Greasing agent for improving strength of leather and preparation method thereof
A fatliquoring agent and strength technology, applied in the field of leather strength fatliquoring agent and its preparation, can solve the problems such as the inability to achieve the tear resistance of leather, and achieve good adsorption and adsorption capacity, stable product quality and low cost. Effect
Patent Information
- Authority / Receiving Office
- CN · China
- Current Assignee / Owner
- Publication Date
- 2010-09-15
- Estimated Expiration
- Not applicable · inactive patent
Abstract
Description
technical field
[0001] The invention relates to a fatliquoring agent for leather strength and its preparation. technical background
[0002] With the development of leather technology level, the strength of leather, that is, the tear resistance has become an important index to measure the quality of leather.
[0003] In the process of processing natural animal skin into leather, the high-grade leather fatliquoring agent should have the softness and toughness of the leather, the fullness and elasticity of the leather, the smoothness of silk fabric, and not dry and hard with the change of climate and time. performance.
[0004] Chinese patent application No. 88106317 discloses the preparation of fatty acid amido sodium carboxylate composite leather fatliquoring agent, which is mainly composed of fatty acid amido sodium carboxylate compounded with sulfated lard, chlorinated paraffin, ammonium alkylsulfonate Composition, the patent claims that the composite fatliquoring agent ...
Examples
Embodiment 1
[0024] Formula: (parts by weight)
[0025] Polyoxyethylene alkyl phosphate 100
[0027] Chlorinated paraffin 50
[0028] Sodium carboxymethyl cellulose 5
[0029] Sodium alkyl sulfonate 100
[0030] Olive Oil PEG 500
[0031] Chlorinated paraffin is 52# chlorinated paraffin;
[0032] The average molecular weight of olive oil polyethylene glycol ester is 2000;
[0033] Sodium alkylsulfonate is sodium dodecylsulfonate.
[0034] Preparation:
[0035] (1) Mix polyoxyethylene alkyl phosphate and fish oil amide evenly at 40°C;
[0036] (2) Mix chlorinated paraffin and olive oil polyethylene glycol ester uniformly at 50°C;
[0037] (3) Add the mixture obtained in step (1) to the mixture obtained in step (2), stir evenly at 50°C, then heat up to 50°C, add sodium carboxymethylcellulose and sodium alkylsulfonate Stir evenly to get the product. Appearance is yellow or white emulsion, pH value is 5.5.
[0038] According to the following process, the...
Embodiment 2
[0045] Formula: (parts by weight)
[0046] Fish oil amide 150
[0047] Chlorinated paraffin 100
[0048] Sodium carboxymethyl cellulose 5
[0049] Sodium alkyl sulfonate 40
[0050] 30# engine oil 450
[0051] Chlorinated paraffin is 52# chlorinated paraffin;
[0052] The sodium alkylsulfonate is a mixture of sodium dodecylsulfonate and sodium octadecylsulfonate with a weight ratio of 1:1.
[0053] The preparation method is:
[0054] (1) Heating fish oil amide to 45°C;
[0055] (2) Mix chlorinated paraffin and 30# engine oil evenly at 55°C;
[0056] (3) Add the mixture obtained in step (1) to the mixture obtained in step (2), stir evenly at 55°C, then heat up to 60°C, add sodium carboxymethylcellulose and sodium alkylsulfonate Stir evenly to get the product. Appearance is yellow or white emulsion, PH 6.0.
[0057] Example two products are tested according to the following process, and the test adopts sheepskin:
[0058] %(W / W)
Weight (g)
chemicals ...
Embodiment 3
[0064] Formula: (parts by weight)
[0065] Polyoxyethylene alkyl phosphate 100
[0066] Fish oil amide 180
[0067] Chlorinated paraffin 50
[0068] Sodium Carboxymethyl Cellulose 1
[0069] Sodium alkyl sulfonate 150
[0070] Olive Oil PEG 500
[0071] 30# engine oil 450
[0072] The average molecular weight of olive oil polyethylene glycol ester is 2000;
[0073] Chlorinated paraffin is 52# chlorinated paraffin;
[0074] The sodium alkylsulfonate is a mixture of sodium dodecylsulfonate and sodium octadecylsulfonate with a weight ratio of 1:1.
[0075] The preparation method is:
[0076] (1) Mix polyoxyethylene alkyl phosphate and fish oil amide evenly at 40°C;
[0077] (2) Mix chlorinated paraffin, olive oil polyethylene glycol ester and 30# engine oil at 55°C;
[0078] (3) Add the mixture obtained in step (1) to the mixture obtained in step (2), stir evenly at 55°C, then heat up to 60°C, add sodium carboxymethylcellulose and sodium alkylsulfonate Stir evenly to g...