High-entropy oxide solid electrolyte material with NASICON structure and preparation method of high-entropy oxide solid electrolyte material
Through the preparation of NASICON structure high-entropy oxide electrolyte materials, the problem of Ti ion reduction in LATP solid electrolyte materials under electrochemical conditions is solved, the lithium ion conductivity and material stability are improved, and the battery energy efficiency and cycle are achieved. life.
Patent Information
- Application Number
- CN202411612388.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-13
- Publication Date
- 2025-01-07
AI Technical Summary
Under electrochemical working conditions, when aluminum-doped lithium titanium phosphate (LATP) solid electrolyte material comes into contact with a high-energy density lithium metal negative electrode, Ti ions are easily reduced to +3 valence, destroying the structure and affecting the transmission of lithium ions, reducing the battery Energy efficiency and cycle life.
Li1.3M0.3Ti1.7(PO4)3 (M stands for M) is prepared by precalcining, wet ball milling, drying, high-temperature solid phase reaction and high-temperature sintering. B, Al, Ga, In) High-entropy LMTP electrolyte material introduces a variety of elements to adjust the lattice and electronic band structure and inhibit the valence state transition of Ti elements.
The ionic conductivity, material stability and cycle life of the electrolyte are significantly improved, the Ti element is not easy to be reduced, and the lithium ion conductivity reaches 5.50×10-4 S/cm, which is better than the existing LATP materials.
Smart Images

Figure CN119275334A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solid-state batteries, and in particular relates to a NASICON structure high-entropy oxide solid electrolyte material and a preparation method thereof. Background Art
[0002] The liquid organic electrolytes widely used in traditional lithium-ion batteries have great safety hazards. They may leak, volatilize and burn at high temperatures during operation, which seriously affects the battery life. In addition, liquid electrolytes are difficult to match with high-voltage positive electrodes due to their narrow electrochemical window, and thus cannot have higher energy density. Using solid electrolyte materials with non-flammable properties to replace liquid electrolytes and organic diaphragms in traditional batteries can greatly improve the safety performance of batteries; at the same time, solid electrolytes with wide electrochemical windows can directly use metallic lithium as the negative electrode and match them with high-voltage positive electrode materials, which can break through the low energy density limitations of liquid organic electrolytes and thus meet the current high safety and high energy density requirements for lithium-ion batteries.
[0003] Common solid electrolytes in the prior art mainly include: polymer solid electrolytes, sulfide solid electrolytes and oxide solid electrolytes. Among them, although polymer solid electrolytes have excellent processing properties, their ion conductivity is low and their mechanical strength is not high; sulfide solid electrolytes have the highest ion conductivity, but their air stability is extremely poor, and they are chemically unstable to lithium metal, making them difficult to use on a large scale; oxide solid electrolytes have relatively high ion conductivity and good chemical stability, and have the best comprehensive performance. They are the electrolyte materials that are easiest to commercialize.
[0004] The oxide solid electrolytes that have been studied more thoroughly are NASICON (sodium super ion conductor) type, LISICON (lithium super ion conductor) type, perovskite type and garnet type. Among them, NASICON type lithium ion inorganic solid electrolytes have attracted much attention due to their high room temperature ionic conductivity and good stability. 1+x Al x Ti 2-x (PO4)3, x = 0.3 ~ 0.5, abbreviation: LATP) as one of the important research systems, has good environmental stability (to water and air), easy synthesis, low cost, high ionic conductivity (10 -4 ~10 -3 S / cm), etc., it is an oxide solid electrolyte material that is expected to achieve industrial large-scale production. Based on this, technicians in this field have conducted a lot of research on its preparation and application.
[0005] However, studies have shown that under electrochemical working conditions, after the LATP solid electrolyte comes into contact with the high-energy-density lithium metal negative electrode, the Ti ions in it are easily reduced from +4 to +3, which not only destroys the structure of LATP, but also the generated reaction products will cause a large interfacial impedance, affecting the transmission of lithium ions, thereby reducing the energy efficiency and cycle life of the battery. Summary of the invention
[0006] The purpose of the present invention is to solve the deficiencies in the prior art and provide a NASICON structure high entropy oxide solid electrolyte material and a preparation method thereof, which can improve the problem that +4-valent titanium ions are reduced to +3-valent titanium ions when the LATP oxide solid electrolyte material contacts a metal negative electrode, and promote the application of NASICON structure high entropy oxide solid electrolytes in solid-state lithium-ion batteries.
[0007] The specific technical solution of the present invention is: a method for preparing a NASICON structure high entropy oxide solid electrolyte material, comprising the following steps: 1) Pre-calcining lithium source, boron source, aluminum source, gallium source, indium source, titanium source and phosphate raw materials; 2) Weigh the pre-calcined raw materials, mix them, wet-mill them, and dry them to obtain ball-milled powder; 3) Calcine the ball-milled powder using a high-temperature solid-phase reaction method to generate electrolyte powder; 4) Wet ball milling the electrolyte powder and drying it to obtain electrolyte fine powder; 5) Sintering electrolyte powder at high temperature to obtain high entropy LMTP solid electrolyte material.
[0008] Furthermore, in step 1), the process of pre-calcining the raw materials is carried out in a muffle furnace, the calcination environment atmosphere is air, the calcination temperature is 100-150° C., and the calcination time is 3-6 h.
[0009] Furthermore, in step 2), the wet ball milling speed is 100-150 rpm, the ball milling time is 6-12 h, and the mass ratio of the raw material, the ball milling balls and the ethanol solvent is 1:3:5.
[0010] Furthermore, in step 3), the calcination temperature is 850-1100°C, the heating rate is 5-10°C / min, the holding time is 5-10 h, and after the calcination is completed, the furnace is cooled to room temperature.
[0011] Furthermore, in step 4), the wet ball milling speed is 200-300 rpm, the ball milling time is 6-12 h, and the mass ratio of the electrolyte powder, the ball milling balls and the ethanol solvent is 1:3:5.
[0012] Furthermore, in step 5), the high temperature sintering method is selected from one of buried powder pressureless sintering, spark plasma sintering or hot pressing sintering.
[0013] Preferably, when the spark plasma sintering technology is adopted, the sintering atmosphere is an inert atmosphere, the sintering temperature is 900~1200℃, and the heating rate is 80~100℃ / min; when the buried powder pressureless sintering technology is adopted, the electrolyte fine powder is first pressed to obtain the green body of the solid electrolyte sheet, the pressing pressure is 150~300 MPa, the holding time is 2~10 min, and then the green body of the solid electrolyte sheet is immersed in the electrolyte fine powder for sintering, the sintering environment atmosphere is air, the heating rate is 8~15℃ / min, the sintering temperature is 900~1200℃, and the holding time is 4~8 h; when the hot pressing sintering process is adopted, the axial pressure is 50-80 MPa, the sintering atmosphere is an inert atmosphere, the heating rate is 8~12℃ / min, the sintering temperature is 1000~1200℃, and the holding time is 1~3 h.
[0014] The high entropy oxide solid electrolyte material prepared by the above method is a NASICON structure electrolyte material, and its chemical formula is Li 1.3 M 0.3 Ti 1.7 (PO4)3, denoted as LMTP, M represents the four elements B, Al, Ga, and In. The sum of the number of atoms of these four elements is equal to 0.3, that is, M 0.3 =B x Al y Ga z In 0.3-x-y-z , where 0<x<0.3, 0<y<0.3, 0<z<0.3.
[0015] The above-mentioned high entropy oxide solid electrolyte materials can be applied in lithium-ion batteries, micro-power sources and devices, electrochromic devices and other electrochemical processes.
[0016] Compared with the prior art, the present invention has the following advantages: The high entropy LMTP solid electrolyte material prepared by the method disclosed in this application is a NASICON structure electrolyte, and its chemical formula is Li 1.3 M 0.3 Ti 1.7 (PO4)3, where M represents B, Al, Ga, and In elements, and the sum of the number of atoms of these four elements is equal to 0.3; by introducing multiple elements into the LATP crystal structure, the size of adjacent atoms and the ionic bond energy in the lattice are different, which leads to local distortion in the lattice. The larger local distortion makes the Li at different sites + The sites can overlap with each other, and the overlapping Li + The site energy reduces the Li+ The migration activation energy can effectively improve the ionic conductivity of LATP solid electrolyte materials. It has been verified that the ionic conductivity of high entropy LMTP solid electrolyte materials can reach 5.50×10 -4 S / cm, significantly better than the existing LATP (3.96×10 -4 S / cm) solid electrolyte; The electrolyte material prepared in this application introduces multiple elements at the Ti position to form high entropy. The high entropy effect can inhibit the transition of the Ti element between different valence states through multiple mechanisms such as the regulation of the electronic energy band structure, lattice distortion, and mixed entropy, which helps to lock the valence of the Ti element and make the material show higher stability. It has been verified that the color of the high entropy electrolyte material prepared in this application does not change significantly when treated with high-temperature reducing gas, indicating that the titanium element is more stable and Ti 4+ Not significantly reduced to Ti 3+ ; The present application utilizes a high-temperature solid-phase method to prepare a high-entropy solid electrolyte powder, and then prepares a high-entropy solid electrolyte product by high-temperature sintering. The preparation process is simple and convenient for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a system flow chart for preparing high-entropy LMTP solid electrolyte materials in this application; Figure 2 is the X-ray diffraction pattern of the high entropy LMTP solid electrolyte material prepared in Example 1; Figure 3 is a SEM-mapping image of the high entropy LMTP solid electrolyte material prepared in Example 1; Figure 4 is the AC impedance spectrum of the high entropy LMTP solid electrolyte material and the LATP electrolyte sheet prepared in Example 1; Figure 5 This is a comparison chart of the color changes of the high entropy LMTP electrolyte sheet and the LATP electrolyte sheet prepared in Example 1 after high-temperature annealing in a reducing atmosphere. DETAILED DESCRIPTION
[0018] The technical solution of the present invention is further described below in conjunction with the accompanying drawings, but is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention. Example
[0019] A preparation method of high entropy LMTP solid electrolyte material, the preparation process is referenced Figure 1 , the specific steps are as follows: 1) Li2CO3, NH4H2PO4, TiO2, B2O3, Al2O3, Ga2O3, and In2O3 were pre-calcined in a muffle furnace at 120°C in an air atmosphere for 3 h. The purpose is to remove carbon dioxide, moisture, and other impurities in the raw materials.
[0020] 2) According to the stoichiometric ratio of 1.3:0.075:0.075:0.075:0.075:1.7:3, weigh pre-calcined Li2CO3, Al2O3, B2O3, Ga2O3, In2O3, TiO2 and NH4H2PO4.
[0021] 3) Pour the weighed raw materials into a planetary ball mill, add ball milling balls and ethanol solvent, the weight ratio of mixed raw materials / ball milling balls / ethanol solvent is 1:3:5, the rotation speed is 120 rpm, the mixing time is 10 h, and after the ball milling is completed, dry at 60°C to obtain ball milled powder.
[0022] 4) The ball-milled powder is placed in a high-temperature furnace and calcined by a high-temperature solid-phase reaction method to generate a high-entropy LMTP electrolyte powder. The heating rate of the furnace is 10°C / min, the calcination temperature is 950°C, and the calcination time is 6 h. After the calcination is completed, it is cooled to room temperature with the furnace.
[0023] 5) Wet-mill the high-entropy LMTP electrolyte powder in a planetary ball mill, with a weight ratio of high-entropy LMTP electrolyte powder / ball milling balls / ethanol solvent of 1:3:5, a ball milling speed of 200 rpm, and a ball milling time of 8 h. After the ball milling is completed, dry at 60° C. for later use.
[0024] 6) The ball-milled high-entropy LMTP electrolyte powder was sintered into a ceramic sheet using spark plasma sintering (SPS) technology. The sintering conditions were as follows: sintering under inert atmosphere, applying an axial pressure of 50-80 MPa, heating at a heating rate of 100°C / min, sintering temperature of 1100°C, keeping warm for 5 min, and cooling to room temperature with the furnace to obtain a high-entropy LMTP solid electrolyte material with a chemical formula of Li 1.3 Al 0.075 B 0.075 Ga 0.075 In 0.075 Ti 1.7 (PO4)3.
[0025] Figure 2 This is the X-ray diffraction spectrum of the high-entropy LMTP solid electrolyte material obtained in this example. From the figure, it can be seen that the XRD diffraction peaks of the obtained material are consistent with the LATP standard card, which is a typical NASICON crystal structure and does not contain other impurities, indicating that B, Al, Ga, and In elements have all been successfully doped into the LATP crystal structure.
[0026] Figure 3 This is the SEM-mapping image of the high entropy LMTP solid electrolyte material obtained in this example. Figure 3 This reflects that the LMTP solid electrolyte sheet is well sintered, has high density, and elements such as B, Al, Ga, and In are evenly distributed.
[0027] The lithium ion conductivity of the high entropy LMTP solid electrolyte material obtained in this example was tested, and the results are shown in Figure 4 The results show that the lithium ion conductivity of the high entropy LMTP solid electrolyte material (5.50×10 -4 S / cm) was significantly better than LATP (3.96×10 -4 S / cm) material.
[0028] The high entropy LMTP electrolyte sheet prepared in this embodiment and the existing LATP electrolyte sheet were treated by high temperature annealing in a reducing atmosphere (5% H2-95% Ar mixed atmosphere, high temperature treatment at 1100°C for 6h), and the color changes of the materials before and after the treatment were observed. The results are shown in Figure 5 , Figure 5 It is shown that after high-temperature reducing gas treatment, the color of the LATP electrolyte sheet changes from white to black (Ti 4+ Reduction to Ti 3+ The color of the high-entropy LMTP electrolyte sheet hardly changed, indicating that the titanium element in the high-entropy LMTP electrolyte material is more stable and not easily reduced to Ti 3+ . Example
[0029] 1) Li2CO3, NH4H2PO4, TiO2, B2O3, Al2O3, Ga2O3 and In2O3 were pre-calcined in a muffle furnace at 150°C in an air atmosphere for 3 h.
[0030] 2) Weigh pre-calcined Li2CO3, Al2O3, B2O3, Ga2O3, In2O3, TiO2 and NH4H2PO4 according to the stoichiometric ratio of 1.3:0.15:0.05:0.05:0.05:1.7:3.
[0031] 3) Pour the weighed raw materials into a planetary ball mill, add ball milling balls and ethanol solvent, the weight ratio of mixed raw materials / ball milling balls / ethanol solvent is 1:3:5, the rotation speed is 150 rpm, the mixing time is 12 h, and after the ball milling is completed, dry at 70°C to obtain ball milled powder.
[0032] 4) The ball-milled powder is placed in a high-temperature furnace and calcined by a high-temperature solid-phase reaction method to generate a high-entropy LMTP electrolyte powder. The heating rate of the furnace is 8°C / min, the calcination temperature is 1000°C, and the calcination time is 8 h. After the calcination is completed, it is cooled to room temperature with the furnace.
[0033] 5) Wet-mill the high-entropy LMTP electrolyte powder in a planetary ball mill, with a weight ratio of high-entropy LMTP electrolyte powder / ball milling balls / ethanol solvent of 1:3:5, a ball milling speed of 250 rpm, and a ball milling time of 8 h. After the ball milling is completed, dry at 70° C. for later use.
[0034] 6) The refined high-entropy LMTP electrolyte powder is pressed by a tablet press to obtain a solid electrolyte sheet body. The applied pressure of the tablet press is 200 MPa and the holding time is 8 min.
[0035] 7) The obtained solid electrolyte sheet green body is immersed in the refined high entropy LMTP electrolyte powder and sintered in a muffle furnace to form a high entropy LMTP solid electrolyte sheet. The sintering conditions are: sintering under air conditions, heating at a heating rate of 10℃ / min, sintering temperature of 1050℃, keeping warm for 6 hours, and cooling to room temperature with the furnace. The high entropy LMTP solid electrolyte material is obtained, and the chemical formula is Li 1.3 Al 0.15 B 0.05 Ga 0.05 In 0.05 Ti 1.7 (PO4)3. Example
[0036] 1) Li2CO3, NH4H2PO4, TiO2, B2O3, Al2O3, Ga2O3 and In2O3 were pre-calcined in a muffle furnace at 130°C in an air atmosphere for 6 h.
[0037] 2) Weigh pre-calcined Li2CO3, Al2O3, B2O3, Ga2O3, In2O3, TiO2 and NH4H2PO4 according to the stoichiometric ratio of 1.3:0.1:0.1:0.05:0.05:1.7:3.
[0038] 3) Pour the weighed raw materials into a planetary ball mill, add ball milling balls and ethanol solvent, the weight ratio of mixed raw materials / ball milling balls / ethanol solvent is 1:3:5, the rotation speed is 100 rpm, the mixing time is 15 h, and after the ball milling is completed, dry at 65°C to obtain ball milled powder.
[0039] 4) The ball-milled powder is placed in a high-temperature furnace and calcined by a high-temperature solid-phase reaction method to generate a high-entropy LMTP electrolyte powder. The heating rate of the furnace is 10°C / min, the calcination temperature is 1100°C, the calcination time is 5 h, and after the calcination is completed, it is cooled to room temperature with the furnace.
[0040] 5) Wet-mill the high-entropy LMTP electrolyte powder in a planetary ball mill, with a weight ratio of high-entropy LMTP electrolyte powder / ball milling balls / ethanol solvent of 1:3:5, a ball milling speed of 200 rpm, and a ball milling time of 10 h. After the ball milling is completed, dry at 65° C. for later use.
[0041] 6) The high entropy LMTP electrolyte powder was sintered into a ceramic sheet using a hot pressing sintering furnace. The sintering conditions were: applying an axial pressure of 60 MPa, sintering under argon, heating at a rate of 10 °C / min, sintering temperature of 1100 °C, keeping warm for 1.5 hours, and cooling to room temperature with the furnace. The high entropy LMTP solid electrolyte material was obtained, with the chemical formula of Li 1.3 Al 0.1 B 0.1 Ga 0.05 In 0.05 Ti 1.7 (PO4)3.
Claims
1. A method for preparing a NASICON structure high entropy oxide solid electrolyte material, characterized in that: The steps include: 1) Pre-calcining lithium source, boron source, aluminum source, gallium source, indium source, titanium source and phosphate raw materials; 2) Weigh the pre-calcined raw materials, mix them, wet-mill them, and dry them to obtain ball-milled powder; 3) Calcine the ball-milled powder using a high-temperature solid-phase reaction method to generate electrolyte powder; 4) Wet ball milling the electrolyte powder and drying it to obtain electrolyte fine powder; 5) Sintering electrolyte powder at high temperature to obtain high entropy LMTP solid electrolyte material.
2. The method for preparing a NASICON structure high entropy oxide solid electrolyte material according to claim 1, characterized in that: In step 1), the process of pre-calcining the raw materials is carried out in a muffle furnace, the calcination environment atmosphere is air, the calcination temperature is 100-150° C., and the calcination time is 3-6 h.
3. The method for preparing a NASICON structure high entropy oxide solid electrolyte material according to claim 1, characterized in that: In step 2), the wet ball milling speed is 100-150 rpm, the ball milling time is 6-12 h, and the mass ratio of the raw material, the ball milling balls and the ethanol solvent is 1:3:
5.
4. The method for preparing a NASICON structure high entropy oxide solid electrolyte material according to claim 1, characterized in that: In step 3), the calcination temperature is 850-1100°C, the heating rate is 5-10°C / min, the holding time is 5-10 h, and after the calcination is completed, the furnace is cooled to room temperature.
5. The method for preparing a NASICON structure high entropy oxide solid electrolyte material according to claim 1, characterized in that: In step 4), the wet ball milling speed is 200-300 rpm, the ball milling time is 6-12 h, and the mass ratio of the electrolyte powder, the ball milling balls and the ethanol solvent is 1:3:
5.
6. The method for preparing a NASICON structure high entropy oxide solid electrolyte material according to claim 1, characterized in that: In step 5), the high temperature sintering method is selected from one of buried powder pressureless sintering, spark plasma sintering or hot pressing sintering.
7. The method for preparing a NASICON structure high entropy oxide solid electrolyte material according to claim 6, characterized in that: When the spark plasma sintering technology is adopted, the sintering atmosphere is an inert atmosphere, the sintering temperature is 900~1200℃, and the heating rate is 80~100℃ / min; when the buried powder pressureless sintering technology is adopted, the electrolyte fine powder is first pressed to obtain the green body of the solid electrolyte sheet, the pressing pressure is 150~300 MPa, the holding time is 2~10 min, and then the green body of the solid electrolyte sheet is immersed in the electrolyte fine powder for sintering, the sintering environment atmosphere is air, the heating rate is 8~15℃ / min, the sintering temperature is 900~1200℃, and the holding time is 4~8 h; when the hot pressing sintering process is adopted, the axial pressure is 50-80 MPa, the sintering atmosphere is an inert atmosphere, the heating rate is 8~12℃ / min, the sintering temperature is 1000~1200℃, and the holding time is 1~3 h.
8. A high entropy oxide solid electrolyte material, characterized in that: It is prepared according to the preparation method described in any one of claims 1 to 7, and is an electrolyte material with a NASICON structure, and its chemical formula is Li 1.3 M 0.3 Ti 1.7 (PO4)3, denoted as LMTP, M represents the four elements B, Al, Ga, and In. The sum of the number of atoms of these four elements is equal to 0.3, that is, M 0.3 =B x Al y Ga z In 0.3-x-y-z , where 0<x<0.3, 0<y<0.3, 0<z<0.
3.
9. Use of a high entropy oxide solid electrolyte material as claimed in claim 8 in a lithium ion battery.
Citation Information
Cited By
Method for eliminating LLZTO pores and improving performance of solid electrolyte through oxygen-assisted sintering
CN120237280A
High-entropy bismuth oxide-based electrolyte as well as preparation method and application thereof