Dyeing and finishing process for green chinlon/spandex side stretch fabric

A technology of four-way stretching and craftsmanship, which is applied in the direction of heating/cooling fabric, fabric surface trimming, dyeing method, etc., and can solve the problem of high probability of contact between fabric edge and dyeing liquid, unfavorable energy saving, emission reduction, consumption reduction, and affecting normal production, etc. problem, to achieve the effect of improving dyeing synchronization, reducing color flower phenomenon, and solving edge-to-edge color difference

CN105544252AActive Publication Date: 2016-05-04杭州天宇印染有限公司
4 Cites 5 Cited by

Patent Information

Authority / Receiving Office
CN · China
Current Assignee / Owner
Publication Date
2016-05-04

Smart Images

  • Figure 1
    Figure 1
  • Figure 2
    Figure 2
  • Figure 3
    Figure 3
Patent Text Reader

Abstract

The invention provides a dyeing and finishing process for green chinlon / spandex side stretch fabric. The dyeing and finishing process comprises a dyeing process. A dyeing agent prepared from 1-1.5 g / L of acid leveling agent, 0.8-1 g / L of acid-releasing agent, 1 g / L of chelating dispersant, 0.5-2% (o.w.f.) of acid light yellow and 0.3-4% (o.w.f.) of acid emerald blue is adopted for the dyeing process. The bath ratio is 1:10, dyeing synchronism of acid light yellow and acid emerald blue is greatly improved, competition of two dyes for fiber dyeing is effectively retarded, and the dyeing defect phenomena generated during dyeing are reduced. Meanwhile, side-to-centre shading generated during warp beam dyeing is avoided, and reworking for dyeing defects is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

technical field

[0001] The invention belongs to the field of fabric dyeing and finishing, in particular to a dyeing and finishing process of green brocade / spandex four-way stretch knitted fabric. Background technique

[0002] Nylon / spandex four-way stretch fabric is an elastic fabric interwoven with nylon fiber and spandex fiber. It has a unique fiber yarn structure, fashionable fabric texture and excellent wearing performance, and has a very broad market prospect. Green is a common color in nature, representing freshness, hope, safety, calm, comfort, life, peace, serenity, nature, environmental protection, growth, vitality, youth and life, so green nylon / spandex four-way stretch fabric is very popular among people favorite.

[0003] The dyeing and finishing process of the traditional green brocade / spandex four-way stretch fabric includes refining process, pre-shrinking, presetting, warp dyeing, color fixing, washing and setting, wherein acid dyes and glacial acetic acid ar...

Examples

Embodiment 1

[0033] A dyeing and finishing process of green brocade / spandex four-way stretch fabric, including the process steps of greige preparation → sewing → refining → preshrinking → dehydration, opening → presetting → warp beam rolling → dyeing → cold water washing → color fixing →washing→unwinding and rolling→softening and shaping→inspection→rolling and packing:

[0034] The refining process is as follows: refining in 8-section continuous refining machine, adding refining degreasing agent 8g / L and chelating dispersant 3g / L in the rolling tank, and controlling the water temperature in the refining tank of 8-section continuous refining machine as 65°C → 92°C ℃→75℃→75℃→60℃→60℃→40℃→40℃, the vehicle speed is 60m / min;

[0035] The pre-shrinking process uses an airflow dyeing machine for pre-shrinking, and heats it for 30 minutes at 90 ° C. The formula is

[0036]

[0037] The temperature of the presetting process is 200°C, and the vehicle speed is 20-30m / min;

[0038] Adopt following...

Embodiment 2

[0047] A dyeing and finishing process of green brocade / spandex four-way stretch fabric, including the process steps of gray fabric preparation → sewing → refining → preshrinking → dehydration, opening → presetting → warp beam rolling → dyeing → cold water washing → color fixing →washing→unwinding and rolling→softening and shaping→inspection→rolling and packing:

[0048] The refining process is as follows: refining in 8-section continuous refiner, adding 8g / L refining degreaser and 3g / L chelating dispersant to the rolling tank, and controlling the water temperature in the refining tank of 8-section continuous refiner as 65°C → 92°C ℃→75℃→75℃→60℃→60℃→40℃→40℃, the vehicle speed is 60m / min.

[0049] The pre-shrinking process uses an airflow dyeing machine for pre-shrinking, and heats it at 90°C for 30 minutes. The formula is:

[0050]

[0051] The temperature of the presetting process is 200°C, and the vehicle speed is 20-30m / min;

[0052] Adopt following dyeing auxiliary for...

Embodiment 3

[0061] A dyeing and finishing process of green brocade / spandex four-way stretch fabric, including the process steps of gray fabric preparation → sewing → refining → preshrinking → dehydration, opening → presetting → warp beam rolling → dyeing → cold water washing → color fixing →washing→unwinding and rolling→softening and shaping→inspection→rolling and packing:

[0062] The refining process is as follows: refining in 8-section continuous refining machine, adding refining degreasing agent 8g / L and chelating dispersant 3g / L in the rolling tank, and controlling the water temperature in the refining tank of 8-section continuous refining machine as 65°C → 92°C ℃→75℃→75℃→60℃→60℃→40℃→40℃, the vehicle speed is 60m / min;

[0063] The pre-shrinking process uses an airflow dyeing machine for pre-shrinking, and heats it at 90°C for 30 minutes. The formula is:

[0064]

[0065] The temperature of the presetting process is 200°C, and the vehicle speed is 20-30m / min;

[0066] Adopt follo...