A connection method and alloy technology, applied in welding equipment, metal processing equipment, welding/welding/cutting articles, etc., can solve the problems of low tensile strength of weld seam, high required temperature, deformation of workpiece, etc., and achieve improvement in high temperature Performance and service life, low equipment vacuum requirements, and the effect of reducing connection temperature
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Publication Date
- 2019-11-29
Abstract
Description
technical field
[0001] The invention relates to a low-temperature joining method of dissimilar refractory alloys, in particular to a joining method of TZM / WRe dissimilar alloys. Background technique
[0002] TZM alloy is a high-temperature alloy formed by adding Ti and Zr with a total amount of no more than 1% in Mo matrix. Compared with pure molybdenum, TZM alloy has higher recrystallization temperature and high temperature strength. TZM alloy is widely used, such as: taking advantage of its good corrosion resistance, it is used in the glass melting furnace and the main shaft of the agitator coated with platinum and rhodium on the glass bulb production line of color picture tube; it is used in the die-casting of non-ferrous metals by taking advantage of its high melting point. Mold: Utilizing its good mechanical properties under high temperature and high pressure, it is used for military components such as gas distribution valve bodies and rocket nozzles on torpedo engines...
Examples
Embodiment 1
[0041] The low-temperature diffusion welding of the TZM / WRe dissimilar alloy of the present embodiment is carried out as follows:
[0042] step 1,
[0043] The surfaces to be welded of TZM alloy and WRe alloy were pre-grinded with #400, #800, #1000, #1500, #2000 metallographic sandpaper in sequence, then polished and ultrasonically cleaned in alcohol.
[0044] Step 2,
[0045] Weigh 0.0158 g of Ti powder with a particle size of 46 μm with an electronic balance (accuracy of 0.1 mg), so as to ensure that the thickness of the titanium active intermediate layer in the later connector is 60-80 μm.
[0046] Step 3,
[0047] Put the treated TZM alloy, Ti powder and WRe alloy into the graphite female mold sequentially from top to bottom, and then press it tightly with the upper and lower pressure heads, and at the same time make the active middle layer of Ti powder be located in the middle of the height of the graphite female mold .
[0048] Step 4,
[0049] Place the graphite mo...
Embodiment 2
[0057] The low-temperature diffusion welding of the TZM / WRe dissimilar alloy of the present embodiment is carried out as follows:
[0058] step 1,
[0059] The surfaces to be welded of TZM alloy and WRe alloy were pre-grinded with #400, #800, #1000, #1500, #2000 metallographic sandpaper in sequence, then polished and ultrasonically cleaned in alcohol.
[0060] Step 2,
[0061] Weigh 0.0158 g of Ti powder with a particle size of 46 μm with an electronic balance (accuracy: 0.1 mg), so as to ensure that the thickness of the Ti active intermediate layer in the later connector is 60-80 μm.
[0062] Step 3,
[0063] Put the treated TZM alloy, Ti powder and WRe alloy into the graphite female mold sequentially from top to bottom, and then press it tightly with the upper and lower pressure heads, and at the same time make the active middle layer of Ti powder be located in the middle of the height of the graphite female mold .
[0064] Step 4,
[0065] Place the graphite mold with ...
Embodiment 3
[0073] The low-temperature diffusion welding of the TZM / WRe dissimilar alloy of the present embodiment is carried out as follows:
[0074] step 1,
[0075] The surfaces to be welded of TZM alloy and WRe alloy were pre-grinded with #400, #800, #1000, #1500, #2000 metallographic sandpaper in sequence, then polished and ultrasonically cleaned in alcohol.
[0076] Step 2,
[0077] Weigh 0.0158 g of Ti powder with a particle size of 46 μm with an electronic balance (accuracy: 0.1 mg), so as to ensure that the thickness of the Ti active intermediate layer in the later connector is 60-80 μm.
[0078] Step 3,
[0079] Put the treated TZM alloy, Ti powder and WRe alloy into the graphite female mold sequentially from top to bottom, and then press it tightly with the upper and lower pressure heads, and at the same time make the active middle layer of Ti powder be located in the middle of the height of the graphite female mold .
[0080] Step 4,
[0081] Place the graphite mold with ...