface 102 away from the base layer 10. The attached figure of this embodiment Figure 1 The case where the second concavo-convex surface 50 is provided on the surface of the first plating layer 20 located on the second surface 102 facing away from the base layer 10 is shown.

[0041] Compared with the structure of the composite conductive film in the prior art, this embodiment processes the surface of the base layer 10 and the surface of the first coating layer 20 so that the surface of the base layer 10 and the surface of the first coating layer 20 become rough and uneven. The roughness can effectively improve the adhesion of the surface of the base layer 10 and the surface of the first coating layer 20, thereby improving the bonding force between the base layer 10 and the first coating layer 20, and between the first coating layer 20 and the second coating layer 30, thereby improving the overall tensile strength of the composite conductive film. When an external tensile force is applied to the composite conductive film, the composite conductive film is not easily torn apart, thereby improving the elongation at break of the composite conductive film.

[0042] Furthermore, the second plating layer 30 in this embodiment has a surface square resistance, and the square resistance change rate ρ of the surface square resistance satisfies the relationship: ρ<5×10 -2 , for example 4×10 -2 4.1×10 -2 4.2×10 -2 , 4.3×10 -2 , 4.4×10 -2 , 4.5×10 -2 , 4.6×10 -2 , 4.7×10 -2 , 4.8×10 -2 , 4.9×10 -2 and less than 5×10 -2Any other value of . In this way, it can be ensured that the composite conductive film will not be damaged by the tensile force, the internal resistance of the battery can be effectively reduced, and the phenomenon of severe heating when the battery is working can be avoided to a certain extent, thereby improving the battery performance and extending the service life of the battery. In other words, compared with the structure of other composite conductive films, the composite conductive film provided in this embodiment can improve the bonding force between the base layer 10 and the first coating layer 20, and between the first coating layer 20 and the second coating layer 30, thereby improving the overall tensile strength of the composite conductive film, effectively ensuring the integrity of the composite conductive film, improving the elongation at break of the composite conductive film to a certain extent, and extending the service life of the battery.

[0043] As can be seen from Table 1, Table 1 shows the square resistance change rate of the second coating layer 30 in the composite conductive film when the composite conductive film is under a certain tensile force and the tensile deformation is within 10%. Among them, the base layer 10 in Examples 1 to 3 and Comparative Examples 1 to 3 is cut according to the specification of 20 cm in length and 5 cm in width, and a 6 μm base layer 10 is used, and a first coating layer 20 is sputtered or plated on the base layer 10 by magnetron sputtering, vacuum evaporation or ion plating, and the thickness of the first coating layer 20 is 30 nm, and then the second coating layer 30 is sputtered or plated on the surface of the first coating layer 20 by magnetron sputtering, vacuum evaporation or ion plating, and the thickness of the second coating layer 30 is 30 nm.

[0044] The difference between Examples 1 to 3 and Comparative Examples 1 to 3 is the setting of the roughness of the first concavo-convex surface 40 and the second concavo-convex surface 50. The results show that when the first surface 101 of the substrate 10 has the first concavo-convex surface 40, and the surface of the first coating 20 located on the second surface 102 away from the substrate 10 has the second concavo-convex surface 50, the square resistance change rate of the second coating 30 is within 5%. At this time, it can be ensured that the composite conductive film will not be damaged by the tensile force, effectively reduce the internal resistance of the battery, and avoid the phenomenon of severe heating when the battery is working to a certain extent; when only the first concavo-convex surface 40 is provided on the first surface 101 of the substrate 10, or only the second concavo-convex surface 50 is provided on the surface of the first coating 20 located on the second surface 102 away from the substrate 10, or the first concavo-convex surface 40 and the second concavo-convex surface 50 are not provided, the square resistance change rate of the second coating 30 is greater than 6%, at this time, it is easy to cause the internal resistance of the battery to increase, thereby causing safety problems when the battery is working.

[0045] It should be noted that the present invention uses the square resistance change rate ρ of the surface square resistance of the second coating layer 30 to represent the elongation at break of the composite conductive film of the present invention. When the square resistance change rate of the second coating layer 30 in this embodiment is less than 5%, it can ensure that the composite conductive film of this embodiment has a good elongation at break.

[0046] Table 1 Verification data of surface square resistance change rate of composite conductive film in the embodiment and comparative example

[0047]

[0048] Further, the roughness of the first concave-convex surface 40 in the present embodiment is 0.18 μm to 0.22 μm, for example, 0.18 μm, 0.19 μm, 0.20 μm, 0.21 μm, 0.22 μm and any value therebetween. When the roughness of the first concave-convex surface 40 is less than 0.18 μm, the surface of the base layer 10 will not have obvious concave-convex undulations, which reduces the bonding force between the first plating layer 20 and the base layer 10; when the roughness of the first concave-convex surface 40 is greater than 0.22 μm, the resistance of the composite conductive film is increased, thereby reducing the service life of the composite conductive film. Specifically, as shown in Table 2, when the roughness of the first concave-convex surface 40 set on the first surface 101 is 0.18 μm, 0.20 μm, and 0.22 μm, the bonding force between the base layer 10 and the first plating layer 20 is improved, effectively preventing the first plating layer 20 from separating from the base layer 10.

[0049] Further, in the present embodiment, the roughness of the second concave-convex surface 50 is 0.18 μm to 0.22 μm, for example, 0.18 μm, 0.19 μm, 0.20 μm, 0.21 μm, 0.22 μm and any value therebetween. When the roughness of the second concave-convex surface 50 is less than 0.18 μm, the surface of the first coating layer 20 will not have obvious concave-convex undulations, thereby reducing the bonding force between the first coating layer 20 and the second coating layer 30; when the roughness of the second concave-convex surface 50 is greater than 0.22 μm, the resistance of the composite conductive film is increased, thereby reducing the service life of the composite conductive film. Specifically, as shown in Table 2, when the roughness of the second concave-convex surface 50 of the first coating 20 located on the second surface 102 facing away from the surface of the base layer 10 is 0.18 μm, 0.20 μm, and 0.22 μm, the bonding force between the first coating 20 and the second coating 30 is improved, and the separation of the first coating 20 and the second coating 30 is effectively avoided.

[0050] It should be noted that, in this embodiment, the bonding condition between the base layer 10 and the first coating layer 20, and the bonding condition between the first coating layer 20 and the second coating layer 30 are tested by tape pasting, as shown in Table 2. Specifically, in the present invention, after the first coating layer 20 is sputtered or plated on the surface of the base layer 10, the tape is first pasted on the first coating layer 20, and then the tape is pulled with the same force using a tensile testing machine until the tape is separated from the first coating layer 20. If there is no metal or non-metal material on the tape to which the first coating layer 20 is adhered, it can be considered that the bonding force between the base layer 10 and the first coating layer 20 is improved.

[0051] Table 2 Verification data of examples and comparative examples of the bonding strength between the base layer and the first coating layer, and between the first coating layer and the second coating layer under different roughness

[0052]

[0053] Furthermore, in this embodiment, the first surface 101 and / or the second surface 102 of the base layer 10 is treated by corona treatment or plasma treatment. The base layer 10 in this embodiment is a thin film. During transportation, the base layer 10 needs to be rolled into a roll before it can be transported. Since the tension values ​​on the first surface 101 and the second surface 102 of the base layer 10 are similar or even equal, this will cause the first surface 101 and the second surface 102 of the base layer 10 rolled into a roll to adhere to each other. Therefore, in this embodiment, the base layer 10 is treated by corona treatment or plasma treatment, which can change the tension value on the first surface 101 or the second surface 102, and to a certain extent increase the tension difference between the first surface 101 and the second surface 102, thereby avoiding the first surface 101 and the second surface 102 of the base layer 10 from adhering to each other. See. Figure 1 As shown, in this embodiment, the first surface 101 of the base layer 10 is treated by corona treatment or plasma treatment.

[0054] Further, the first coating 20 in the present embodiment is a metal coating made of one or more of copper, aluminum, copper alloy, aluminum alloy, nickel alloy and titanium alloy; or, the first coating 20 in the present embodiment is a non-metal coating made of one or more of aluminum oxide and silicon nitride. In other words, the first coating 20 in the present invention can be a metal coating or a non-metal coating. When the first coating 20 is made of multiple of copper, aluminum, copper alloy, aluminum alloy, nickel alloy and titanium alloy or multiple of aluminum oxide and silicon nitride, the ratio of copper, aluminum, copper alloy, aluminum alloy, nickel alloy and titanium alloy can be arbitrarily selected, and the ratio of aluminum oxide and silicon nitride can also be arbitrarily selected, and the present invention does not make specific limitations. Since copper, aluminum, copper alloys, aluminum alloys, nickel alloys and titanium alloys have good electrical and thermal conductivity, high chemical stability and good corrosion resistance, using them as the first coating 20 can give full play to the excellent performance of the composite conductive film and enhance the conductivity of the composite conductive film to a certain extent; since the aluminum oxide layer is wear-resistant, corrosion-resistant, high-temperature resistant and has good adhesion, it is easy to combine with other functional layers; the silicon nitride layer has extremely high thermal stability and can operate stably under high temperature and high pressure environments.

[0055] Further, along the first direction, the thickness of the metal coating in this embodiment is 10nm to 1000nm, for example, 10nm, 50nm, 100nm, 200nm, 400nm, 600nm, 800nm, 1000nm and any value therebetween. When the first coating 20 is a metal coating, if the thickness of the metal coating is less than 10nm, it will affect the firmness between the first coating 20 and the second coating 30. If the thickness of the metal coating is greater than 1000nm, the weight of the first coating 20 will be increased, thereby increasing the overall weight of the composite conductive film, thereby increasing the manufacturing cost of the composite conductive film; or,

[0056] Along the first direction, the thickness of the non-metallic coating in this embodiment is 10nm to 500nm, for example, 10nm, 50nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, 500nm and any value therebetween. When the first coating 20 is a non-metallic coating, if the thickness of the non-metallic coating is less than 10nm, it will affect the firmness between the first coating 20 and the second coating 30. If the thickness of the non-metallic coating is greater than 500nm, the weight of the first coating 20 will increase, thereby increasing the overall weight of the composite conductive film, and further increasing the production cost of the composite conductive film.

[0057] Furthermore, the second coating 30 in the present embodiment is made of one or more of copper, aluminum, copper alloy, aluminum alloy, nickel alloy and titanium alloy. When the second coating 30 is made of multiple of copper, aluminum, copper alloy, aluminum alloy, nickel alloy and titanium alloy, the proportion of copper, aluminum, copper alloy, aluminum alloy, nickel alloy and titanium alloy can be selected arbitrarily, and the present invention does not make specific restrictions. Since copper, aluminum, copper alloy, aluminum alloy, nickel alloy and titanium alloy have good electrical conductivity and thermal conductivity, high chemical stability and good corrosion resistance, using them as the first coating 20 can give full play to the excellent performance of the composite conductive film and enhance the electrical conductivity of the composite conductive film to a certain extent.

[0058] Furthermore, the base layer 10 in this embodiment is made of one or more of polyethylene, polypropylene, ethylene-propylene copolymer, polyethylene terephthalate, polyethylene naphthalate, poly(p-phenylene terephthalamide), acrylonitrile-butadiene-styrene copolymer, poly(p-phenylene terephthalamide), polypropylene, polyoxymethylene, epoxy resin, phenolic resin, polytetrafluoroethylene, polyvinylidene fluoride, silicone rubber and polycarbonate. When the base layer 10 is prepared from a variety of polyethylene, polypropylene, ethylene-propylene copolymer, polyethylene terephthalate, polyethylene naphthalate, and poly(p-phenylene terephthalamide), acrylonitrile-butadiene-styrene copolymer, poly(p-phenylene terephthalamide), polypropylene, polyoxymethylene, epoxy resin, phenolic resin, polytetrafluoroethylene, polyvinylidene fluoride, silicone rubber and polycarbonate, the proportions of polyethylene, polypropylene, ethylene-propylene copolymer, polyethylene terephthalate, polyethylene naphthalate, and poly(p-phenylene terephthalamide), acrylonitrile-butadiene-styrene copolymer, poly(p-phenylene terephthalamide), polypropylene, polyoxymethylene, epoxy resin, phenolic resin, polytetrafluoroethylene, polyvinylidene fluoride, silicone rubber and polycarbonate can be selected arbitrarily, and the present invention is not specifically limited thereto.

[0059] Specifically, in one embodiment of the present invention, the base layer 10 in the present invention is preferably made of polypropylene material. This is because polypropylene has strong corrosion resistance and is inert to most acids, alkalis, salts, and oxidants. When the composite conductive film in the present invention is used in a battery, polypropylene is selected as the base layer 10 of the composite conductive film, which is not easily corroded by the electrolyte in the battery, thereby extending the service life of the composite conductive film to a certain extent.

[0060] Specifically, in another embodiment of the present invention, the base layer 10 of the present invention can be made of polypropylene and polyethylene terephthalate. Specifically, the base layer 10 in this embodiment can be a single-layer structure, a double-layer structure, or a multi-layer structure. When the base layer 10 is a single-layer structure, the base layer 10 can be made of a mixture of polypropylene and polyethylene terephthalate, wherein the content of polypropylene is 80% to 90%, such as 80%, 82%, 85%, 87% and 90% and any value therebetween, and the content of polyethylene terephthalate is 10% to 20%, such as 10%, 12%, 14%, 16%, 18%, 20% and any value therebetween; when the base layer 10 is a double-layer structure, polypropylene can be used as the first layer and polyethylene terephthalate can be used as the second layer, wherein the second layer is arranged on two opposite surfaces of the first layer, and the thickness of the second layer is 10nm to 100nm, such as 10nm, 20nm, 40nm, 60nm, 80nm, 100nm. Such an arrangement can improve the adhesion of the base layer 10 without affecting the overall thickness of the base layer 10.

[0061] Table 3 shows the effect of the presence of polyethylene terephthalate on the bonding force between the base layer 10 and the first coating layer 20, wherein the base layer 10 is cut according to the specification of 20 cm in length and 5 cm in width, and a 30 nm first coating layer 20 is sputtered or coated on the base layer 10 by magnetron sputtering, vacuum evaporation or ion plating, and then tested by tape pasting. Embodiments 1 to 3 are base layers 10 made of a mixture of polypropylene and polyethylene terephthalate, and comparative examples 1 to 3 are base layers 10 made of polypropylene. Combined with Table 3, it can be known that the polyethylene terephthalate added to the base layer 10 makes the bonding force between the base layer 10 and the first coating layer 20 greater than 120 N / m. It can be seen that polyethylene terephthalate is easy to bond with the first coating layer 20, thereby improving the bonding force between the base layer 10 and the first coating layer 20.

[0062] It should be noted that the bonding force between the base layer 10 and the first coating layer 20 in Table 3 is tested by tape pasting. Specifically, after the first coating layer 20 is sputtered or plated on the surface of the base layer 10, the present invention first pastes the tape on the first coating layer 20, and then uses a tensile testing machine to pull the tape with a force gradually increasing from 0 tension until the tape is separated from the first coating layer 20. At this time, the number displayed on the tensile testing machine is the bonding force between the base layer 10 and the first coating layer 20. If there is no metal or non-metal material on the tape to which the first coating layer 20 is adhered, it can be considered that the bonding force between the base layer 10 and the first coating layer 20 is qualified.

[0063] Table 3 Effect of the presence of polyethylene terephthalate on the bonding strength between the substrate layer and the first coating layer

[0064]

[0065] At the same time, as shown in Table 4, the present invention uses the prepared composite conductive film as a negative electrode in a battery, and tests the cycle life of the battery. The results show that when the composite conductive film has a first concave-convex surface 40 and a second concave-convex surface 50, the number of cycles of the battery is greater than 900 times, and when the composite conductive film is not provided with the first concave-convex surface 40 and the second concave-convex surface 50, the number of cycles of the battery is less than 850 times. It can be seen that the composite conductive film in the present invention forms the first concave-convex surface 40 and the second concave-convex surface 50 by treating the first surface 101 of the base layer 10 and the surface of the first coating 20 located on the second surface 102 away from the base layer 10, so as to improve the bonding force between the base layer 10 and the first coating 20, and between the first coating 20 and the second coating 30. When the composite conductive film is used as a negative electrode in a battery, the cycle life of the battery is effectively improved.

[0066] Table 4 Verification data of battery cycle life examples and comparative examples

[0067]

[0068]

[0069] Further, along the first direction, the thickness of the second coating layer 30 in the present embodiment is 10 nm to 1000 nm, for example, 10 nm, 50 nm, 100 nm, 200 nm, 400 nm, 600 nm, 800 nm, 1000 nm and any value therebetween. When the thickness of the second coating layer 30 is less than 10 nm, it is not conducive to sputtering or coating the second coating layer 30 on the first coating layer 20. If the thickness of the second coating layer 30 is greater than 1000 nm, the weight of the second coating layer 30 will be increased, thereby increasing the weight of the entire composite conductive film, thereby increasing the manufacturing cost of the composite conductive film.

[0070] Further, along the first direction, the thickness of the base layer 10 in this embodiment is 3 μm to 8 μm, for example, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm and any value therebetween. When the thickness of the base layer 10 is less than 3 μm, the base layer 10 is easily damaged during the stretching process, which is not conducive to the subsequent sputtering or plating of the first plating layer 20 and the second plating layer 30; when the thickness of the base layer 10 is greater than 8 μm, the overall weight of the current collector is increased, thereby increasing the production cost of the current collector.

[0071] On the other hand, the embodiment of the present invention further provides a method for preparing a composite conductive film, hereinafter referred to as the preparation method, which is used to prepare the above-mentioned composite conductive film, and therefore, the preparation method includes all the technical effects of the above-mentioned composite conductive film. Since the technical effects of the composite conductive film have been described in detail above, they will not be repeated here.

[0072] Further, see Figure 2 As shown, the method for preparing the composite conductive film in this embodiment further includes:

[0073] Step S1: preparing a base layer 10, and processing the first surface 101 and / or the second surface 102 of the base layer 10 to obtain a first concave-convex surface 40, wherein the roughness of the first concave-convex surface 40 is a first predetermined value;

[0074] Step S2: preparing a first coating layer 20 on the first surface 101 and the second surface 102, and processing the surface of the first coating layer 20 on the first surface 101 away from the base layer 10 and / or the surface of the first coating layer 20 on the second surface 102 away from the base layer 10 to obtain a second concave-convex surface 50, wherein the roughness of the second concave-convex surface 50 is a second predetermined value;

[0075] Step S3: preparing a second coating layer 30 on the surface of the first coating layer 20 facing away from the base layer 10 .

[0076] Further, in step S1, the first surface 101 and / or the second surface 102 are treated by plasma treatment or corona treatment so that the first predetermined value is 0.18 μm to 0.22 μm, and the base layer 10 is prepared by casting, extrusion or blow molding. Figure 1 The situation when the first surface 101 is treated by a plasma treatment method or a corona treatment method is shown.

[0077] Further, in step S2, a plasma treatment method or a corona treatment method is used to treat the surface of the first coating 20 away from the base layer 10, so that the second predetermined value is 0.18 μm to 0.22 μm, and a magnetron sputtering method or a vacuum evaporation method or an ion plating method is used to prepare the first coating 20 on the first surface 101 and the second surface 102. Specifically, in the present invention, the first coating 20 is Figure 1 The diagram shows a situation where the surface of the first coating layer 20 located on the second surface 102 facing away from the base layer 10 is treated by a plasma treatment method or a corona treatment method.

[0078] Furthermore, in step S3 , the second coating layer 30 is prepared on the surface of the first coating layer 20 away from the base layer 10 by using magnetron sputtering, vacuum evaporation or ion plating.

[0079] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.

[0080] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. If not otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.

[0081] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A composite conductive film, characterized in that: include: A base layer (10), along a first direction, the base layer (10) comprising a first surface (101) and a second surface (102) opposite to the first surface (101), at least one of the first surface (101) and the second surface (102) having a first concavo-convex surface (40), the first concavo-convex surface (40) being at least used to improve the surface adhesion of the base layer (10); a first coating (20), the first coating (20) being disposed on the first surface (101) and the second surface (102), respectively, at least one of a surface of the first coating (20) on the first surface (101) facing away from the base layer (10) and a surface of the first coating (20) on the second surface (102) facing away from the base layer (10) having a second concavo-convex surface (50), the second concavo-convex surface (50) being used at least to improve the surface adhesion of the first coating (20); A second coating layer (30), wherein the second coating layer (30) is arranged on a surface of the first coating layer (20) facing away from the base layer (10).

2. The composite conductive film according to claim 1, characterized in that: The second plating layer (30) has a surface square resistance, and the square resistance change rate ρ of the surface square resistance satisfies the relationship: ρ<5×10 -2 .

3. The composite conductive film according to any one of claims 1 to 2, characterized in that: The roughness of the first concavo-convex surface (40) is 0.18 μm to 0.22 μm; and / or, The roughness of the second concavo-convex surface (50) is 0.18 μm to 0.22 μm.

4. The composite conductive film according to claim 3, characterized in that: The first coating (20) is a metal coating made of one or more of copper, aluminum, copper alloy, aluminum alloy, nickel alloy and titanium alloy; or, The first coating (20) is a non-metallic coating made from one or more of aluminum oxide and silicon nitride.

5. The composite conductive film according to claim 4, characterized in that: Along the first direction, the thickness of the metal coating is 10 nm to 1000 nm; or, Along the first direction, the thickness of the non-metallic coating is 10 nm to 500 nm.

6. The composite conductive film according to claim 1, 2, 4 or 5, characterized in that: The second coating (30) is made of one or more of copper, aluminum, copper alloy, aluminum alloy, nickel alloy and titanium alloy; and / or, The base layer (10) is made of one or more of polyethylene, polypropylene, ethylene-propylene copolymer, polyethylene terephthalate, polyethylene naphthalate, poly(p-phenylene terephthalamide), acrylonitrile-butadiene-styrene copolymer, poly(p-phenylene terephthalamide), polypropylene, polyoxymethylene, epoxy resin, phenolic resin, polytetrafluoroethylene, polyvinylidene fluoride, silicone rubber and polycarbonate.

7. The composite conductive film according to claim 1, 2, 4 or 5, characterized in that: Along the first direction, the thickness of the second coating layer (30) is 10 nm to 1000 nm.

8. The composite conductive film according to claim 1, 2, 4 or 5, characterized in that: Along the first direction, the thickness of the base layer (10) is 3 μm to 8 μm.

9. A method for preparing a composite conductive film, characterized in that: The method for preparing the composite conductive film is used to prepare the composite conductive film according to any one of claims 1 to 8, and the method for preparing the composite conductive film further comprises: Step S1: preparing the base layer (10), and processing the first surface (101) and / or the second surface (102) of the base layer (10) to obtain the first concave-convex surface (40), wherein the roughness of the first concave-convex surface (40) is a first predetermined value; Step S2: preparing the first coating layer (20) on the first surface (101) and the second surface (102), and processing the surface of the first coating layer (20) on the first surface (101) facing away from the base layer (10) and / or the surface of the first coating layer (20) on the second surface (102) facing away from the base layer (10) to obtain the second concave-convex surface (50), wherein the roughness of the second concave-convex surface (50) is a second predetermined value; Step S3: preparing the second coating layer (30) on the surface of the first coating layer (20) facing away from the base layer (10).

10. The method for preparing a composite conductive film according to claim 9, characterized in that: In the step S1, the first surface (101) and / or the second surface (102) are treated by a plasma treatment method or a corona treatment method so that the first predetermined value is 0.18 μm to 0.22 μm, and the base layer (10) is prepared by a casting method, an extrusion method or a blow molding method; In the step S2, a surface of the first coating layer (20) facing away from the base layer (10) is subjected to a plasma treatment method or a corona treatment method so that the second predetermined value is 0.18 μm to 0.22 μm, and the first coating layer (20) is prepared on the first surface (101) and the second surface (102) by a magnetron sputtering method or a vacuum evaporation method or an ion plating method; In the step S3, the second coating layer (30) is prepared on the surface of the first coating layer (20) facing away from the base layer (10) by using a magnetron sputtering method, a vacuum evaporation method or an ion plating method.