Size reduction and reconstitution of grain refiner for casting of inclusion sensitive alloys
Patent Information
- Application Number
- CN202580024387.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-03-26
- Filing Date
- 2025-03-21
- Publication Date
- 2026-11-03
AI Technical Summary
Traditional grain refiners interact with impurity elements in recycled aluminum alloys, leading to the formation of intermetallic compound particles, which in turn cause cracks and other defects in cast products, especially in aluminum alloys containing recycled components.
The grain refiner product is mechanically deformed into grain refiner fragments with a particle size of less than 1000 µm, wherein at least a portion of the particles are TiAl3 phase particles with an equivalent spherical diameter of less than or about 50 µm, and these fragments are added to the liquid aluminum alloy to reduce the necessary residence time in order to reduce the formation of intermetallic compound particles larger than or about 50 µm.
It effectively reduces the size of intermetallic compound particles, improves the grain characteristics of cast products, and reduces the risk of rivet formation defects, especially in recycled aluminum alloys.
Smart Images

Figure CN123036394A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the processing of molten aluminum and aluminum alloys. In particular, this technology relates to the crushing and refining of grain refiner products and their use in the processing of molten aluminum and aluminum alloys. Background Technology
[0002] Nucleating agents, such as titanium-containing grain refiners, are typically added to molten aluminum and aluminum alloys during the casting process. Grain refiners can be incorporated into the melt to improve the as-cast grain structure, making it more uniform and containing a high percentage of fine grains. However, grain refiners are carefully tailored to the aluminum alloys present in the melt because various alloying elements can lead to undesirable crystal formation during solidification. That is, conventional grain refiners interact adversely with some alloying elements, such as magnesium and vanadium, especially at high concentrations, forming intermetallic compound particles. These intermetallic compound particles do not disperse or dissolve in the melt, leading to cracks and other defects in the cast product.
[0003] Recycled scrap metal includes metals from scrap metal products, which are collected and used to manufacture other metal products. Waste beverage cans (UBC) scrap is metal collected from waste beverage cans and similar products, which can be recycled for use in other metal products. Aluminum UBC scrap is typically a mixture of various aluminum alloys (e.g., from different alloys used for can bodies and can ends) and may often contain foreign matter such as rainwater, beverage residues, organic matter (e.g., paint and laminations), and other materials. UBC scrap can be shredded and decoated or stripped before melting to serve as a liquid metal feedstock when casting new metal products. However, such recycled scrap from beverage containers and other recycled components contains impurities and unbalanced alloying elements, such as increased levels of silicon (Si), magnesium (Mg), vanadium (V), calcium (Ca), strontium (Sr), titanium (Ti), beryllium (Be), chromium (Cr), and / or manganese (Mn), which are difficult to remove from the recycled scrap and the resulting alloy melt.
[0004] With the increasing demand for utilizing recycled scrap metal, controlling alloys within the elemental range of conventional grain refiner products has become increasingly problematic. Specifically, the use of conventional grain refiner products has resulted in large intermetallic compound particles detected in articles containing recycled alloy components, which can lead to cracking and other problems, such as rivet formation defects. Therefore, there is a need in the art for a grain refiner product compatible with various alloy impurities. There is also a need in the art for casting aluminum alloys with alloy impurities that exhibit improved grain characteristics. Summary of the Invention
[0005] The embodiments covered by this patent are defined by the following claims, not by the content of this invention. The content of this invention is a high-level generalization of various embodiments and introduces some concepts further described in the following detailed description section. The content of this invention is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used alone to define the scope of the claimed subject matter. This subject matter should be understood by referring to the appropriate portions of the entire specification of this patent, any or all of the drawings, and each claim.
[0006] This technology relates to a metal casting method and a suitable grain refiner product. The method includes forming a liquid aluminum alloy. The method includes mechanically deforming the grain refiner product into grain refiner fragments with a particle size less than 1000 µm, wherein at least a portion of the mechanically deformed grain refiner fragment particles comprises one or more TiAl3 phase particles with an equivalent spherical diameter less than or about 50 µm. The method includes adding the mechanically deformed grain refiner fragments to the liquid aluminum alloy, casting the liquid metal into a metal product, and rolling the metal product.
[0007] In the embodiments, substantially all grain refiner debris comprises TiAl3 phase particles with an equivalent spherical diameter of less than or equal to 50 μm. Furthermore, in the embodiments, the mechanically deformed grain refiner debris is added in the form of chips, granules, tablets, or combinations thereof. In more embodiments, mechanical deformation includes sawing, grinding, rolling, extrusion, machining, impact, or combinations thereof. Additionally or alternatively, in the embodiments, mechanical deformation is performed for a period of time to produce greater than or equal to 500 TiAl3 particles / mm. 2In further embodiments, the metal product comprises one or more intermetallic compound particles, each of which has an equivalent spherical diameter of less than or about 10 μm. Additionally, in embodiments, the aluminum alloy comprises one or more of beryllium, magnesium, vanadium, strontium, titanium, and calcium. In further embodiments, the aluminum alloy comprises 5xxx series alloys. In embodiments, the molten metal comprises greater than or 10% by weight recycled aluminum alloy. In further embodiments, the aluminum alloy comprises 0.01% by weight to 0.1% by weight titanium. Furthermore, in embodiments, the aluminum alloy comprises 1% by weight to 7% by weight magnesium. In embodiments, the aluminum alloy comprises 0.01% by weight to 0.1% by weight vanadium. Embodiments include where greater than or 50% by weight of the grain refiner debris comprises TiAl3 phase particles with an equivalent diameter of less than or equal to 50 μm. Alternatively or additionally, in embodiments, greater than or 50% by weight of the grain refiner debris comprises TiAl3 phase particles with an equivalent diameter of less than or equal to 20 μm. Furthermore, in the embodiments, greater than or 50% by weight of the grain refiner debris comprises TiAl3 phase particles with an equivalent diameter of less than or equal to 10 μm. This technology also relates generally to metal products cast by any one or more of the methods discussed above.
[0008] This technology also relates generally to 5xxx series aluminum alloy products. 5xxx series aluminum alloy products contain 0.01–1.0 wt% Cu, 0.1–0.8 wt% Fe, 0.5–7.0 wt% Mg, 0.01–1.2 wt% Mn, 0–1.5 wt% Si, 0–0.2 wt% Ti, 0–8.0 wt% Zn, 0–0.3 wt% Cr, 0–0.15 wt% Zr, 0–0.1 wt% V, 0–0.15 wt% Ca, up to 0.15 wt% impurities, and Al. The aluminum alloy products contain intermetallic compound particles, wherein the intermetallic compound particles contain two or more of aluminum, beryllium, magnesium, vanadium, strontium, titanium, and calcium, wherein the intermetallic compound particles have an equivalent spherical diameter of less than 50 μm. This technology also relates generally to a beverage container comprising an aluminum alloy product as discussed herein.
[0009] This technology also relates generally to a TiAl3-containing grain refiner product. The grain refiner product comprises grain refiner fragments with a particle size less than 1000 μm, wherein more than 50% by weight of the grain refiner fragments contain TiAl3 phase particles with an equivalent spherical diameter less than or equal to 50 μm. In an embodiment, substantially all of the grain refiner fragments contain TiAl3 phase particles with an equivalent spherical diameter less than or equal to 50 μm.
[0010] The various embodiments described herein may include additional systems, methods, features, and advantages that may not necessarily be explicitly disclosed herein but will be apparent to those skilled in the art upon review of the following detailed description and accompanying drawings. All such systems, methods, features, and advantages are intended to be included within this disclosure and protected by the appended claims. Attached Figure Description
[0011] This specification refers to the following figures, in which the same reference numerals are used in different figures to illustrate the same or similar parts.
[0012] Figure 1 An example of a metal handling system according to the implementation plan is shown. Detailed Implementation
[0013] The subject matter of the embodiments described herein is intended to satisfy statutory requirements, but this description is not necessarily intended to limit the scope of the claims. The claimed subject matter may be embodied in other ways, may include different elements or steps, and may be used in conjunction with other existing or future techniques. This description should not be construed as implying any particular order or arrangement of the various steps or elements, except where the order of the arrangement of the various steps or elements is clearly described. Directional references such as “up,” “down,” “top,” “bottom,” “left,” “right,” “front,” and “rear” are intended to refer to the orientation shown and described in one or more figures referring to the parts and directions. While the systems and methods described herein can be used with any metal, they are particularly suitable for aluminum or aluminum alloys.
[0014] Grain refiner products are typically manufactured by reacting molten aluminum with various reactive salts (such as K₂TiF₄ and KBF₄, by way of example only) to form a suspension of TiB₂ and TiAl₃. The suspension is then formed into bars with diameters from approximately 9.5 mm to approximately 50 mm. The grain refiner product is then introduced into the molten aluminum alloy early in the casting process, such as upstream of the degasser and / or metal filter, to interact with the alloy and nucleate the system. The grain refiner product is typically introduced at this stage to ensure complete dissolution of TiAl₃ before ingot formation. That is, existing grain refiner products require a significant residence time in the melt to ensure complete dissolution and dispersion of TiAl₃ particles. However, with the increase of recycled components in the alloy precursor material, prolonged residence time in the melt is considered to lead to the formation of intermetallic compound particles. For example, as discussed above, the presence or increased concentration of Ti, Mg, V, and / or Ca in the recycled components can lead to Al… x Mg y Ti z V t Cau The formation of intermetallic compound particles, where, by way of example only, x can range from 0 to 18, y and u can be independently selected from 0 to 3, and z and t can be independently selected from 0 to 2. Furthermore, due to the nucleation effect of the grain refiner product, it is believed that such intermetallic compound particles can form around, or even completely surround, TiAl3 particles, thereby preventing the dissolution and dispersion of TiAl3 particles and allowing the formation of TiAl3 particles and / or intermetallic compound particles larger than 100 μm in the final melt and ingot. This is increasingly problematic for products with thin dimensions (such as beverage containers), as rivets formed in the can body or can end may have a product thickness of less than 150 μm, making the product susceptible to breakage and damage due to the large particles formed in or around the grain refiner.
[0015] This document describes grain refiner products with improved performance, even in alloys containing one or more impurities, such as one or more impurities from recycled components. The technology also includes methods for forming such grain refiner products and methods for forming aluminum alloy articles using such grain refiner products. Surprisingly, this technology has found that one or more of the aforementioned problems can be solved by mechanically deforming the grain refiner product to a carefully controlled particle size (referred to herein as "grain refiner chips"). That is, the grain refiner chips according to this technology can reduce the necessary residence time, thereby reducing the formation of intermetallic compound particles with a particle size greater than or equal to about 50 μm. Furthermore, the grain refiner chips according to this technology can also exhibit a reduced TiAl3 phase particle size, thereby further reducing the size of intermetallic compound particles or TiAl3 particles in the final melt due to smaller nucleating particles.
[0016] Definitions and descriptions: As used herein, the terms “invention,” “the invention,” “this invention,” and “the present invention” are intended to refer to the entire subject matter of this patent application and the following claims. Statements containing these terms should not be construed as limiting the subject matter described herein or limiting the meaning or scope of the patent claims below.
[0017] As used herein, unless the context clearly indicates otherwise, “a” or “the” means both singular and plural referents.
[0018] As used herein, the thickness of a sheet is typically greater than about 15 mm. For example, a sheet may refer to an aluminum product having a thickness greater than about 15 mm, greater than about 20 mm, greater than about 25 mm, greater than about 30 mm, greater than about 35 mm, greater than about 40 mm, greater than about 45 mm, greater than about 50 mm, or greater than about 100 mm.
[0019] As used in this article, shate (also known as sheet board) typically has a thickness of about 4 mm to about 15 mm. For example, shate can have a thickness of about 4 mm, about 5 mm, about 6 mm, about 7 mm, about 8 mm, about 9 mm, about 10 mm, about 11 mm, about 12 mm, about 13 mm, about 14 mm or about 15 mm.
[0020] As used herein, sheet material generally refers to aluminum products having a thickness of less than about 4 mm. For example, sheet material may have a thickness of less than about 4 mm, less than about 3 mm, less than about 2 mm, less than about 1 mm, less than about 0.5 mm, or less than about 0.3 mm (e.g., about 0.2 mm).
[0021] As used herein, the term foil refers to alloy thicknesses in the range of up to about 0.2 mm (i.e., 200 micrometers (μm)). For example, foil thicknesses can be up to 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, or 200 μm.
[0022] This specification mentions alloys identified by aluminum industry designations such as "Series" or "5xxx". For information on the most commonly used numerical designation systems for naming and identifying aluminum and its alloys, see the Aluminum Association's "International Alloy Designations and Chemical Composition Limits for Wrought Aluminum and Wrought Aluminum Alloys" or "Registration Record of Aluminum Association Alloy Designations and Chemical Composition Limits for Aluminum Alloys in the Form of Castings and Ingots".
[0023] In this application, reference is made to alloy tempering or tempering. For the most commonly used descriptions of alloy tempering, see “American National Standard (ANSI) H35 Nomenclature System for Alloys and Tempering”. F tempering refers to manufactured aluminum alloys. O tempering refers to annealed aluminum alloys. Hxx tempering, also referred to herein as H tempering, refers to non-heat-treatable aluminum alloys that have been cold-rolled and may or may not have undergone heat treatment (e.g., annealing). Suitable H temperings include HX1, HX2, HX3, HX4, HX5, HX6, HX7, HX8, or HX9 temperings. T1 tempering refers to aluminum alloys cooled from hot working and subjected to natural aging (e.g., at room temperature). T2 tempering refers to aluminum alloys cooled from hot working, cold-worked, and subjected to natural aging. T3 tempering refers to aluminum alloys that have undergone solution heat treatment, cold working, and natural aging. T4 tempering refers to aluminum alloys that have undergone solution heat treatment and natural aging. T5 temper or tempered refers to aluminum alloys that have been cooled from hot working and undergone artificial aging (at high temperature). T6 temper or tempered refers to aluminum alloys that have undergone solution heat treatment and artificial aging. T7 temper or tempered refers to aluminum alloys that have undergone solution heat treatment and artificial aging. T8x temper or tempered refers to aluminum alloys that have undergone solution heat treatment, cold working, and artificial aging. T9 temper or tempered refers to aluminum alloys that have undergone solution heat treatment, artificial aging, and cold working. W temper or tempered refers to aluminum alloys after solution heat treatment.
[0024] As used herein, "room temperature" can mean from about 15°C to about 30°C, for example, about 15°C, about 16°C, about 17°C, about 18°C, about 19°C, about 20°C, about 21°C, about 22°C, about 23°C, about 24°C, about 25°C, about 26°C, about 27°C, about 28°C, about 29°C, or about 30°C.
[0025] As used herein, terms such as “cast metal products,” “cast products,” and “cast aluminum alloy products” are interchangeable and refer to products produced by direct cooling casting (including direct cooling co-casting) or semi-continuous casting, continuous casting (including, for example, using a twin-belt casting machine, twin-roll casting machine, block casting machine, or any other continuous casting machine), electromagnetic casting, hot-top casting, or any other casting method.
[0026] As used herein, the term "metal product" may appropriately refer to any cast product of suitable shape or size.
[0027] All ranges disclosed herein should be understood to encompass any and all subranges included therein. For example, the specified range “1 to 10” should be considered to include any and all subranges between the minimum value 1 and the maximum value 10 (and including the endpoints); that is, all subranges begin with a minimum value of 1 or greater (such as 1 to 6.1) and end with a maximum value of 10 or less (such as 5.5 to 10).
[0028] The following aluminum alloys are described in terms of elemental composition as a percentage by weight (wt%) of the total alloy weight. In certain instances of each alloy, the remainder is aluminum, and the maximum wt% of the total sum of impurities is 0.15%.
[0029] As used herein, the term recycled waste (e.g., recycled raw materials) can refer to a collection of recycled metals. Recycled waste can include materials recovered from any suitable source, such as from metal production facilities (e.g., metal casting facilities), from metal processing facilities (e.g., production facilities that use metal products to manufacture consumer products), or from post-consumer sources (e.g., regional recycling facilities). Certain aspects of this disclosure may be well suited for recycled waste from sources other than metal production facilities, as such recycled waste may contain mixtures of alloys or be mixed with other impurities or elements (e.g., paints or coatings). Recycled waste can refer to recycled aluminum, such as recycled aluminum sheet products (e.g., aluminum pots and pans), recycled cast aluminum products (e.g., aluminum grills and rims), UBC waste (e.g., beverage cans), aluminum wire, and other aluminum materials.
[0030] aluminum alloy This document describes aluminum alloys. As discussed above, aluminum alloys can be prepared from at least a portion of recycled waste. However, it should be understood that the alloys discussed herein may also contain one or more of the following alloying elements (also referred to as “impurities”) from independent sources, and in embodiments, may not contain any recycled components. Therefore, it should be understood that the following discussion and the amounts of various components can be obtained from recycled components or from alloy mixtures.
[0031] Nevertheless, in embodiments, the technology disclosed herein allows suitable casting products to be produced from modified liquid metal containing equal to or greater than about 5%, about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, about 80%, about 90%, about 92%, about 94%, about 96%, or about 98%, or any range or value thereof, of recycled waste. In other words, the casting products described herein may contain equal to or less than about 90%, about 80%, about 70%, about 60%, about 50%, about 40%, about 30%, about 20%, about 10%, about 8%, about 6%, about 4%, or about 2%, or any range or value thereof, of primary aluminum.
[0032] In some cases, recycled waste includes recycled aluminum scrap, such as UBC scrap. UBC scrap typically contains mixtures of metals from various alloys, such as metals from the tank body (e.g., 3104, 3004, or other 3xxx aluminum alloys) and the tank end (e.g., 5182 or other 5xxx aluminum alloys). Other modified liquid metals contain other mixtures of alloys, as well as mixtures containing primary aluminum.
[0033] Optionally, the modified liquid metal can be modified with one or more additional elements to prepare alloys. In some instances, it may be necessary to add additional magnesium (Mg) and / or other alloying elements to the modified liquid metal, which can produce alloys with improved castability of the liquid metal and improved metallurgical properties of the final product. For example, added Mg can increase the formability and strength of cast metal products. However, as discussed above, high Mg content has previously been problematic because it contributes to increased intermetallic compound particle size. However, using the methods discussed herein, in some instances, Mg can be added to the modified liquid metal to achieve a Mg percentage in the modified metal alloy of about 0.50% to about 7.0% based on the total weight of the alloy (e.g., about 1.5% to about 6.0%, about 2.0% to about 5.0%, about 2.5% to about 4.5%, or about 3.0% to about 4.0%). The percentage of Mg can be equal to or greater than approximately 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%. 3.9%, 4.0%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5.0%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6.0%, 6.1%, 6.2%, 6.3%, 6.4%, 6.5%, 6.6%, 6.7%, 6.8%, 6.9%, or 7.0%. In some cases, Mg can be added to modified liquid metal to achieve a Mg weight percentage of at least 1.5% and equal to or less than about 6.0%, 5.9%, 5.8%, 5.7%, 5.6%, 5.5%, 5.4%, 5.3%, 5.2%, 5.1%, 5.0%, 4.9%, 4.8%, 4.7%, 4.6%, 4.5%, 4.4%, 4.3%, 4.2%, 4.1%, 4.0%, 3.9%, 3.8%, 3.7%, 3.6%, 3.5%, 3.4%, 3.3%, 3.2%, 3.1%, or 3.0%.
[0034] In some instances, the metal alloys described herein may have the following elemental compositions as provided in Table 1.
[0035] Table 1
[0036] In some instances, the metal alloys described herein may have the following elemental compositions as provided in Table 2.
[0037] Table 2
[0038] In some instances, the metal alloys described herein may have the following elemental compositions as provided in Table 3.
[0039] Table 3
[0040] In some instances, the alloys described herein contain approximately 0.01% to approximately 1.0% (e.g., approximately 0.02% to approximately 1.0%, approximately 0.03% to approximately 0.9%, approximately 0.04% to approximately 0.8%, or approximately 0.05% to approximately 0.40%) of Cu based on the total weight of the alloy. For example, the alloy may contain 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, 0.20%, 0.21%, 0.22%, 0.23%, or 0.24% Cu. 0.25%, 0.26%, 0.27%, 0.28%, 0.29%, 0.30%, 0.31%, 0.32%, 0.33%, 0.34%, 0.35%, 0.36%, 0.37%, 0.38%, 0.39%, 0.40%, 0.41%, 0.42%, 0.43%, 0.44%, 0.45%, 0.46%, 0.47%, 0.48%, 0.49%, 0 0.50%, 0.51%, 0.52%, 0.53%, 0.54%, 0.55%, 0.56%, 0.57%, 0.58%, 0.59%, 0.60%, 0.61%, 0.62%, 0.63%, 0.64%, 0.65%, 0.66%, 0.67%, 0.68%, 0.69%, 0.70%, 0.71%, 0.72%, 0.73%, 0.74%, 0. 75%, 0.76%, 0.77%, 0.78%, 0.79%, 0.80%, 0.81%, 0.82%, 0.83%, 0.84%, 0.85%, 0.86%, 0.87%, 0.88%, 0.89%, 0.90%, 0.91%, 0.92%, 0.93%, 0.94%, 0.95%, 0.96%, 0.97%, 0.98%, 0.99%, or 1.0% Cu. All percentages are expressed by weight.
[0041] In some instances, the alloys described herein contain approximately 0.1% to approximately 0.8% (e.g., approximately 0.15% to approximately 0.7% or approximately 0.2% to approximately 0.6%) of iron (Fe) based on the total weight of the alloy. For example, the alloy may contain 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, 0.20%, 0.21%, 0.22%, 0.23%, 0.24%, 0.25%, 0.26%, 0.27%, 0.28%, 0.29%, 0.30%, 0.31%, 0.32%, 0.33%, 0.34%, 0.35%, 0.36%, 0.37%, 0.38%, 0.39%, 0.40%, 0.41%, 0.42%, 0.43%, 0.44% of the total weight of the alloy. %, 0.45%, 0.46%, 0.47%, 0.48%, 0.49%, 0.50%, 0.51%, 0.52%, 0.53%, 0.54%, 0.55%, 0.56%, 0.57%, 0.58%, 0.59%, 0.60%, 0.61%, 0.62%, 0.63%, 0.64%, 0.65%, 0.66%, 0.67%, 0.68%, 0.69%, 0.70%, 0.71%, 0.72%, 0.73%, 0.74%, 0.75%, 0.76%, 0.77%, 0.78%, 0.79%, 0.80% Fe. All expressed as weight percent.
[0042] In some instances, the alloys described herein contain approximately 0.50% to approximately 7.0% (e.g., approximately 1.0% to approximately 6.0%, approximately 2% to approximately 5.5%, approximately 2.5% to approximately 5.0%, or approximately 3.0% to approximately 4.75%) of Mg based on the total weight of the alloy. For example, the alloy may contain 0.51%, 0.52%, 0.53%, 0.54%, 0.55%, 0.56%, 0.57%, 0.58%, 0.59%, 0.60%, 0.61%, 0.62%, 0.63%, 0.64%, 0.65%, 0.66%, 0.67%, 0.68%, 0.69%, 0.70%, 0.71%, 0.72%, 0.73%, and 0.74% of Mg. 0.75%, 0.76%, 0.77%, 0.78%, 0.79%, 0.80%, 0.81%, 0.82%, 0.83%, 0.84%, 0.85%, 0.86%, 0.87%, 0.88%, 0.89%, 0.90%, 0.91%, 0.92%, 0.93%, 0.94%, 0.95%, 0.96%, 0.97%, 0.98%, 0.99%, 1 0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5.0%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6.0%, 6.1%, 6.2%, 6.3%, 6.4%, 6.5%, 6.6%, 6.7%, 6.8%, 6.9% or 7.0%. Mg. All values are expressed as a percentage by weight.
[0043] In some instances, the alloys described herein contain manganese (Mn) in amounts from about 0.01% to about 1.2% (e.g., from about 0.05% to about 1.0%, from about 0.1% to about 0.9%, or from about 0.2% to about 0.7%) based on the total weight of the alloy. For example, the alloy may contain 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, 0.20%, 0.21%, 0.22%, 0.23%, 0.24%, 0.25%, 0.26%, 0.27%, 0.28%, or 0.29% of the alloy's total weight. 0.30%, 0.31%, 0.32%, 0.33%, 0.34%, 0.35%, 0.36%, 0.37%, 0.38%, 0.39%, 0.40%, 0.41%, 0.42%, 0.43%, 0.44%, 0.45%, 0.46%, 0.47%, 0.48%, 0.49%, 0.50%, 0.51%, 0.52%, 0.53%, 0.54%, 0.55%, 0.56%, 0.57%, 0.58%, 0.59%, 0 0.60%, 0.61%, 0.62%, 0.63%, 0.64%, 0.65%, 0.66%, 0.67%, 0.68%, 0.69%, 0.70%, 0.71%, 0.72%, 0.73%, 0.74%, 0.75%, 0.76%, 0.77%, 0.78%, 0.79%, 0.80%, 0.81%, 0.82%, 0.83%, 0.84%, 0.85%, 0.86%, 0.87%, 0.88%, 0.89%, 0. 90%, 0.91%, 0.92%, 0.93%, 0.94%, 0.95%, 0.96%, 0.97%, 0.98%, 0.99%, 1.0%, 1.01%, 1.02%, 1.03%, 1.04%, 1.05%, 1.06%, 1.07%, 1.08%, 1.09%, 1.10%, 1.11%, 1.12%, 1.13%, 1.14%, 1.15%, 1.16%, 1.17%, 1.18%, 1.19%, or 1.20% Mn. All expressed as weight percent.
[0044] In some instances, the alloys described herein contain an amount of Si up to about 1.5% by weight (e.g., about 0.01% to about 1.0%, about 0.02% to about 0.5%, or about 0.03% to about 0.1%) based on the total weight of the alloy. For example, the alloy may contain 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, 0.20%, 0.21%, 0.22%, 0.23%, 0.24%, 0.25%, 0.26%, 0.27%, 0.28%, 0.29%, 0.30%, 0.31%, 0.32%, 0.33%, 0.34%, 0.35%, 0.36%, 0.3%... 7%, 0.38%, 0.39%, 0.40%, 0.41%, 0.42%, 0.43%, 0.44%, 0.45%, 0.46%, 0.47%, 0.48%, 0.49%, 0.50%, 0.51%, 0.52%, 0.53%, 0.54%, 0.55%, 0.56%, 0.57%, 0.58%, 0.59%, 0.60%, 0.61%, 0.62%, 0.63%, 0.64%, 0.65%, 0.66%, 0.67%, 0.68%, 0.69%, 0.70%, 0.71%, 0.72%, 0.73%, 0.74%, 0 0.75%, 0.76%, 0.77%, 0.78%, 0.79%, 0.80%, 0.81%, 0.82%, 0.83%, 0.84%, 0.85%, 0.86%, 0.87%, 0.88%, 0.89%, 0.90%, 0.91%, 0.92%, 0.93%, 0.94%, 0.95%, 0.96%, 0.97%, 0.98%, 0.99%, 1.0%, 1.01%, 1.02%, 1.03%, 1.04%, 1.05%, 1.06%, 1.07%, 1.08%, 1.09%, 1.10%, 1.11%, 1.12% 1.13%, 1.14%, 1.15%, 1.16%, 1.17%, 1.18%, 1.19%, 1.20%, 1.21%, 1.22%, 1.23%, 1.24%, 1.25%, 1.26%, 1.27%, 1.28%, 1.29%, 1.30%, 1.31%, 1.32%, 1.33%, 1.34%, 1.35%, 1.36%, 1.37%, 1.38%, 1.39%, 1.40%, 1.41%, 1.42%, 1.43%, 1.44%, 1.45%, 1.46%, 1.47%, 1.48%, 1.49%, or 1.50% Si.In some cases, the alloy contains no Si (i.e., 0%). All figures are expressed as a percentage by weight.
[0045] In some instances, the alloys described herein contain up to about 0.2% (e.g., about 0.01% to about 0.15% or about 0.02% to about 0.1%) of titanium (Ti) based on the total weight of the alloy. For example, the alloy may contain 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, or 0.20% Ti. In some cases, Ti is absent from the alloy (i.e., 0%). All figures are expressed as a percentage by weight.
[0046] In some instances, the alloys described herein contain an amount of zinc (Zn) of about 0% to about 8.0% (e.g., about 0.01% to about 5.0% or about 0.02% to about 1.0%) based on the total weight of the alloy.For example, the alloy may contain 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, 0.20%, 0.21%, 0.22%, 0.23%, 0.24%, 0.25%, 0.26%, 0.27%, 0.28%, 0.29%, 0.30%, 0.31%, 0.32%, 0.33%, 0.34%, 0.35%, 0.36%, 0.37%, 0.38%, 0. 39%, 0.40%, 0.41%, 0.42%, 0.43%, 0.44%, 0.45%, 0.46%, 0.47%, 0.48%, 0.49%, 0.50%, 0.51%, 0.52%, 0.53%, 0.54%, 0.55%, 0.56%, 0.57%, 0.58%, 0.59%, 0.60%, 0.61%, 0.62%, 0.63%, 0.64%, 0.65%, 0.66%, 0.67%, 0.68%, 0.69%, 0.70%, 0.71%, 0.72%, 0.73%, 0.74%, 0.75%, 0.76%, 0.77%, 0.78%, 0 0.79%, 0.80%, 0.81%, 0.82%, 0.83%, 0.84%, 0.85%, 0.86%, 0.87%, 0.88%, 0.89%, 0.90%, 0.91%, 0.92%, 0.93%, 0.94%, 0.95%, 0.96%, 0.97%, 0.98%, 0.99%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%. 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5.0%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6.0%, 6.1%, 6.2%, 6.3%, 6.4%, 6.5%, 6.6%, 6.7%, 6.8%, 6.9%, 7.0%, 7.1%, 7.2%, 7.3%, 7.4%, 7.5%, 7.6%, 7.7%, 7.8%, 7.9%, or 8.0% Zn. In some cases, Zn is absent in the alloy (i.e., 0%). All figures are expressed as a percentage by weight.
[0047] In some instances, the alloys described herein contain up to about 0.30% (e.g., about 0.01% to about 0.25% or about 0.02% to about 0.1%) of chromium (Cr) based on the total weight of the alloy. For example, the alloy may contain 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, 0.20%, 0.21%, 0.22%, 0.23%, 0.24%, 0.25%, 0.26%, 0.27%, 0.28%, 0.29%, or 0.30% Cr. In some cases, Cr is absent in the alloy (i.e., 0%). All figures are expressed as a percentage by weight.
[0048] In some instances, the alloys described herein contain approximately 0% to approximately 0.15% (e.g., approximately 0.01% to approximately 0.1% or approximately 0.02% to approximately 0.05%) of zirconium (Zr) based on the total weight of the alloy. For example, the alloy may contain 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, or 0.15% Zr. In some cases, Zr is absent from the alloy (i.e., 0%). All figures are expressed as a percentage by weight.
[0049] In some instances, the alloys described herein contain vanadium (V) in amounts from about 0% to about 0.15% (e.g., from about 0.01% to about 0.1% or from about 0.02% to about 0.05%) based on the total weight of the alloy. For example, the alloy may contain 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, or 0.15% V. In some cases, V is absent from the alloy (i.e., 0%). All figures are expressed as a percentage by weight.
[0050] In some instances, the alloys described herein contain calcium (Ca) in amounts from about 0% to about 0.15% (e.g., from about 0.003% to about 0.1%, about 0.01% to about 0.1%, or about 0.02% to about 0.05%) based on the total weight of the alloy. For example, the alloy may contain 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, or 0.15% Ca. In some cases, Ca is absent in the alloy (i.e., 0%). All figures are expressed as a percentage by weight. However, in the implementation scheme, the alloy discussed herein may contain one or more of calcium, vanadium, and titanium.
[0051] In some instances, the alloys described herein contain approximately 0% to approximately 0.15% (e.g., approximately 0.003% to approximately 0.1%, approximately 0.01% to approximately 0.1%, or approximately 0.02% to approximately 0.05%) of strontium (Sr) based on the total weight of the alloy. For example, the alloy may contain 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, or 0.15% Sr. In some cases, Sr is absent from the alloy (i.e., 0%). All figures are expressed as a percentage by weight.
[0052] In some instances, the alloys described herein contain beryllium (Be) in amounts from about 0% to about 0.15% (e.g., from about 0.003% to about 0.1%, from about 0.01% to about 0.1%, or from about 0.02% to about 0.05%) based on the total weight of the alloy. For example, the alloy may contain 0.0001%, 0.0002%, 0.0003%, 0.0004%, 0.0005%, 0.0006%, 0.0007%, 0.0008%, 0.0009%, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, or 0.15% Be. In some cases, Be is absent in the alloy (i.e., 0%). All are expressed as a percentage by weight.
[0053] Optionally, the alloy compositions described herein may also contain other trace elements, sometimes referred to as impurities, in amounts of 0.05% or less, 0.04% or less, 0.03% or less, 0.02% or less, or 0.01% or less. These impurities may include, but are not limited to, Sn, Ga, Bi, Na, Pb, Li, W, Mo, Ni, B, C, or combinations thereof. Thus, Sn, Ga, Bi, Na, Pb, Li, W, Mo, Ni, B, or C may be present in the alloy in amounts of 0.05% or less, 0.04% or less, 0.03% or less, 0.02% or less, or 0.01% or less. In some cases, the sum of all impurities does not exceed 0.15% (e.g., 0.10%). All figures are expressed as weight percent. The remaining percentage of the alloy is aluminum.
[0054] In some instances, suitable alloys for the alloys described herein may be 1xxx series aluminum alloys, 2xxx series aluminum alloys, 3xxx series aluminum alloys, 4xxx series aluminum alloys, 5xxx series aluminum alloys, 6xxx series aluminum alloys, 7xxx series aluminum alloys, 8xxx series aluminum alloys, or any combination thereof. 1xxx, 2xxx, 3xxx, 4xxx, 5xxx, 6xxx, 7xxx, or 8xxx series aluminum alloys may be modified to include certain amounts of Mg, Cu, and / or Si as described above.
[0055] Suitable 1xxx series aluminum alloys for use with the alloys described herein include, for example, AA1050, AA1060, AA1070, AA1100, AA1100A, AA1200, AA1200A, AA1300, AA1110, AA1120, AA1230, AA1230A, AA1235, AA1435, AA1145, AA1345, AA1445, AA1150, AA1350, AA1350A, AA1450, AA1370, AA1275, AA1185, AA1285, AA1385, AA1188, AA1190, AA1290, AA1193, AA1198 and AA1199.
[0056] Suitable 2xxx series aluminum alloys for use with the alloys described herein include, for example, AA2001, A2002, AA2004, AA2005, AA2006, AA2007, AA2007A, AA2007B, AA2008, AA2009, AA2010, AA2011, AA2011A, AA2111, AA2111A, AA2111B, AA2012, AA2013, AA2014, and AA2014A. , AA2214, AA2015, AA2016, AA2017, AA2017A, AA2117, AA2018, AA2218, AA2618, AA2618A, AA2219, AA231 9. AA2419, AA2519, AA2021, AA2022, AA2023, AA2024, AA2024A, AA2124, AA2224, AA2224A, AA2324, AA242 4. AA2524, AA2624, AA2724, AA2824, AA2025, AA2026, AA2027, AA2028, AA2028A, AA2028B, AA2028C, AA2 029, AA2030, AA2031, AA2032, AA2034, AA2036, AA2037, AA2038, AA2039, AA2139, AA2040, AA2041, AA20 44. AA2045, AA2050, AA2055, AA2056, AA2060, AA2065, AA2070, AA2076, AA2090, AA2091, AA2094, AA209 5. AA2195, AA2295, AA2196, AA2296, AA2097, AA2197, AA2297, AA2397, AA2098, AA2198, AA2099 and AA2199.
[0057] Suitable 3xxx series aluminum alloys for use with the alloys described herein include, for example, AA3002, AA3102, AA3003, AA3103, AA3103A, AA3103B, AA3203, AA3403, AA3004, AA3004A, AA3104, AA3204, AA3304, AA3005, AA3005A, AA3105, AA3105A, AA3105B, and AA3007. AA3107, AA3207, AA3207A, AA3307, AA3009, AA3010, AA3110, AA3011, AA3012, AA3012A, AA3013, AA3014, AA3015, AA3016, AA3017, AA3019, AA3020, AA3021, AA3025, AA3026, AA3030, AA3130 and AA3065.
[0058] Suitable 4xxx series aluminum alloys for use with the alloys described herein include, for example, AA4004, AA4104, AA4006, AA4007, AA4008, AA4009, AA4010, AA4013, AA4014, AA4015, AA4015A, AA4115, AA4016, AA4017, AA4018, AA4019, AA4020, AA4021, AA4026, AA4032, AA4043, AA4043A, AA4143, AA4343, AA4643, AA4943, AA4044, AA4045, AA4145, AA4145A, AA4046, AA4047, AA4047A and AA4147.
[0059] Suitable 5xxx series aluminum alloys for use with the alloys described herein include, for example, AA5005, AA5005A, AA5205, AA5305, AA5505, AA5605, AA5006, AA5106, AA5010, AA5110, AA5110A, AA5210, AA5310, AA5016, AA5017, AA5018, AA5018A, AA5019, AA5019A, AA5119, AA5119A, AA5021, AA... 5022, AA5023, AA5024, AA5026, AA5027, AA5028, AA5040, AA5140, AA5041, AA5042, AA5043, AA5049, AA5149, AA524 9. AA5349, AA5449, AA5449A, AA5050, AA5050A, AA5050C, AA5150, AA5051, AA5051A, AA5151, AA5251, AA5251A, AA5 351, AA5451, AA5052, AA5252, AA5352, AA5154, AA5154A, AA5154B, AA5154C, AA5254, AA5354, AA5454, AA5554, AA 5654, AA5654A, AA5754, AA5854, AA5954, AA5056, AA5356, AA5356A, AA5456, AA5456A, AA5456B, AA5556, AA5556A, AA5556B, AA5556C, AA5257, AA5457, AA5557, AA5657, AA5058, AA5059, AA5070, AA5180, AA5180A, AA5082, AA5182, AA5083, AA5183, AA5183A, AA5283, AA5283A, AA5283B, AA5383, AA5483, AA5086, AA5186, AA5087, AA5187 and AA5088.
[0060] Suitable 6xxx series aluminum alloys for use with the alloys described herein include, for example, AA6101, AA6101A, AA6101B, AA6201, AA6201A, AA6401, AA6501, AA6002, AA6003, AA6103, AA6005, AA6005A, AA6005B, AA6005C, AA6105, AA6205, AA6305, AA6006, AA6106, AA6206, AA6306, and AA6008. , AA6009, AA6010, AA6110, AA6110A, AA6011, AA6111, AA6012, AA6012A, AA6013, AA6113, AA6014, AA6015, AA6016 ,AA6016A,AA6116,AA6018,AA6019,AA6020,AA6021,AA6022,AA6023,AA6024,AA6025,AA6026,AA6027,AA6028, AA6031, AA6032, AA6033, AA6040, AA6041, AA6042, AA6043, AA6151, AA6351, AA6351A, AA6451, AA6951, AA6053, A A6055, AA6056, AA6156, AA6060, AA6160, AA6260, AA6360, AA6460, AA6460B, AA6560, AA6660, AA6061, AA6061A, A A6261, AA6361, AA6162, AA6262, AA6262A, AA6063, AA6063A, AA6463, AA6463A, AA6763, A6963, AA6064, AA6064A, AA6065, AA6066, AA6068, AA6069, AA6070, AA6081, AA6181, AA6181A, AA6082, AA6082A, AA6182, AA6091 and AA6092.
[0061] Suitable 7xxx series aluminum alloys for use with the alloys described herein include, for example, AA7019, AA7020, AA7021, AA7039, AA7072, AA7075, AA7085, AA7108, AA7108A, AA7015, AA7017, AA7018, AA7019A, AA7024, AA7025, AA7028, AA7030, AA7031, AA7035, AA7035A, AA7046, AA7046A, AA7003, AA7004, AA7005, AA7009, AA7010, AA7011, AA7012, AA7014, AA7016, AA7116, AA7122, AA7023, AA7026, AA7029, AA7129, AA72 29. AA7032, AA7033, AA7034, AA7036, AA7136, AA7037, AA7040, AA7140, AA7041, AA7049, AA7049A, AA7149, AA7249, AA7349, AA7449, AA7050, AA7050A, AA7150, AA7250, AA7055, A A7155, AA7255, AA7056, AA7060, AA7064, AA7065, AA7068, AA7168, AA7175, AA7475, AA7076, AA7178, AA7278, AA7278A, AA7081, AA7181, AA7185, AA7090, AA7093, AA7095 and AA7099.
[0062] Suitable 8xxx series aluminum alloys for use with the alloys described herein include, for example, AA8005, AA8006, AA8007, AA8008, AA8010, AA8011, AA8011A, AA8111, AA8211, AA8112, AA8014, AA8015, AA8016, AA8017, AA8018, AA8019, AA8021, AA8021A, AA8021B, AA8022, AA8023, AA8024, AA8025, AA8026, AA8030, AA8130, AA8040, AA8050, AA8150, AA8076, AA8076A, AA8176, AA8077, AA8177, AA8079, AA8090, AA8091, and AA8093.
[0063] Nevertheless, in the implementation, the aluminum alloy can be a 5xxx aluminum alloy, such as 5182.
[0064] Various products comprising the alloys described herein can be produced. In some instances, the prepared products comprising the alloys described herein may be coated products comprising a core layer and one or more cladding layers. The core layer has a first side and a second side, and one or more cladding layers may be bonded to the first side or the second side of the core layer. In some instances, the core layer is clad on only one side (i.e., one cladding layer is present in the coated aluminum alloy product). In other instances, the core layer is clad on both sides (i.e., two cladding layers are present in the coated aluminum alloy product).
[0065] For example, the cladding layer can be attached to the core layer in the following ways: direct cooling co-casting (i.e., melt casting), as described, for example, in U.S. Patent Nos. 7,748,434 and 8,927,113, which are incorporated herein by reference in their entirety; hot-rolled and cold-rolled composite casting ingots, as described in U.S. Patent No. 7,472,740, which is incorporated herein by reference in its entirety; or rolling bonding to achieve the desired metallurgical bonding between the core and the cladding.
[0066] The alloys described herein can be used as a core layer or as one or more cladding layers. Optionally, one or more cladding layers may comprise 1xxx series aluminum alloys, 2xxx series aluminum alloys, 3xxx series aluminum alloys, 4xxx series aluminum alloys, 5xxx series aluminum alloys, 6xxx series aluminum alloys, 7xxx series aluminum alloys, or 8xxx series aluminum alloys. In some instances, the clad product is prepared from an alloy as described herein as a core and one or both of 5xxx or 6xxx series aluminum alloys as cladding layers.
[0067] The aluminum alloy products described herein can be in any suitable specification. The alloy can be cast and machined into various sizes and thicknesses, such as foil (e.g., less than about 0.20 mm), sheet (e.g., about 0.20 mm to 4.0 mm), sheet (e.g., about 4.0 mm to 15.0 mm), or plate (e.g., greater than about 15.0 mm), but other thicknesses and ranges are also possible. In some instances, the aluminum alloy products described herein may be supplied and delivered to customers or end users in intermediate specifications (e.g., specifications that will be further reduced as needed by the customer or end user). In some instances, the aluminum alloy products described herein may be supplied and delivered to customers or end users in final specifications (e.g., specifications that will not be further reduced by the customer or end user).
[0068] Products containing the alloy described herein may have a hydrogen content of 0.15 ml / 100 g or less (e.g., equal to or less than 0.10 ml / 100 g, equal to or less than 0.08 ml / 100 g, or equal to or less than 0.06 ml / 100 g). For example, the amount of hydrogen contained in an aluminum alloy product may be equal to or less than approximately 0.15 ml / 100 g, 0.14 ml / 100 g, 0.13 ml / 100 g, 0.12 ml / 100 g, 0.11 ml / 100 g, 0.1 ml / 100 g, 0.09 ml / 100 g, 0.08 ml / 100 g, 0.07 ml / 100 g, 0.06 ml / 100 g, 0.05 ml / 100 g, 0.04 ml / 100 g, 0.03 ml / 100 g, 0.02 ml / 100 g, or 0.01 ml / 100 g. Optionally, the hydrogen content in the product may be at least 0.08 ml / 100 g. For example, the hydrogen content can be from 0.08 mL / 100 g to 0.25 mL / 100 g, 0.1 mL / 100 g to 0.20 mL / 100 g, or 0.12 mL / 100 g to 0.18 mL / 100 g. The amount of dissolved hydrogen present affects the properties of the resulting metallic product. During casting, dissolved hydrogen can affect the castability of the metallic product (e.g., resistance to hot cracking) and the mechanical properties of the resulting metallic product (e.g., flexural strength, toughness, fatigue strength, maximum elongation, impact resistance, surface quality, corrosion resistance, and other properties). Dissolved hydrogen can affect solidification and can lead to porosity in the cast metallic product. Products prepared from the alloys described herein with the above-mentioned hydrogen contents are not subject to these adverse effects.
[0069] The aluminum alloy products described herein contain intermetallic compound particles containing aluminum (Al), silicon (Si), magnesium (Mg), vanadium (V), calcium (Ca), strontium (Sr), titanium (Ti), beryllium (Be), chromium (Cr), and / or manganese (Mn), such as (in embodiments) one or more of aluminum (Al), magnesium (Mg), titanium (Ti), vanadium (V), and / or calcium (Ca). Surprisingly, however, due to the methods and grain refiner debris discussed herein, the intermetallic compound particles in the aluminum alloy products can have a length (e.g., equivalent diameter or maximum size) of less than or about 50 µm, such as less than or about 45 µm, such as less than or about 40 µm, such as less than or about 35 µm, such as less than or about 30 µm, or ranging from about 1 µm to about 50 µm (e.g., about 5 µm to about 45 µm or about 10 µm to about 40 µm). In embodiments, the intermetallic compound particles can be Al particles nucleated individually or by one or more TiAl3 particles. x Mg y Ti x V tCa v Particles. Nevertheless, this technique has found that the methods and grain refiner debris discussed herein can prevent the formation of intermetallic compound particles with a length or maximum size greater than 50 μm.
[0070] In embodiments, the intermetallic compound particles may contain Mg in amounts from about 1.0% to about 10.0% (e.g., about 2.0% to about 9.5%, about 2.5% to about 9.0%, about 3.0% to about 8.5%, or about 3.5% to about 8.0%) based on the total weight of the alloy. For example, the intermetallic compound particles may contain 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, and 4.8% of the total alloy weight. 4.9%, 5.0%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6.0%, 6.1%, 6.2%, 6.3%, 6.4%, 6.5%, 6.6%, 6.7%, 6.8%, 6.9%, 7.0%, 7.1%, 7.2%, 7.3%, 7.4%, 7.5%, 7.6%, 7.7%, 7.8%, 7.9%, 8.0%, 8.1%, 9.2%, 9.3%, 9.4%, 9.5%, 9.6%, 9.7%, 9.8%, 9.9% or 10.0% Mg. All expressed as weight percent.
[0071] In embodiments, the intermetallic compound particles may contain approximately 0.50% to approximately 7.0% (e.g., approximately 1.0% to approximately 6.0%, approximately 2% to approximately 5.5%, approximately 2.5% to approximately 5.0%, or approximately 3.0% to approximately 4.75%) of Ti based on the total weight of the alloy. For example, the intermetallic compound particles may contain 0.51%, 0.52%, 0.53%, 0.54%, 0.55%, 0.56%, 0.57%, 0.58%, 0.59%, 0.60%, 0.61%, 0.62%, 0.63%, 0.64%, 0.65%, 0.66%, 0.67%, 0.68%, 0.69%, 0.70%, 0.71%, 0.72%, 0.73%, 0. 0.74%, 0.75%, 0.76%, 0.77%, 0.78%, 0.79%, 0.80%, 0.81%, 0.82%, 0.83%, 0.84%, 0.85%, 0.86%, 0.87%, 0.88%, 0.89%, 0.90%, 0.91%, 0.92%, 0.93%, 0.94%, 0.95%, 0.96%, 0.97%, 0.98%, 0.99% %, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4 0.0%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5.0%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6.0%, 6.1%, 6.2%, 6.3%, 6.4%, 6.5%, 6.6%, 6.7%, 6.8%, 6.9%, or 7.0% Ti. All are expressed as a percentage by weight.
[0072] In an embodiment, the intermetallic compound particles may contain an amount of V based on about 0.50% to about 6.0% (e.g., about 1.0% to about 5.5%, about 2% to about 5.0%, about 2.5% to about 4.5%, or about 3.0% to about 4.75%) of the total weight of the alloy. For example, intermetallic compound particles may contain 0.51%, 0.52%, 0.53%, 0.54%, 0.55%, 0.56%, 0.57%, 0.58%, 0.59%, 0.60%, 0.61%, 0.62%, 0.63%, 0.64%, 0.65%, 0.66%, 0.67%, 0.68%, 0.69%, 0.70%, 0.71%, 0.72%, 0.73%, 0.74%, 0.75%, 0.76%, 0.77%, 0.78%, 0.79%, 0.80%, 0.81%, 0.82%, 0.83%, 0.84%, 0.85%, 0.86%, 0.87%, 0.88%, 0.89%, 0.90%, 0.91%, 0.92%, 0.93%, 0.94%, 0.9 5%, 0.96%, 0.97%, 0.98%, 0.99%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5.0%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9% or 6.0% V. All expressed as a percentage by weight.
[0073] In embodiments, the intermetallic compound particles may contain approximately 0.10% to approximately 5.0% (e.g., approximately 0.5% to approximately 4.5%, approximately 1.0% to approximately 4.0%, approximately 1.5% to approximately 3.5%, or approximately 2.0% to approximately 3.0%) of Ca based on the total weight of the alloy. For example, the intermetallic compound particles may contain 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, 0.20%, 0.21%, 0.22%, 0.23%, 0.24%, 0.25%, 0.26%, 0.27%, 0.28%, 0.29%, 0.30%, 0.31%, 0.32%, 0.33%, 0.34%, 0.35%, 0.36%, 0.37%, and 0.38% of Ca. 0.39%, 0.40%, 0.41%, 0.42%, 0.43%, 0.44%, 0.45%, 0.46%, 0.47%, 0.48%, 0.49%, 0.51%, 0.52%, 0.53%, 0.54%, 0.55%, 0.56%, 0.57%, 0.58%, 0.59%, 0.60%, 0.61%, 0.62%, 0.63%, 0.64%, 0.65%, 0.66%, 0.67%, 0.68%, 0.69%, 0.70%, 0. 71%, 0.72%, 0.73%, 0.74%, 0.75%, 0.76%, 0.77%, 0.78%, 0.79%, 0.80%, 0.81%, 0.82%, 0.83%, 0.84%, 0.85%, 0.86%, 0.87%, 0.88%, 0.89%, 0.90%, 0.91%, 0.92%, 0.93%, 0.94%, 0.95%, 0.96%, 0.97%, 0.98%, 0.99%, 1.0%, 1.1%, 1.2%, 1 0.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9% or 5.0% Ca. All expressed as a percentage by weight.
[0074] In embodiments, the intermetallic compound particles may contain an amount of Cr of about 0% to about 1.0% (e.g., about 0.01% to about 0.5% or about 0.02% to about 0.1%) based on the total weight of the alloy. For example, the intermetallic compound particles may contain 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, 0.20%, 0.21%, 0.22%, 0.23%, 0 0.24%, 0.25%, 0.26%, 0.27%, 0.28%, 0.29%, 0.30%, 0.31%, 0.32%, 0.33%, 0.34%, 0.35%, 0.36%, 0.37%, 0.38%, 0.39%, 0.40%, 0.41%, 0.42%, 0.43%, 0.44%, 0.45%, 0.46%, 0.47%, 0.48%, 0.49% %, 0.50%, 0.51%, 0.52%, 0.53%, 0.54%, 0.55%, 0.56%, 0.57%, 0.58%, 0.59%, 0.60%, 0.61%, 0.62%, 0.63%, 0.64%, 0.65%, 0.66%, 0.67%, 0.68%, 0.69%, 0.70%, 0.71%, 0.72%, 0.73%, 0.74%, 0 0.75%, 0.76%, 0.77%, 0.78%, 0.79%, 0.80%, 0.81%, 0.82%, 0.83%, 0.84%, 0.85%, 0.86%, 0.87%, 0.88%, 0.89%, 0.90%, 0.91%, 0.92%, 0.93%, 0.94%, 0.95%, 0.96%, 0.97%, 0.98%, 0.99%, or 1.0% Cr. In some cases, Cr is absent in the intermetallic compound particles (i.e., 0%). All are expressed as weight percent.
[0075] In embodiments, the intermetallic compound particles may contain an amount of Mn of about 0% to about 1.0% (e.g., about 0.01% to about 0.5% or about 0.02% to about 0.1%) based on the total weight of the alloy. For example, the intermetallic compound particles may contain 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, 0.20%, 0.21%, 0.22%, 0.23%, 0. 0.24%, 0.25%, 0.26%, 0.27%, 0.28%, 0.29%, 0.30%, 0.31%, 0.32%, 0.33%, 0.34%, 0.35%, 0.36%, 0.37%, 0.38%, 0.39%, 0.40%, 0.41%, 0.42%, 0.43%, 0.44%, 0.45%, 0.46%, 0.47%, 0.48%, 0.49% %, 0.50%, 0.51%, 0.52%, 0.53%, 0.54%, 0.55%, 0.56%, 0.57%, 0.58%, 0.59%, 0.60%, 0.61%, 0.62%, 0.63%, 0.64%, 0.65%, 0.66%, 0.67%, 0.68%, 0.69%, 0.70%, 0.71%, 0.72%, 0.73%, 0.74%, 0 0.75%, 0.76%, 0.77%, 0.78%, 0.79%, 0.80%, 0.81%, 0.82%, 0.83%, 0.84%, 0.85%, 0.86%, 0.87%, 0.88%, 0.89%, 0.90%, 0.91%, 0.92%, 0.93%, 0.94%, 0.95%, 0.96%, 0.97%, 0.98%, 0.99%, or 1.0% Mn. In some cases, Mn is absent in the intermetallic compound particles (i.e., 0%). All are expressed as weight percent.
[0076] In the implementation scheme, the remainder of the intermetallic compound particles may be aluminum.
[0077] In some cases, the metal products described herein may have a yield strength of at least about 100 MPa. For example, the metal products described herein may have a yield strength of about 100 MPa to about 300 MPa (e.g., about 150 MPa to about 250 MPa). In some cases, the yield strength may be about 100 MPa, 110 MPa, 120 MPa, 130 MPa, 140 MPa, 150 MPa, 160 MPa, 170 MPa, 180 MPa, 190 MPa, 200 MPa, 210 MPa, 220 MPa, 230 MPa, 240 MPa, 250 MPa, 260 MPa, 270 MPa, 280 MPa, 290 MPa, or 300 MPa.
[0078] In some cases, the metal products described herein may have an ultimate tensile strength of at least about 210 MPa. For example, the metal products described herein may have an ultimate tensile strength of about 210 MPa to about 350 MPa (e.g., about 250 MPa to about 325 MPa). In some cases, the ultimate tensile strength may be about 210 MPa, 220 MPa, 230 MPa, 240 MPa, 250 MPa, 260 MPa, 270 MPa, 280 MPa, 290 MPa, 300 MPa, 310 MPa, 320 MPa, 330 MPa, 340 MPa, or 350 MPa.
[0079] In some cases, the metal products described herein may have a uniform elongation of at least about 18%. For example, the metal products described herein may have a uniform elongation of about 18% to about 25% (e.g., about 19% to about 23%). In some cases, the uniform elongation may be about 18%, 18.5%, 19%, 19.5%, 20%, 20.5%, 21%, 21.5%, 22%, 22.5%, 23%, 23.5%, 24%, 24.5%, or 25%.
[0080] In some cases, the metal products described herein may have a total elongation of at least about 20.5%. For example, the metal products described herein may have a total elongation of about 20.5% to about 27.5% (e.g., about 22% to about 26%). In some cases, the total elongation may be about 20.5%, 21%, 21.5%, 22%, 22.5%, 23%, 23.5%, 24%, 24.5%, 25%, 25.5%, 26%, 26.5%, 27%, or 27.5%.
[0081] Preparation method The alloys discussed herein (which may contain one or more impurities) can be used to cast a variety of metal casting products, such as billets, ingots, or strips. Prior to casting, grain refiner debris, as discussed herein, is introduced into the liquid metal. As discussed above, the grain refiner debris decreases in size when subjected to simultaneous or sequential mechanical deformation. That is, this technique has surprisingly found that the unique combination of particle size and particle deformation provides unique benefits to the melt, even in the presence of sensitizing impurities (e.g., impurities that readily form intermetallic compound particles, particularly in the presence of grain refiner products). After the introduction of the grain refiner debris, the liquid metal may optionally be degassed to reduce the amount of hydrogen dissolved in the liquid metal. In some cases, degassed ...
[0082] Although the melt can be optionally degassed and filtered using a metal filter, the alloy described herein can be cast using any suitable casting method known to those skilled in the art. Surprisingly, compared to conventional casting processes, the residence time of the melt after the introduction of grain refiner debris is maintained or even reduced because the grain refiner debris interacts more completely in a shorter time, even in the presence of a large weight percentage of impurities. This is surprising because previously, grain refiner products required additional residence time in the presence of high weight percentages of impurities.
[0083] As some non-limiting examples, the casting process may include direct cooling (DC) casting or continuous casting (CC) casting. A direct cooling casting system may include a mold cavity and a retractable base block. As the molten metal solidifies in the mold cavity, the base block may retract from the mold cavity to support the solidified ingot (e.g., an embryonic ingot), because the ingot grows continuously in length due to the metal solidifying at its surface and the ingot continuously and completely solidifies. A continuous casting system may include a pair of moving opposing casting surfaces (e.g., moving opposing belts, rolls, or blocks), a casting cavity located between these moving opposing casting surfaces, and a molten metal ejector. The molten metal ejector may have end openings through which molten metal exits the ejector and is ejected into the casting cavity. Certain aspects of this disclosure may relate to continuous casting using a twin-belt continuous casting apparatus or a twin-roll continuous casting apparatus.
[0084] After casting, the metal product (e.g., metal sheet, plate, or other cast product) can be rolled to the desired specifications. Metal products cast from alloys as disclosed herein can have higher concentrations of alloying elements and / or impurities than usual. Conventional rolling techniques involve hot rolling followed by cold rolling. Hot rolling is performed at temperatures above the recrystallization temperature of the metal, while cold rolling is performed at temperatures below the recrystallization temperature. Because cold rolling involves deforming the metal at temperatures below the recrystallization temperature, the metal undergoes strain hardening by forming dislocations within the metal matrix.
[0085] Optionally, the metal products described herein may be delivered in any suitable specification as described herein. For example, the metal products may be delivered to customers (e.g., original equipment manufacturers) or any other suitable end users in intermediate or final specifications. In some cases, hot-rolled to specification may include receiving metal products from direct casting units and / or continuous casting units, but this is not always the case.
[0086] These illustrative embodiments are provided to introduce the general subject matter discussed herein and are not intended to limit the scope of the disclosed concepts. Various additional features and embodiments are described in the following sections with reference to the accompanying drawings, in which similar numerals denote similar elements, and directional descriptions are used to describe illustrative embodiments but, as with the illustrative embodiments, should not be used to limit this disclosure. Elements included in the illustrations herein may not be drawn to scale.
[0087] Figure 1 This is a flowchart depicting a process 100 for casting and hot rolling a metal product that may contain recycled scrap, according to certain aspects of this disclosure. At block 102, a melt is formed from a melt precursor, which may contain primary aluminum and / or recycled scrap as discussed above. The melt precursor can be melted in any suitable container, such as a rotary kiln, crucible furnace, or any other suitable heating device. The liquid metal produced from the melt precursor may contain alloying elements that make the liquid metal a non-standard alloy, such as alloys not typically used for beverage parts (e.g., can ends or can bodies) or automotive parts (e.g., automotive hood liners), such as when utilizing recycled scrap.
[0088] Grain refiner debris may be formed at block 103, sequentially or simultaneously. In embodiments where blocks 102 and 103 are sequentially formed, the grain refiner debris may be formed before or after melt formation at block 102. Nevertheless, as discussed above, the art has found that block 103 can produce grain refiner debris with maximum grain size and high deformation, thereby providing grain refiner debris that improves melt homogeneity and reduces the likelihood of large intermetallic compound particle formation. For example, block 103 may contain one or more operations 103A and 103B. In embodiments, grain refiner debris may be formed by mechanically pulverizing the as-received grain refiner product at operation 103A. Operation 103A may include cutting, sawing, grinding, rolling, extruding, machining, impacting, and other mechanical refining processes as known in the art, as well as any one or more of the mechanical deformations discussed herein, of the as-received grain refiner product or combinations thereof. In the implementation scheme, the original grain refiner product may include bars, strips, ingots, etc., and combinations thereof having one or more of the dimensions discussed above prior to deformation.
[0089] In the implementation scheme, mechanical crushing can be carried out over a period of time and by means of mechanical deformation sufficient to significantly deform the received grain refiner into multiple individual grain refiner particles, such as greater than or about 500 particles / mm. 2 Such as larger than or approximately 750 particles / mm 2 Such as larger than or approximately 1000 particles / mm 2 Such as larger than or approximately 1250 particles / mm 2 Such as larger than or approximately 1500 particles / mm 2 Such as larger than or approximately 1750 particles / mm 2 Such as larger than or approximately 2000 particles / mm 2 Such as larger than or approximately 2250 particles / mm 2 Such as larger than or approximately 2500 particles / mm 2 Such as larger than or approximately 2750 particles / mm 2 Such as larger than or approximately 3000 particles / mm 2 , or any range or value between them.
[0090] Regardless of the mechanical method chosen, grain refiner products can be pulverized into grain refiner fragments having a particle size of less than or about 1000 μm, such as less than or about 950 µm, such as less than or about 900 µm, such as less than or about 850 µm, such as less than or about 800 µm, such as less than or about 750 µm, such as less than or about 700 µm, such as less than or about 650 µm, such as less than or about 600 µm, such as less than or about 550 µm, such as less than or about 500 µm, such as less than or about 450 µm, such as less than or about 400 µm, such as less than or about 350 µm, such as less than or about 300 µm, such as less than or about 250 µm, such as less than or about 200 µm, such as less than or about 150 µm, such as less than or about 100 µm, such as less than or about 500 µm. granularity (e.g., equivalent diameter or maximum size) of µm or any range or value therein.
[0091] In addition, due to mechanical crushing, the grain refiner debris contains significantly reduced-size aluminide phases (such as TiAl3 phase), boride clusters, carbide clusters, oxide stripes, and refractive impurities. For example, in an embodiment, operation 103A may be performed over a period of time and / or under mechanical force such that some, substantially all or all of the TiAl3 phase present in the grain refiner debris have an equivalent spherical diameter of less than or about 100 μm, such as less than or about 95 µm, such as less than or about 90 µm, such as less than or about 85 µm, such as less than or about 80 µm, such as less than or about 75 µm, such as less than or about 70 µm, such as less than or about 65 µm, such as less than or about 60 µm, such as less than or about 55 µm, such as less than or about 50 µm, such as less than or about 45 µm, such as less than or about 40 µm, such as less than or about 35 µm, such as less than or about 30 µm, such as less than or about 25 µm, such as less than or about 20 µm, such as less than or about 15 µm, such as less than or about 10 µm, such as less than or about 5 µm, or any range or value thereof. In addition, a high proportion of grain refiner debris particles may have any one or more of the above-mentioned particle sizes, such as greater than or about 50% (D50), greater than or about 60%, greater than or about 70%, greater than or about 80%, greater than or about 90%, or any range or value between them.
[0092] In one embodiment, grain refiner debris may be added in particulate form at box 103. However, in another embodiment, the grain refiner debris may be incorporated into bars, pellets, etc., before being added to the melt, as illustrated in optional operation 103B. For example, mechanically deformed grain refiner product particles may be restructured into one or more forms for ease of handling, such as removing the particles (which may also be or include chips and / or flakes) and forming compacts, pucks, coarse particles, bars, blocks, combinations thereof, etc. Regardless of the form in which the grain refiner debris is incorporated into the melt, in one embodiment, the grain refiner debris may retain its individual particle size and dimensions, even when restructured into one or more larger forms for ease of handling.
[0093] At box 104, grain refiner debris, along with any optional additional alloying elements, can be added to the liquid metal. However, it should be understood that, in embodiments, the modified grain refiner product can be incorporated at any point before or during casting, such as before or after degassing and / or filtration. Additionally, in embodiments, the grain refiner product can be continuously incorporated during processing, before casting, or during casting. Box 104 is shown upstream of the degassing operation (box 105, which may include an optional metal filtration operation). However, in embodiments, grain refiner debris can be introduced after degassing box 105 due to the increased nucleation and dispersibility of the grain refiner and the increased dissolution rate. That is, as discussed above, conventional grain refiner products are introduced before degassing and / or metal filtration because conventional grain refiner products require a longer residence time in the melt to fully dissolve and disperse any impurities before ingot formation. However, this becomes increasingly problematic in the presence of various impurities such as magnesium, vanadium, calcium, and / or titanium, or at high concentrations thereof, as longer residence times allow for the formation of more intermetallic compound particles. Therefore, this technology can provide a faster melting process, at least in part, due to the increased surface area and deformed facets, or can incorporate grain refiner debris at later stages (e.g., downstream of degassing), thereby allowing for further improvements in melt homogeneity and intermetallic compound particle size. That is, not wanting to be bound by theory, it is believed that high deformation shortens the dissolution time, which, alone or in combination with the increased surface area, significantly improves the dissolution and dispersion time of grain refiner debris compared to conventional grain refiner products.
[0094] Nevertheless, the addition of optional alloying elements may include dissolving aluminum and raw elements or mixtures thereof into the liquid metal from box 102. After the addition of alloying elements, the modified liquid metal may have the desired composition of alloying elements and aluminum.
[0095] At box 105, the liquid metal from box 104 can be degassed to reduce the amount of dissolved gas in the modified liquid metal. Degasting the liquid metal may include reducing the hydrogen concentration in the modified liquid metal to a desired concentration, such as the concentration determined above (e.g., equal to or less than 0.25 mL / 100 g). For example, the amount of hydrogen contained in the degassed liquid metal may be equal to or less than approximately 0.25 mL / 100 g, 0.24 mL / 100 g, 0.23 mL / 100 g, 0.22 mL / 100 g, 0.21 mL / 100 g, 0.2 mL / 100 g, 0.19 mL / 100 g, 0.18 mL / 100 g, 0.17 mL / 100 g, 0.16 mL / 100 g, etc. The concentrations are 0.15 ml / 100g, 0.14 ml / 100g, 0.13 ml / 100g, 0.12 ml / 100g, 0.11 ml / 100g, 0.1 ml / 100g, 0.09 ml / 100g, 0.08 ml / 100g, 0.07 ml / 100g, 0.06 ml / 100g, or 0.05 ml / 100g. Any suitable technique can be used to degas the modified liquid metal.
[0096] At box 106, the degassed liquid metal from box 105 can be cast using direct cooling casting to produce intermediate metal product 116. In some cases, instead of casting using a direct cooling casting apparatus, as described with reference to box 106, the degassed liquid metal from box 105 can be cast using a continuous casting apparatus at box 107. The resulting intermediate-grade metal product can be intermediate metal product 116. Rolling to intermediate grades can include using any suitable equipment, such as a reversible rolling mill, to reduce the thickness of the ingot from the direct cooling casting.
[0097] At box 108, the intermediate metal product 116 can be hot-rolled to specifications or an intermediate specification. Hot rolling to specifications may include applying pressure to the intermediate metal product 116 through one or more work rolls at a high temperature (such as a temperature at or above the recrystallization temperature of the intermediate metal product 116), but lower temperatures may also be used. For example, in some cases, hot rolling may be performed at or above approximately 400°C, but other temperatures may be used. As a result of hot rolling at box 108, the thickness of the intermediate metal product 116 is reduced from the as-cast specification to the desired specification for delivery to the original equipment manufacturer (OEM) or other user, or reduced to an intermediate specification. In one example, the as-cast specification of the intermediate metal product 116 may be approximately 10 mm, while the final specification (e.g., the desired specification for delivery to the OEM) may be approximately 1.5 mm, but other specifications may be used. During hot rolling, the metal product may pass through any number of rolls, which are implemented through any number of mill stands. After hot rolling, the metal product can be considered as hot-rolled metal product 118. Hot-rolled metal product 118 may have T4 or O tempering.
[0098] In some cases, metal products can be preheated before hot rolling. For example, the metal product can be preheated to a temperature at or above the recrystallization temperature. In one example, the metal product can be preheated to a temperature at or above approximately 400°C, 450°C, 500°C, 550°C, 560°C, 570°C, or 580°C. In some cases, the metal product can be preheated in an oven at 400°C to 580°C for a period of 5 minutes to 24 hours. In some cases, the oven temperature can be approximately 550°C to 570°C, and the time can be 30 minutes to 6 hours. In some cases, the oven temperature can be approximately 560°C, and the time can be 30 minutes to 6 hours. In some cases, preheating can be carried out at other temperatures and for other durations.
[0099] At box 110, hot-rolled metal product 118 may optionally be cold-rolled from an intermediate specification to a final specification, if desired or desired. Cold rolling to specification may include applying pressure to the hot-rolled metal product 118 through one or more work rolls at a temperature below the recrystallization temperature of the hot-rolled metal product 118. For example, in some cases, cold rolling may be performed at a temperature below approximately 400°C, but other temperatures may be used. As a result of cold rolling at box 110, the thickness of the hot-rolled metal product 118 is reduced from an intermediate specification to the desired specification for delivery to an OEM or other user. In one example, the intermediate specification of the hot-rolled metal product 118 may be approximately 4 mm, while the final specification (e.g., the desired specification for delivery to an OEM) may be approximately 1.5 mm, but other specifications may be used. During cold rolling, the metal product may pass through any number of rolls, which are implemented through any number of mill stands. After cold rolling, the metal product may be considered cold-rolled metal product 119. Cold-rolled metal product 119 may have undergone T3 tempering.
[0100] At optional box 112, the hot-rolled metal product 118 may undergo heat treatment. In some cases, the heat treatment includes annealing. At box 112, the hot-rolled metal product 118 may be reheated to at or above the annealing temperature for a suitable period of time. For example, heating the hot-rolled metal product 118 to a temperature at or above 350°C for approximately 1 hour may achieve 0% tempering of the metal product.
[0101] In some cases, heat treatment may include solution treatment of the hot-rolled metal product 118 to allow certain alloying elements, such as silicon and copper, to re-enter the solid solution. As part of the solution treatment, the reheated metal product may be quenched to promote the retention of alloying elements in solution.
[0102] Heat treatment can improve the metallurgical and / or mechanical properties of metal products. For example, annealing can improve the formability of metal products.
[0103] At box 114, metal products can be wound up for delivery to the OEM. In some cases, metal products can be further processed before delivery, or parts can be manufactured directly without winding.
[0104] Regardless of the method chosen, the metal products are well-suited for part forming, such as for can end or lid blanks. That is, the metal products discussed herein can exhibit a combination of strength and other key properties, such as corrosion resistance, formability, and joining capabilities. Joining methods may include, but are not limited to, resistance spot welding (RSW), friction stir welding, remote laser welding, metallic inert gas (MIG) welding, tungsten inert gas (TIG) welding, bonding, and self-piercing riveting. Alloy products can be used in a wide range of applications, including beverage containers, automotive, transportation, electronics, and others. As discussed above, even at very low final specifications (such as those used in beverage container applications), and particularly at rivet locations on such beverage containers, the metal products described herein can exhibit reduced cracking and breakage.
[0105] Furthermore, at least in part due to mechanical crushing during the formation of the metal melt, the metal product may contain very little to no aluminide phases or intermetallic compound particles (such as TiAl3 phase), boride clusters, oxide streaks, and refractive impurities. Additionally, if any aluminide phase remains, some, substantially all, or all of the phases exhibit a significantly reduced equivalent spherical diameter relative to the metal product formed using conventional grain refiner products. For example, in embodiments, some, substantially all, or all of the TiAl3 phase present in the metal product has an equivalent spherical diameter of less than or about 50 μm, such as less than or about 45 µm, such as less than or about 40 µm, such as less than or about 35 µm, such as less than or about 30 µm, such as less than or about 25 µm, such as less than or about 20 µm, such as less than or about 15 µm, such as less than or about 10 µm, such as less than or about 5 µm, or any range or value between these values. Furthermore, a high proportion of grain refiner debris particles may have any or more of the aforementioned particle sizes, such as greater than or about 50% (D50), greater than or about 60%, greater than or about 70%, greater than or about 80%, greater than or about 90%, greater than or about 95%, greater than or about 97.5%, greater than or about 99%, or any range or value between these. However, it should be understood that, in embodiments, very little to no aluminide phase or intermetallic compound particles remain in the metal product.
[0106] The following provides a collection of exemplary embodiments, including at least some embodiments that are explicitly listed as “illustrations” providing additional descriptions of various example embodiments in accordance with the concepts described herein. These examples are not intended to be mutually exclusive, exhaustive, or limiting; and this disclosure is not limited to these exemplary examples, but covers all possible modifications and variations within the scope of the proposed claims and their equivalents.
[0107] As used below, any reference to a series of aspects (e.g., “aspects 1-4”) or an unlisted group of aspects (e.g., “any preceding or subsequent aspect”) shall be understood as a separate reference to each of those aspects (e.g., “aspects 1-4” shall be understood as “aspect 1, aspect 2, aspect 3 or aspect 4”).
[0108] Aspect 1: A metal casting method comprising: forming a liquid aluminum alloy; mechanically deforming a grain refiner product into grain refiner fragments with a particle size of less than 1000 μm, wherein at least a portion of the mechanically deformed grain refiner fragment particles comprises one or more TiAl3 phase particles with an equivalent spherical diameter of less than or about 50 μm; adding the mechanically deformed grain refiner fragments to the liquid aluminum alloy; casting the liquid metal into a metal product; and rolling the metal product.
[0109] Aspect 2: The method as described in aspect 1, wherein substantially all of the grain refiner debris comprises TiAl3 phase particles with an equivalent spherical diameter of less than or equal to 50 μm.
[0110] Aspect 3: The method as described in aspect 1 or 2, wherein the mechanically deformed grain refiner debris is added in the form of debris, granules, tablets, or a combination thereof.
[0111] Aspect 4: The method of any one of Aspects 1 to 3, wherein the mechanical deformation includes sawing, grinding, rolling, extrusion, machining, impact, or a combination thereof.
[0112] Aspect 5: The method of any one of Aspects 1 to 4, wherein the mechanical deformation is performed for a period of time to produce more than or 500 TiAl3 particles / mm 2 .
[0113] Aspect 6: The method of any one of Aspects 1 to 5, wherein the metal product comprises one or more intermetallic compound particles, each of the one or more intermetallic compound particles having an equivalent spherical diameter of less than or about 10 μm.
[0114] Aspect 7: The method of any one of Aspects 1 to 6, wherein the aluminum alloy comprises one or more of beryllium, magnesium, vanadium, strontium, titanium and calcium.
[0115] Aspect 8: The method of any one of Aspects 1 to 7, wherein the aluminum alloy comprises 5xxx series alloys.
[0116] Aspect 9: The method of any one of Aspects 1 to 8, wherein the molten metal comprises more than or 10% by weight of recycled aluminum alloy.
[0117] Aspect 10: The method of any one of Aspects 1 to 9, wherein the aluminum alloy comprises 0.01 wt% to 0.1 wt% titanium.
[0118] Aspect 11: The method of any one of Aspects 1 to 10, wherein the aluminum alloy comprises 1% to 7% magnesium by weight.
[0119] Aspect 12: The method of any one of Aspects 1 to 11, wherein the aluminum alloy contains 0.01 wt% vanadium to 0.1 wt% vanadium.
[0120] Aspect 13: The method of any one of Aspects 1 to 12, wherein more than or 50% by weight of the grain refiner debris comprises TiAl3 phase particles with an equivalent diameter of less than or equal to 50 μm.
[0121] Aspect 14: The method of any one of Aspects 1 to 13, wherein more than or 50% by weight of the grain refiner debris comprises TiAl3 phase particles with an equivalent diameter of less than or equal to 20 μm.
[0122] Aspect 15: The method of any one of Aspects 1 to 14, wherein more than or 50% by weight of the grain refiner debris comprises TiAl3 phase particles with an equivalent diameter of less than or equal to 10 μm.
[0123] Aspect 16: A metal product cast by any one of aspects 1 to 15.
[0124] Aspect 17: A 5xxx series aluminum alloy product comprising 0.01–1.0 wt% Cu, 0.1–0.8 wt% Fe, 0.5–7.0 wt% Mg, 0.01–1.2 wt% Mn, 0–1.5 wt% Si, 0–0.2 wt% Ti, 0–8.0 wt% Zn, 0–0.3 wt% Cr, 0–0.15 wt% Zr, 0–0.1 wt% V, 0–0.15 wt% Ca, up to 0.15 wt% impurities, and Al, wherein the aluminum alloy product comprises intermetallic compound particles comprising two or more of aluminum, beryllium, magnesium, vanadium, strontium, titanium, and calcium, having an equivalent spherical diameter of less than 50 μm.
[0125] Aspect 18: A beverage container comprising an aluminum alloy product as described in aspect 17, or cast by any one of aspects 1 to 15.
[0126] Aspect 19: A TiAl3-containing grain refiner product comprising grain refiner debris with a particle size of less than 1000 μm, wherein more than 50% by weight of the grain refiner debris comprises TiAl3 phase particles with an equivalent spherical diameter of less than or equal to 50 μm.
[0127] Aspect 20: A TiAl3-containing grain refiner product as described in aspect 19, wherein substantially all of the grain refiner debris comprises TiAl3 phase particles with an equivalent spherical diameter of less than or equal to 50 μm.
[0128] The foregoing aspects are merely possible examples of embodiments, set forth only for the purpose of clearly understanding the principles of this disclosure. Many variations and modifications may be made to one or more of the foregoing embodiments without substantially departing from the spirit and principles of this disclosure. All such modifications and variations are intended to be included herein within the scope of this disclosure, and all possible claims relating to aspects or combinations of elements or steps are intended to be supported by this disclosure. Furthermore, although specific terminology is used herein and in the appended claims, such specific terminology is used in a general and descriptive sense only and is not intended to limit the described embodiments or the purposes of the appended claims.
Claims
1. A metal casting method, comprising: Forming a liquid aluminum alloy; The grain refiner product is mechanically deformed into grain refiner fragments with a particle size of less than 1000 µm, wherein at least a portion of the mechanically deformed grain refiner fragment particles include one or more TiAl3 phase particles with an equivalent spherical diameter of less than or about 50 µm. Mechanically deformed grain refiner debris is added to the liquid aluminum alloy. Casting the liquid metal into a metal product; and The metal product is rolled.
2. The method of claim 1, wherein substantially all of the grain refiner debris comprises TiAl3 phase particles with an equivalent spherical diameter of less than or equal to 50 μm.
3. The method of claim 1, wherein the mechanically deformed grain refiner debris is added in the form of debris, granules, tablets, or a combination thereof.
4. The method of claim 1, wherein the mechanical deformation includes sawing, grinding, rolling, extrusion, machining, impact, or a combination thereof.
5. The method of claim 4, wherein the mechanical deformation is performed for a period of time to produce greater than or equal to 500 TiAl3 particles / mm. 2 .
6. The method of claim 1, wherein the metal product comprises one or more intermetallic compound particles, each of the one or more intermetallic compound particles having an equivalent spherical diameter of less than or about 10 μm.
7. The method of claim 1, wherein the aluminum alloy comprises one or more of beryllium, magnesium, vanadium, strontium, titanium and calcium.
8. The method of claim 7, wherein the aluminum alloy comprises 5xxx series alloys.
9. The method of claim 7, wherein the molten metal comprises more than or 10% by weight of recycled aluminum alloy.
10. The method of claim 9, wherein the aluminum alloy comprises 0.01 wt% to 0.1 wt% titanium.
11. The method of claim 9, wherein the aluminum alloy comprises 1% to 7% magnesium by weight.
12. The method of claim 9, wherein the aluminum alloy comprises 0.01% wt% vanadium to 0.1% wt% vanadium.
13. The method of claim 1, wherein greater than or 50% by weight of the grain refiner debris comprises TiAl3 phase particles with an equivalent diameter of less than or equal to 50 μm.
14. The method of claim 13, wherein more than 50% by weight of the grain refiner debris comprises TiAl3 phase particles with an equivalent diameter of less than or equal to 20 μm.
15. The method of claim 14, wherein greater than or 50% by weight of the grain refiner debris comprises TiAl3 phase particles with an equivalent diameter of less than or equal to 10 μm.
16. A metal product cast by the method of claim 1.
17. A 5xxx series aluminum alloy product, comprising... 0.01–1.0 wt% Cu, 0.1–0.8 wt% Fe, 0.5–7.0 wt% Mg 0.01–1.2 wt% Mn, 0–1.5 wt% Si, 0–0.2 wt% Ti, 0–8.0 wt% Zn 0–0.3% by weight Cr 0–0.15% by weight Zr 0–0.1% by weight V 0–0.15 wt% Ca, Impurities up to 0.15% by weight, and Al, The aluminum alloy product therein comprises intermetallic compound particles, which include two or more of aluminum, beryllium, magnesium, vanadium, strontium, titanium and calcium, and the intermetallic compound particles have an equivalent spherical diameter of less than 50 μm.
18. A beverage container comprising the aluminum alloy product as described in claim 17.
19. A grain refiner product containing TiAl3, comprising... Grain refiner debris with a particle size of less than 1000 μm The grain refiner debris comprising more than 50% by weight contains TiAl3 phase particles with an equivalent spherical diameter of less than or equal to 50 μm.
20. The TiAl3-containing grain refiner product of claim 19, wherein substantially all of the grain refiner debris comprises TiAl3 phase particles with an equivalent spherical diameter of less than or equal to 50 μm.
Citation Information
Patent Citations
Method for casting composite ingot
US7472740B2
Sequential casting of metals having high co-efficients of contraction
US7748434B2
Composite metal ingot
US8927113B2