Test method for clogging of geotextiles by axial compression
Through the geotextile axial compression method silt test method, the problems of pressure measuring tube reading stability and water resource waste in the gradient ratio test are solved, and the rapid and accurate determination of geotextile silt characteristics is achieved, which is suitable for low permeability Tests under different pressure conditions.
Patent Information
- Application Number
- CN201710845025.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2017-09-19
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2037-09-19
AI Technical Summary
The existing gradient ratio method blocking test methods have problems such as long stable reading time of pressure measuring tube, difficulty in accurately determining stability, easy blockage of pipe mouth, long test cycle, waste of water resources and low labor efficiency, especially in low permeability soils. It is difficult to accurately determine the silt characteristics of geotextiles.
The geotextile axial compression method is used to block the test method, and the water of the soil sample itself is used to transfer the soil particles by applying an axial pressurization device. The deformation measurement device records the height change of the sample, calculates the amount of retention and the vertical permeability coefficient, and simplifies the The test process avoids external water sources and long-term head stability problems.
It realizes a fast and accurate geotextile silt test, which is suitable for low permeability soils. It can measure silt characteristics under different pressure conditions, reduces water resource consumption, and improves the test efficiency and stability of results.
Smart Images

Figure CN107703038B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of geosynthetics testing, and in particular relates to a geotextile axial compression clogging test method. Background Art
[0002] Blockage refers to the process in which small particles in the soil pass through the geotextile, gather on the surface of the geotextile, or form a weak permeable layer, or block the end of the geotextile filtration channel, or stay inside the geotextile, resulting in a decrease in the water permeability of the geotextile. Blockage is usually evaluated based on the reduction of water flow through the fabric and the increase of soil particles entering the fabric.
[0003] On the one hand, with the rapid development of my country's port engineering, water transport engineering and offshore engineering, a large number of soft soil foundations need to be reinforced. Soft soil foundations have the characteristics of high water content, poor gradation, high clay content and low permeability coefficient. Plastic drain boards combined with vacuum preloading method are basically used for reinforcement. Plastic drain boards play a triple role of drainage, filtration and blocking for reinforced soil. Under the action of vacuum suction, water in the foundation enters the filter membrane through the soil layer, and soil particles also gather around the filter membrane of the plastic drain board under the action of vacuum suction. Some fine particles adhere to the surface of the filter membrane, and some fine particles are embedded in the pores of the filter membrane, causing the filter membrane to be blocked, thereby causing the drainage channel to fail and affecting the reinforcement effect. Therefore, it is very important to conduct clogging tests on geotextiles used as filter membranes, but many problems are encountered in conventional clogging tests, and the clogging characteristics of the filter membrane in soft soil cannot be measured.
[0004] On the other hand, the external conditions of the soil and geotextile system, such as the surrounding pressure, also have an important influence on the clogging of geotextiles. The surrounding pressure will reduce the thickness of the geotextile and reduce its porosity, thereby reducing the permeability of the geotextile and aggravating the clogging. However, conventional clogging tests cannot apply a specific pressure to measure the clogging performance of geotextiles under a certain pressure.
[0005] The commonly used plugging test method internationally is the gradient ratio method. The gradient ratio test was first proposed by Calhoun in the 1970s and later adopted by the U.S. Army Corps of Engineers. The gradient ratio test method is the most commonly used method for plugging tests. There are the American standard "Gradient Ratio Plug Test Method for Soil and Geotextile Systems" (ASTM D5101-2006) and the FHWA "Geotextile Engineering Manual", both of which are basically the same. The plugging test methods specified in my country's "Test Procedures for Geosynthetics" (SL / T 235-2012) and "Test Procedures for Geosynthetics for Highway Engineering" (JTG E50-2006) are both gradient ratio methods and are compiled according to American standards.
[0006] Typical test equipment for gradient ratio test is as follows: Figure 8The diameter of the cylinder is 100mm, the height of the soil sample above the fabric is 100mm, and there should be enough space above the soil sample to ensure uniform and stable water flow. There are six pressure measuring tubes in total, and the inner diameter of the pressure measuring tube is not less than 3mm. A filter layer should be set at the joint to prevent the soil sample from blocking the pressure measuring tube orifice.
[0007] Continuously measure the change of water level in each pressure measuring tube over time and calculate the hydraulic gradient as follows: Where i1 is the hydraulic gradient of the soil sample 25 mm above the geotextile; i2 is the hydraulic gradient of the soil sample 25 mm to 75 mm above the geotextile.
[0008] The specific method is: load the air-dried soil sample and saturate it, adjust the hydraulic gradient to 1.0, read the water level and seepage of the piezometer tube once an hour after the piezometer tube is stable, and read it continuously for 24 hours. If the reading is not completely stable, the test time can be appropriately extended until it is stable. Then adjust the hydraulic gradient to 2.5, 4.0 and 10.0. For each increase, the piezometer tube reading should be stable and seepage should be allowed to last for at least 1.5 hours under the hydraulic gradient. When the hydraulic gradient is 10.0, read the water level and seepage of the piezometer tube once an hour after the piezometer tube is stable, and read it continuously for 24 hours. If the reading is not completely stable, the test time can be appropriately extended until it is stable.
[0009] The gradient ratio GR is used to evaluate the clogging characteristics of the fabric. The larger the gradient ratio, the more serious the clogging, and the more soil particles gather on the surface and inside of the fabric. When the filter membrane is clogged and its permeability coefficient becomes smaller, the head loss of the filter membrane and the soil layer near it during seepage will increase, causing the gradient ratio to increase in value, at this time GR>1; when the filter membrane cannot play a role in soil conservation and soil particles continue to be lost with the seepage, the soil sample in the soil layer near the filter membrane loses fine particles, the permeability coefficient increases, causing the gradient ratio to decrease in value, that is, GR<1.
[0010] Problems with gradient ratio tests
[0011] 1) The piezometer reading takes a long time to stabilize. In the gradient ratio clogging test, the piezometer water level must be read. The piezometer water level refers to the height of the seepage water in the piezometer.
[0012] According to Darcy's law, the amount of permeate water Q = k|At
[0013] The time required for water to reach a height of h in the piezometer is t = h / (kJ)
[0014] When the hydraulic gradient of the gradient ratio test is 1, if the permeability coefficient of the soil is 10 -6 cm / s (permeability coefficient of silty clay is 10 -6 ~10 -7cm / s, the permeability coefficient of clay is even smaller), the time required for the height of the piezometer at 25cm above the fabric to change by 1mm is no less than 11.9h, and the time required for the height of the piezometer at 75cm above the fabric to change by 1mm is no less than 5.6h. In addition, as the water head of the piezometer increases, the water seepage rate will also decrease; the longer it takes for the water head of the piezometer to stabilize, the greater the impact of water evaporation on it. In summary, when using soils with low permeability coefficients such as silty clay and clay, the gradient ratio method water head stabilization time is as long as several days, and the test cycle is long.
[0015] 2) It is difficult to accurately determine whether the pressure gauge reading is stable. Because the water head of the pressure gauge changes very slowly, coupled with the influence of water evaporation, it is difficult to accurately determine whether the pressure gauge is stable. If the judgment is wrong, it will directly lead to errors in the calculation results of the gradient ratio.
[0016] 3) Due to the long test time and the high content of fine particles in the soil, the pressure measuring tube outlet is very easy to be blocked.
[0017] 4) Due to the above reasons, the water head data of the pressure measuring tubes at the same horizontal height often vary greatly, which brings certain troubles to the selection of test data.
[0018] 5) The gradient ratio method siltation test requires saturated soil after sampling. For low permeability soil, the saturation speed is slow, and due to the low structural strength of the soil, soil damage will occur if water enters too quickly. The saturation degree is also difficult to control. If the saturation is not thorough, the infiltration rate will be reduced, which will have a significant impact on the test results.
[0019] 6) The test water depends on external water sources. The water head must be maintained during the test. A long test time will result in a waste of water resources.
[0020] 7) The gradient ratio clogging tester can only test one sample at a time, and the reading is taken once an hour. The number of readings when the pressure measuring tube can be stable within 24 hours is 51 times. The gradient ratio clogging test has a high reading frequency and low labor efficiency. Summary of the invention
[0021] In order to solve the above problems, the present invention provides a geotextile axial compression clogging test method.
[0022] The technical solution of the present invention is a geotextile axial compression method for clogging test, wherein the test device used includes a sample container, a deformation measuring device and an axial pressure device, and is characterized in that the sample container includes a water tank, a protective ring, a ring knife, a water-permeable plate and a sample cover, and the protective ring, the water-permeable plate, the ring knife and the sample cover are sequentially arranged in the water tank, and the deformation measuring device and the axial pressure device are in contact with the sample cover;
[0023] The permeable plate includes a top permeable plate and a bottom permeable plate, a ring knife is arranged between the top permeable plate and the bottom permeable plate, the bottom permeable plate, the ring knife, the top permeable plate and the sample cover are arranged in sequence from bottom to top in the protective ring, the sample is arranged in the ring knife, and the sample includes a bottom geotextile, a soil sample, and a top geotextile arranged in sequence from bottom to top, the inner diameter of the ring knife is greater than or equal to 79.8 mm, and the sizes of the protective ring, the ring knife, the sample, the permeable plate and the sample cover match.
[0024] Furthermore, a steel ball is provided at the center of the top surface of the sample cover, and the axial pressure device is in contact and connected with the sample cover through the steel ball; a shallow groove is provided at the bottom of the water tank for placing the guard ring, and a drain port is provided at the bottom of the guard ring for serving as a water circulation channel;
[0025] The diameter of the inner edge of the shallow groove is smaller than the inner diameter of the guard ring, and the diameter of the outer edge of the shallow groove is larger than the outer diameter of the guard ring.
[0026] Furthermore, the deformation measuring device comprises a dial indicator and a meter stand, one end of the meter stand is connected to the water tank, and the other end of the meter stand is connected to the dial indicator.
[0027] Furthermore, the deformation measuring device adopts a displacement sensor.
[0028] Furthermore, the dial indicator has a measuring range of 10 to 20 mm and a minimum division of 0.01 mm.
[0029] Furthermore, the displacement sensor adopts a zero-order displacement sensor.
[0030] Furthermore, the axial pressure device adopts a hydraulic, pneumatic, lever or scale type device.
[0031] The geotextile axial compression clogging test method is characterized by comprising the following steps:
[0032] Step 1. Prepare the sample: cut 2 pieces of geotextile with a diameter of 79.8 mm, measure the area and weigh them, measure their thickness according to the geotextile thickness measurement test method, saturate the geotextile and the permeable plate with water, cut the original soil sample with a ring knife or fill the disturbed soil sample in the ring knife, if the soil sample is unsaturated, saturate the soil sample, place geotextiles on the top and bottom of the soil sample respectively, and the contact surface between the geotextile and the soil sample should be the same as in the engineering application to simulate the working state of the geotextile;
[0033] Step 2: Install the sample: Place the guard ring into the shallow groove of the water tank, place the permeable plate with a slightly larger diameter into the guard ring, apply a layer of vaseline on the outer wall of the ring cutter, and place the cutting edge downward into the guard ring until it contacts the bottom permeable plate. Place the top permeable plate and the sample cover on the sample in turn;
[0034] Step 3: Connect the axial pressure device: The axial pressure device is connected to the steel ball on the sample cover to ensure that the force direction of the sample is perpendicular to its cross section;
[0035] Step 4: Install the deformation measuring device: Use the axial pressure device to apply a pre-pressure of 1 kPa to the sample to make all parts in close contact, wrap the sample with moisturizing materials such as wet cotton yarn and keep it moisturized during the entire test process, install a dial indicator or displacement sensor, unload, and adjust the deformation reading to zero;
[0036] Step 5: Apply axial pressure: Design the axial load sequence according to the strength of the soil and the test requirements. For soil with high water content and low strength, a vertical load of 1 to 5 kPa should be applied first. After the load is applied, the deformation of the sample at different times, that is, the height change, is recorded. The deformation stability standard is that the deformation in the last hour does not exceed 0.001 to 0.01 mm. After the deformation is stable, the load is applied step by step according to the load sequence.
[0037] Step 6: After the test, unload, remove the sample, peel off the geotextile, remove the surface soil, quickly put a piece of geotextile into the permeameter, and measure its vertical permeability coefficient according to the vertical permeability test method of geotextile. After a piece of geotextile is air-dried, weigh it;
[0038] Step 7. Calculation: Calculate the amount of retained soil and the reduction in the vertical permeability coefficient of geotextiles.
[0039] Furthermore, the step six and the step seven also include a thickness measurement step, which is as follows:
[0040] The comprehensive permeability coefficient of the sample, the consolidation coefficient of the soil sample, and the compression modulus parameters of the soil sample need to be calculated. The change of geotextile thickness with load cannot be ignored. The geotextile needs to be cut and its thickness measured according to the geotextile thickness measurement test method according to the axial load sequence of the test. The height change of the soil sample is calculated based on the deformation of the sample and the change of geotextile thickness.
[0041] The calculation formula of soil sample deformation under a certain load level is:
[0042] H=(h0-h1)-(t0-t1)
[0043] Where H is the deformation of the soil sample under a certain level of load, mm; h0 is the height of the sample at the end of the previous level of load, mm; h1 is the height of the sample at the end of a certain level of load, mm; t0 is the thickness of the geotextile under the previous level of load, mm; t1 is the thickness of the geotextile under a certain level of load, mm.
[0044] Furthermore, the calculation formula for the amount of retained soil in step eight is:
[0045] Where η is the amount of soil retained by the geotextile, g / cm 2 ; m is the mass of geotextile, g; m1 is the mass of geotextile and soil after the test, g; A is the area of geotextile, cm 2 ;
[0046] The calculation formula for the reduction of vertical permeability coefficient of geotextiles is:
[0047]
[0048] Where K is the reduced vertical permeability of geotextile; k0 is the initial vertical permeability of geotextile, cm / s; k1 is the vertical permeability of geotextile after the test, cm / s.
[0049] The beneficial effects of the present invention are:
[0050] (1) The overall structure is simple and the design is reasonable. Through the axial pressure device, the water in the soil sample itself drives the soil particles to migrate under the action of pressure, thereby causing the geotextile to be blocked. This solves a series of problems such as the traditional gradient ratio method must use an external water source to provide hydraulic gradient, must read the water level of the piezometer and calculate the permeability coefficient through the seepage of the soil, there may be an error between the water level of the piezometer and the actual water head, and it cannot be used for the blockage test when the geotextile is used as a filter layer of low permeability soil. The geotextile axial compression method blockage test does not need to measure the seepage of the soil, which solves the problem that it is impossible to conduct a blockage test of geotextiles in low permeability soil.
[0051] The judgment of clogging is usually evaluated by the reduction of water flow through the fabric and the increase of soil particles entering the fabric. The reduction of flow in the gradient ratio method clogging test is expressed by the gradient ratio, and the soil particles entering the fabric are expressed by the amount of soil retained per unit volume of the geotextile after the test; the reduction of flow in the geotextile axial compression method clogging test is quantitatively expressed by the reduction of the vertical permeability coefficient of the geotextile, and the soil particles entering the fabric are expressed by the amount of soil retained per unit area of the geotextile after the test. Compared with the two results, the vertical permeability reduction is more intuitive and easier to understand than the gradient ratio; due to the large difference in thickness of different fabrics, the amount of soil retained per unit area is more suitable for comparing their clogging characteristics than the amount of soil retained per unit volume.
[0052] (2) The present invention can be used not only for the clogging test of geotextiles in low permeability soils, but also for the clogging test of geotextiles in general permeability soils, and has a wide range of applications. However, it is not suitable for the clogging test of geotextiles in coarse-grained soils.
[0053] (3) The present invention can apply axial pressure according to actual needs to measure the clogging characteristics of geotextiles under a certain vertical pressure, and can simulate the overburden pressure or surrounding pressure that geotextiles are subjected to during engineering applications.
[0054] (4) Geotextile axial compression method clogging test Each container of the test device can hold two samples for simultaneous testing. The soil sample for the axial compression method clogging test can be the original soil sample, which can directly reflect the filtration and drainage effect of the soil and geotextile.
[0055] (5) Using saturated soil samples, the present invention can calculate the change in the porosity of the soil by recording the change in the height of the sample and the change in the thickness of the geotextile under axial pressure, thereby calculating the discharge of water in the soil, thereby calculating the comprehensive permeability coefficient of the sample composed of the geotextile and the soil, and also deriving the consolidation characteristics of the soil.
[0056] (6) The test proves that the soil retention and vertical permeability coefficient of the plastic drain filter membrane measured by the geotextile axial compression clogging test method are very close to those of the plastic drain filter membrane after construction, with an error of 5-25%, and the results of the axial compression clogging test method are slightly smaller than those of the plastic drain filter membrane after construction. Since the plastic drain filter membrane works for several months and the clogging mechanism is more complicated, it is very reasonable that the results of the geotextile axial compression clogging test method are slightly smaller than the actual results.
[0057] (7) The present invention does not require an additional water source, uses less soil, uses conventional instruments and equipment, is simple to operate, has a fast test speed, and produces stable and reliable results.
[0058] Comparing the two clogging test methods, the gradient ratio method saturates the soil with an external water source and provides a water head. The water penetrates into the soil and drives the migration of soil particles. The measured values are the water head of the pressure tube, the amount of infiltrated water and the mass of the sample. The test results are the gradient ratio and the soil content per unit volume. It is suitable for testing the clogging of fabrics in soils with a certain permeability coefficient. The axial compression method forces the self-water in the soil to be discharged by applying external pressure to drive the migration of soil particles for clogging tests. The measured values are the sample height, thickness, mass and permeability of geotextiles. The test results are the reduction of vertical permeability coefficient and the amount of retained soil per unit area. It is suitable for testing the clogging of geotextiles in soils with low permeability coefficient and high saturation and when there is a vertical load. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] Figure 1 It is a structural schematic diagram of a geotextile axial compression method clogging test device of the present invention.
[0060] Figure 2 It is a front view of the present invention.
[0061] Figure 3 yes Figure 2 AA section view.
[0062] Figure 4 It is a schematic diagram of the structure of the sample of the present invention.
[0063] Figure 5 It is a schematic structural diagram of the guard ring of the present invention.
[0064] Figure 6 It is a structural schematic diagram of a water tank of the present invention.
[0065] Figure 7 The present invention is a flow chart of the geotextile axial compression method for clogging test.
[0066] Figure 8 It is a schematic diagram of the structure of a typical test device for gradient ratio test.
[0067] In the figure: 1 is a meter stand, 2 is a steel ball, 3 is a sample cover, 4 is a top water-permeable plate, 5 is a sample, 6 is a ring knife, 7 is a guard ring, 8 is a water trough, 9 is a bottom water-permeable plate, 10 is a dial indicator, 11 is an axial pressure device, 12 is a top geotextile, 13 is a soil sample, 14 is a bottom geotextile, 15 is a shallow groove, 16 is a drain port, 17 is a connecting rod, 18 is an adjusting rod, 19 is a connecting hole, and 20 is a mounting hole. DETAILED DESCRIPTION
[0068] A specific implementation of the present invention is described below with reference to the accompanying drawings.
[0069] In the figure: 1 is a meter stand, 2 is a steel ball, 3 is a sample cover, 4 is a top water-permeable plate, 5 is a sample, 6 is a ring knife, 7 is a guard ring, 8 is a water trough, 9 is a bottom water-permeable plate, 10 is a dial indicator, 11 is an axial pressure device, 12 is a top geotextile, 13 is a soil sample, 14 is a bottom geotextile, 15 is a shallow groove, 16 is a drain port, 17 is a connecting rod, 18 is an adjusting rod, 19 is a connecting hole, and 20 is a mounting hole.
[0070] The clogging test device of geotextile axial compression method comprises a sample container, a deformation measuring device and an axial pressure device 11, wherein the sample container comprises a water tank 8, a protective ring 7, a ring knife 6, a water-permeable plate and a sample cover 3, the protective ring 7, the water-permeable plate and the sample cover 3 are sequentially arranged in the water tank 8, the deformation measuring device and the axial pressure device 11 are in contact with and connected to the sample cover 3, the overall connection is convenient, easy to implement, the structure is reasonably arranged, and the measurement is convenient;
[0071] The permeable plate includes a top permeable plate 4 and a bottom permeable plate 9, a ring knife 6 is arranged between the top permeable plate 4 and the bottom permeable plate 9, the bottom permeable plate 4, the ring knife 6, the top permeable plate 9 and the sample cover 3 are arranged in the protective ring 7 from bottom to top, and the sample 5 is arranged in the ring knife 6. The sample 5 includes a bottom geotextile 14, a soil sample 13 and a top geotextile 12 arranged in sequence from bottom to top. The inner diameter of the ring knife 6 is greater than or equal to 79.8 mm, and the sizes of the protective ring 7, the ring knife 6, the sample 5, the permeable plate and the sample cover 3 match each other. The size of the ring knife 6 is reasonably set, and the size of the ring knife 6 is larger than the conventional setting, which is an unconventional selection, so that there are enough samples to measure the retained soil volume and vertical permeability coefficient after the test. The protective ring 7, the ring knife 6, the sample 5, the permeable plate and the sample cover 3 are increased accordingly, and the contact surface between the geotextile and the soil sample should be the same as that in engineering applications.
[0072] A steel ball 2 is provided at the center of the top surface of the sample cover 3, and the axial pressure device 11 is connected to the sample cover 3 through the steel ball to ensure that the force applied to the sample is in the axial direction thereof.
[0073] A shallow groove 15 is provided at the bottom of the water trough 8 for placing the guard ring 7. A drain port 16 is provided at the bottom of the guard ring 7. There are 4 to 6 drain ports 16, which are used as water circulation channels to drain water in time. The diameter of the water trough 8 is 100 to 150 mm, and the height of the water trough 8 is 40 to 80 mm. The size setting is reasonable, which is convenient for taking and placing the guard ring 7, the ring knife 6, the water-permeable plate and the sample cover 3.
[0074] The inner diameter of the shallow groove 15 is smaller than the inner diameter of the guard ring 7 , and the outer diameter of the shallow groove 15 is larger than the outer diameter of the guard ring 7 , which facilitates the positioning and installation of the guard ring.
[0075] The deformation measuring device includes a dial gauge 10 and a meter stand 1. One end of the meter stand 1 is connected to the water tank 8, and the other end of the meter stand 1 is connected to the dial gauge 10. Specifically, the meter stand 1 includes a connecting rod 17 and an adjusting rod 18. The connecting rod 17 and the adjusting rod 18 are vertically arranged. Mounting holes 20 are arranged at both ends of the adjusting rod 18. A connecting hole 19 is arranged on the outer wall of the water tank 8. The mounting hole 20 at one end of the adjusting rod 18 is connected and fixed to the dial gauge 10. The mounting hole 20 at the other end of the adjusting rod 18 is connected to one end of the connecting rod 17. The other end of the connecting rod 17 is connected to the connecting hole 19 on the outer wall of the water tank 8. The distance between the adjusting rod 18 and the connecting rod 17 and the adjusting rod 18 and the dial gauge 10 is adjusted to ensure the accuracy of the test. The dial gauge 10 has a range of 10 to 20 mm, a minimum graduation of 0.01 mm, high precision and reliability, and meets the test needs.
[0076] The deformation measuring device adopts a displacement sensor, and the displacement sensor adopts a zero-level displacement sensor, which can be a strain sensor, inductance sensor, differential transformer sensor, eddy current sensor, or Hall sensor. It has high accuracy and reliability and meets the test needs.
[0077] The axial pressure device 11 adopts a hydraulic, pneumatic, lever or scale type device, and can be implemented using existing products.
[0078] The inner diameter of the ring cutter is 79.8-90mm, and the height of the ring cutter 6 is 20-50mm; the diameters of the top geotextile 4 and the bottom geotextile 9 are 79.8-90mm, and the size setting is appropriate. The contact surface between the geotextile and the soil sample should be the same as in engineering applications.
[0079] The inner diameter of the guard ring 7 is larger than the outer diameter of the ring cutter 6 , and the inner diameter of the guard ring 7 is 81.1-91.4 mm. The height of the guard ring 7 is larger than the height of the ring cutter 6 , and the height is 23-53 mm, so that the ring cutter 6 can be easily taken in and out.
[0080] The thickness of the top water-permeable plate 9 and the bottom water-permeable plate 9 is 5-10 mm, the diameter of the bottom water-permeable plate is slightly smaller than the inner diameter of the guard ring, and the diameter is 79.8-91 mm, and the diameter of the top water-permeable plate is smaller than the inner diameter of the ring cutter, and the diameter is 79.4-89.7 mm;
[0081] The diameter of the sample cover 3 is smaller than the inner diameter of the ring cutter 6, and the diameter of the sample cover is 79.4-89.7 mm.
[0082] The geotextile axial compression clogging test method is characterized by comprising the following steps:
[0083] Step 1. Prepare the sample: Cut 2 pieces of geotextiles with a diameter of 79.8 mm or more, measure the area and weigh them, and measure their thickness according to the geotextile thickness measurement test method. The geotextile and the permeable plate are saturated with water. Use a ring cutter to cut the original soil sample or fill the disturbed soil sample in the ring cutter. If the soil sample is unsaturated, a saturated soil sample is required. Place geotextiles on the top and bottom of the soil sample respectively. The contact surface between the geotextile and the soil sample should be the same as in the engineering application to simulate the working state of the geotextile;
[0084] Step 2: Install the sample: Place the guard ring into the shallow groove of the water tank, place the permeable plate with a slightly larger diameter into the guard ring, apply a layer of vaseline on the outer wall of the ring cutter, and place the cutting edge downward into the guard ring until it contacts the bottom permeable plate. Place the top permeable plate and the sample cover on the sample in turn;
[0085] Step 3: Connect the axial pressure device: The axial pressure device is connected to the steel ball on the sample cover to ensure that the force direction of the sample is perpendicular to its cross section;
[0086] Step 4: Install the deformation measuring device: Use the axial pressure device to apply a pre-pressure of 1 kPa to the sample to make all parts in close contact, wrap the sample with moisturizing materials such as wet cotton yarn and keep it moisturized during the entire test process, install a dial indicator or displacement sensor, unload, and adjust the deformation reading to zero;
[0087] Step 5. Apply axial pressure: Design the axial load sequence according to the strength of the soil and the test requirements. For soils with high water content and low strength, a vertical load of 1 to 5 kPa should be applied first. After the load is applied, the deformation of the sample at different times, that is, the height change, is recorded. The deformation stability standard is that the deformation in the last hour does not exceed 0.001 to 0.01 mm. After the deformation stabilizes, the load is applied step by step according to the load sequence.
[0088] Step 6: After the test, unload, remove the sample, peel off the geotextile, remove the surface soil, quickly put a piece of geotextile into the permeameter, and measure its vertical permeability coefficient according to the vertical permeability test method of geotextile. After the piece of geotextile is air-dried, weigh it;
[0089] Step 7, thickness measurement: It is necessary to calculate the comprehensive permeability coefficient of the sample, the consolidation coefficient of the soil sample, the compression modulus of the soil sample and other parameters. If the change of the thickness of the geotextile with the load cannot be ignored, it is also necessary to cut the geotextile and measure its thickness according to the axial load sequence of the test according to the geotextile thickness measurement test method. The height change of the soil sample is calculated according to the deformation of the sample and the change of the thickness of the geotextile;
[0090] The calculation formula of soil sample deformation under a certain load level is:
[0091] H=(h0-h1)-(t0-t1)
[0092] Where H is the deformation of the soil sample under a certain level of load, mm; h0 is the height of the sample at the end of the previous level of load, mm; h1 is the height of the sample at the end of a certain level of load, mm; t0 is the thickness of the geotextile under the previous level of load, mm; t1 is the thickness of the geotextile under a certain level of load, mm.
[0093] Step 8. Calculation: Calculate the amount of retained soil and the reduction in the vertical permeability coefficient of geotextiles.
[0094] The calculation formula for the amount of retained soil is:
[0095] Where η is the amount of soil retained by the geotextile, g / cm 2 ; m is the mass of geotextile, g; m1 is the mass of geotextile and soil after the test, g; A is the area of geotextile, cm 2 ;
[0096] The calculation formula for the reduction of vertical permeability coefficient of geotextiles is:
[0097]
[0098] Where K is the reduced vertical permeability of geotextile; k0 is the initial vertical permeability of geotextile, cm / s; k1 is the vertical permeability of geotextile after the test, cm / s.
[0099] Example 1
[0100] See attached Figure 1 The geotextile axial compression method clogging test device comprises a sample container, a deformation measuring device and an axial pressure device 11. The sample container comprises a water tank 8, a retaining ring 7, a ring knife 6, a water-permeable plate and a sample cover 3. The retaining ring 7, the water-permeable plate and the sample cover 3 are sequentially arranged in the water tank 8. The deformation measuring device and the axial pressure device 11 are in contact with and connected to the sample cover 3. The overall connection is convenient and easy to implement. The structure is reasonably arranged and convenient for measurement.
[0101] The water-permeable plate includes a top water-permeable plate 4 and a bottom water-permeable plate 9, a ring knife 6 is arranged between the top water-permeable plate 4 and the bottom water-permeable plate 9, and the bottom water-permeable plate 4, the ring knife 6, the top water-permeable plate 9 and the sample cover 3 are arranged in the protective ring 7 from bottom to top, and the sample 5 is arranged in the ring knife 6. Figure 4 The sample 5 includes a bottom geotextile 14, a soil sample 13, and a top geotextile 12 arranged from bottom to top. The inner diameter of the ring cutter 6 is equal to 79.8 mm. The sizes of the retaining ring 7, the ring cutter 6, the sample 5, the permeable plate and the sample cover 3 match. The size of the ring cutter 6 is reasonably set. The size of the ring cutter 6 is larger than the conventional setting. The unconventional selection is convenient for having enough samples to measure the retained soil volume and the vertical permeability coefficient after the test. The retaining ring 7, the ring cutter 6, the sample 5, the permeable plate and the sample cover 3 are increased accordingly. The contact surface between the geotextile and the soil sample should be the same as that in engineering applications.
[0102] A steel ball 2 is provided at the center of the top surface of the sample cover 3, and the axial pressure device 11 is connected to the sample cover 3 through the steel ball to ensure that the force applied to the sample is in the axial direction thereof.
[0103] See attached Figure 5 , there are several drain holes 16 at the bottom of the guard ring 7. Figure 6 , a shallow groove 15 is provided at the bottom of the water tank 8. A shallow groove 15 is provided at the bottom of the water tank 8 for placing the guard ring 7. A drain port 16 is provided at the bottom of the guard ring 7. There are 4-6 drain ports 16, which are used as a water flow channel to drain water in time. The diameter of the water tank 8 is 100-150 mm, and the height of the water tank 8 is 40-80 mm. The size setting is reasonable, which is convenient for taking and placing the guard ring 7, the ring knife 6, the water-permeable plate and the sample cover 3.
[0104] The clogging test device of geotextile axial compression method is to load the sample 5 into the ring cutter 6. The sample includes the top geotextile 12, soil sample 13, and bottom geotextile 14 arranged from top to bottom. The guard ring 7 is placed into the shallow groove 15 of the water tank 8. The bottom water-permeable plate 9, the ring cutter 6, the top water-permeable plate 4, and the sample cover 3 are placed in the guard ring 7 in sequence. The cutting edge of the ring cutter 6 is downward. The axial pressure device 11 is adjusted to contact with the steel ball 2. The dial indicator 10 is installed on the table frame 1 and contacts with the sample cover 3 for measurement. The overall structure is simple and the design is reasonable. Through the axial pressure device, the water of the soil sample itself drives the soil particles to migrate under the action of pressure, thereby causing the clogging of the geotextile. This solves the problem that the traditional gradient ratio method must use an external water source to provide a hydraulic gradient, and must read the water level of the pressure tube and calculate the permeability coefficient through the seepage of the soil body. There may be an error between the water level of the pressure tube and the actual water head.
[0105] The meter frame 1 includes a connecting rod 17 and an adjusting rod 18, which are arranged vertically. Mounting holes 20 are arranged at both ends of the adjusting rod 18, and a connecting hole 19 is arranged on the outer wall of the water tank 8. The mounting hole 20 at one end of the adjusting rod 18 is connected and fixed to the dial gauge 10, and the mounting hole 20 at the other end of the adjusting rod 18 is connected to one end of the connecting rod 17, and the other end of the connecting rod 17 is connected to the connecting hole 19 on the outer wall of the water tank 8. The distance between the dial gauge 10 and the sample cover 3 is adjusted by adjusting the distance between the adjusting rod 18 and the connecting rod 17, and between the adjusting rod 18 and the dial gauge 10 to ensure the accuracy of the test. The dial gauge 10 has a range of 10 to 20 mm, and a minimum division of 0.01 mm, with high precision and reliability, meeting the test needs.
[0106] The top geotextile 12 and the bottom geotextile 14 are respectively placed with a geotextile having a diameter of 79.8 mm, and the size is set appropriately, and the contact surface between the geotextile and the soil sample should be the same as in the engineering application.
[0107] The inner diameter of the ring cutter 6 is 79.8 mm, the height is 20-50 mm, it has a certain rigidity, and the inner wall is smooth, which is convenient for sampling.
[0108] The top permeable plate 4 and the bottom permeable plate 9 are made of non-corrosive materials, with a permeability coefficient greater than that of the sample 5, a thickness of 5 to 10 mm, and a certain rigidity. The vertical deformation generated during the test can be ignored. The diameter of the bottom permeable plate 9 is slightly smaller than the inner diameter of the guard ring, with a diameter of 79.8 to 81 mm, which is convenient for taking and placing. The diameter of the top permeable plate 4 is slightly smaller than the inner diameter of the ring cutter 6, with a diameter of 79.4 to 79.7 mm, which is convenient for pressing on the top geotextile 12 in the ring cutter 6.
[0109] The inner diameter of the guard ring 7 is slightly larger than the outer diameter of the ring cutter 6, and the height is slightly larger than the height of the ring cutter 6, which is 23-53 mm. It has a certain rigidity and a drain port 16 at the bottom, which is used as a water flow channel and plays a drainage role, which meets the actual engineering application.
[0110] The diameter of the sample cover 3 is slightly smaller than the inner diameter of the ring cutter 6, with a diameter of 79.4-79.7 mm, a smooth surface, and a certain rigidity, so that the deformation generated during the test can be ignored. A steel ball 2 is provided at the center of the top surface of the sample cover 3.
[0111] The dial indicator 10 has a measuring range of 10 to 20 mm and a minimum graduation of 0.01 mm. It is placed on the surface of the sample cover 3 , and the meter stand 1 is used to fix the dial indicator 10 .
[0112] The axial pressure device 11 is connected to the steel ball 2 on the sample cover 3, and can be a hydraulic, pneumatic, lever or scale type device.
[0113] The specific steps of the geotextile axial compression clogging test method are as follows:
[0114] ① Prepare sample 5: Cut the top geotextile 12 and bottom geotextile 14 with a diameter of 79.8 mm, determine their area and weigh them, measure their thickness, immerse the top and bottom geotextiles 12, 14 and the permeable plates 4, 9 in water and saturate them, use the ring knife 6 to cut the original soil sample 13 or fill the disturbed soil sample 13 in the ring knife 6, if the soil sample 13 is unsaturated, a saturated soil sample is required, place the bottom geotextile 14 at the bottom of the soil sample, and place the top geotextile 12 at the top of the soil sample, the contact surface between the top geotextile 12 and the bottom geotextile 14 and the soil sample 13 should be the same as that in engineering applications to simulate the working state of the geotextile;
[0115] ②Install the sample 5: Place the guard ring 7 into the shallow groove 15 of the water tank 8, place the bottom water-permeable plate 9 into the guard ring 7, apply a layer of vaseline on the outer wall of the ring cutter 6 carrying the sample 5, and place the cutting edge downward into the guard ring 7 until it contacts the bottom water-permeable plate 9. Place the top water-permeable plate 9 and the sample cover 3 on the sample 5 in sequence;
[0116] ③ Connect the axial pressure device 11: The axial pressure device 11 is connected to the steel ball 2 on the sample cover 3 to ensure that the force direction of the sample is perpendicular to the cross section;
[0117] ④ Install the deformation measuring device: use the axial pressure device 11 to apply a pre-pressure of 1 kPa to the sample 5, so that all parts are in close contact, wrap the sample with moisturizing materials such as wet cotton yarn and keep it moist during the entire test process, install the dial indicator 10 on the table frame 1, adjust the table frame 1 so that the dial indicator 10 is in contact with the sample cover 3, or install the displacement sensor, unload, and adjust the deformation reading to zero;
[0118] ⑤ Apply axial pressure: Design the axial load sequence according to the strength of the soil and the test requirements. For soils with high water content and low strength, a vertical load of 1 to 5 kPa should be applied first. After the load is applied, the deformation of the sample at different times, that is, the height change, is recorded. The deformation stability standard is that the deformation in the last hour does not exceed 0.001 to 0.01 mm. After the deformation stabilizes, the load is applied step by step according to the load sequence.
[0119] ⑥ After the test, unload, remove the sample, peel off the geotextile, remove the surface soil, quickly put a piece of geotextile into the permeameter, and determine its vertical permeability coefficient according to the vertical permeability test method of geotextile. After a piece of geotextile is air-dried, weigh it; then determine its vertical permeability coefficient according to the vertical permeability test method of geotextile; push out soil sample 5, and conduct necessary tests on soil sample 5 as needed.
[0120] ⑦Calculation: Calculate the amount of retained soil and the reduction of the vertical permeability coefficient of geotextiles. ⑧
[0121] Retained soil volume:
[0122] In the formula
[0123] η——The amount of soil retained by geotextile, g / cm 2 ;
[0124] m0——mass of geotextile, g;
[0125] m1——mass of geotextile and soil after the test, g;
[0126] A——area of geotextile, cm 2 .
[0127] Reduction of vertical permeability coefficient of geotextiles:
[0128]
[0129] K——reduction of vertical permeability coefficient of geotextile;
[0130] k0——initial vertical permeability of geotextile, cm / s;
[0131] k1——vertical permeability coefficient of geotextile after test, cm / s.
[0132] Example 2
[0133] In the technical scheme of the test device of the geotextile axial compression method clogging test method, the displacement sensor adopts a zero-level displacement sensor, and a linear displacement Hall sensor can be used. Placed on the surface of the sample cover 3, the sensor has high accuracy and high reliability, meeting the test needs. The displacement sensor can also be a photoelectric displacement sensor, eliminating mechanical contact, long life and high reliability.
[0134] In the technical scheme of the geotextile axial compression clogging test method, steps ⑥ and ⑦ also include a thickness measurement step, as follows
[0135] It is necessary to calculate the comprehensive permeability coefficient of the sample, the consolidation coefficient of the soil sample, the compression modulus of the soil sample and other parameters. If the change of the thickness of the geotextile with the load cannot be ignored, it is also necessary to cut the geotextile and measure its thickness according to the axial load sequence of the test according to the geotextile thickness measurement test method. The height change of the soil sample is calculated based on the deformation of the sample and the change of the geotextile thickness.
[0136] The calculation formula of soil sample deformation under a certain load level is:
[0137] H=(h0-h1)-(t0-t1)
[0138] Where H is the deformation of the soil sample under a certain level of load, mm; h0 is the height of the sample at the end of the previous level of load, mm; h1 is the height of the sample at the end of a certain level of load, mm; t0 is the thickness of the geotextile under the previous level of load, mm; t1 is the thickness of the geotextile under a certain level of load, mm.
[0139] Other technical solutions are the same as those in Example 1.
[0140] Compared with the existing technology, the overall structure is simple and the design is reasonable. Through the axial pressure device, the water in the soil sample itself drives the soil particles to migrate under the action of pressure, thereby causing the clogging of the geotextile. This solves the problem that the traditional gradient ratio method must use an external water source to provide hydraulic gradient, must read the water level of the piezometer and calculate the permeability coefficient through the seepage of the soil, there may be an error between the water level of the piezometer and the actual water head, and it cannot be used for the clogging test when the geotextile is used as a filter layer of low permeability soil. The clogging test of the geotextile axial compression method does not need to measure the seepage of the soil, which solves the problem that it is impossible to conduct a clogging test of geotextiles in low permeability soil.
[0141] Each container of the geotextile axial compression clogging test device can hold two samples for simultaneous testing. The axial compression clogging test soil sample can use the original soil sample, which can directly reflect the anti-filtration and drainage effect of the soil and geotextile.
[0142] The judgment of clogging is usually evaluated by the reduction of water flow through the fabric and the increase of soil particles entering the fabric. The reduction of flow in the gradient ratio method clogging test is expressed by the gradient ratio, and the reduction of flow in the geotextile axial compression method clogging test is quantitatively expressed by the reduction of the vertical permeability coefficient of the geotextile. The soil particles entering the fabric are expressed by the amount of soil retained per unit area of the geotextile after the test. Compared with the two results, the vertical permeability reduction is more intuitive and easier to understand than the gradient ratio; due to the large difference in thickness of different fabrics, the amount of soil retained per unit area is more suitable for comparing their clogging characteristics than the amount of soil retained per unit volume. Comparing the two clogging test methods, the gradient ratio method saturates the soil with an external water source and provides a water head. The water penetrates into the soil and drives the migration of soil particles. The measured values are the water head of the pressure tube, the amount of infiltrated water and the mass of the sample. The test results are the gradient ratio and the soil content per unit volume. It is suitable for testing the clogging of fabrics in soils with a certain permeability coefficient. The axial compression method forces the self-water in the soil to be discharged by applying external pressure to drive the migration of soil particles for clogging tests. The measured values are the sample height, thickness, mass and permeability of geotextiles. The test results are the reduction of vertical permeability coefficient and the amount of retained soil per unit area. It is suitable for testing the clogging of geotextiles in soils with low permeability coefficient and high saturation and when there is a vertical load.
[0143] This technical solution can be used not only for the clogging test of geotextiles in low permeability soils, but also for the clogging test of geotextiles in general permeability soils, and has a wide range of applications. When testing the clogging characteristics of geotextiles, this technical solution can also test the influence of vertical loads on the clogging characteristics of geotextiles. Geotextiles are affected by overburden pressure during operation, and the axial compression clogging test can study the clogging performance of geotextiles under specific vertical pressure, which is not possible with conventional gradient ratio tests.
[0144] This technical solution can apply axial pressure according to actual needs to measure the clogging characteristics of geotextiles under a certain vertical pressure, and can simulate the overburden pressure or surrounding pressure on geotextiles during engineering applications.
[0145] Using saturated soil samples, this technical solution can calculate the change in the soil porosity by recording the height change of the sample and the thickness change of the geotextile under axial pressure, thereby calculating the amount of water discharged from the soil, and thus calculating the comprehensive permeability coefficient of the sample composed of geotextile and soil, and can also derive the consolidation characteristics of the soil.
[0146] The test shows that the soil retention and vertical permeability coefficient of the plastic drainage board filter membrane measured by the geotextile axial compression clogging test method are very close to those of the plastic drainage board filter membrane after construction, with an error of 5-26%, and the results of the axial compression clogging test method are slightly smaller than those of the plastic drainage board filter membrane after construction. Since the plastic drainage board filter membrane works for several months and the clogging mechanism is more complicated, it is very reasonable that the results of the geotextile axial compression clogging test method are slightly smaller than the actual results.
[0147] Table 1 Comparison of clogging test results of geotextile after construction and axial compression method
[0148]
[0149] The present invention does not require an additional water source, uses a small amount of soil, adopts conventional instruments and equipment, has simple operation, fast test speed, and stable and reliable results.
[0150] The above is a detailed description of an example of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. Geotextile axial compression clogging test method, the test device used includes a sample container, a deformation measuring device and an axial pressure device, characterized in that: The sample container comprises a water tank, a guard ring, a ring knife, a water permeable plate and a sample cover, wherein the guard ring, the water permeable plate, the ring knife and the sample cover are sequentially arranged in the water tank, the deformation measuring device and the axial pressure device are in contact with the sample cover, the deformation measuring device comprises a dial indicator and a meter stand, one end of the meter stand is connected to the water tank, and the other end of the meter stand is connected to the dial indicator, or the deformation measuring device is composed of a displacement sensor; The water-permeable plate comprises a top water-permeable plate and a bottom water-permeable plate, a ring knife is arranged between the top water-permeable plate and the bottom water-permeable plate, the bottom water-permeable plate, the ring knife, the top water-permeable plate and the sample cover are arranged in the guard ring from bottom to top, the sample is arranged in the ring knife, the inner diameter of the ring knife is greater than or equal to 79.8 mm, and the sizes of the guard ring, the ring knife, the sample, the water-permeable plate and the sample cover match; A steel ball is provided at the center of the top surface of the sample cover, and the axial pressure device is in contact and connected with the sample cover through the steel ball; a shallow groove is provided at the bottom of the water tank for placing the guard ring, and a drain port is provided at the bottom of the guard ring for serving as a water circulation channel; The diameter of the inner edge of the shallow groove is smaller than the inner diameter of the guard ring, and the diameter of the outer edge of the shallow groove is larger than the outer diameter of the guard ring; The specimens were prepared by placing earth fabric on the top and bottom of the soil sample; The following steps are involved: Step 1. Prepare the sample: Cut 2 pieces of geotextiles with a diameter of 79.8 mm or more, measure the area and weigh them, and measure their thickness according to the geotextile thickness measurement test method. The geotextile and the permeable plate are saturated with water. Use a ring cutter to cut the original soil sample or fill the disturbed soil sample in the ring cutter. If the soil sample is unsaturated, a saturated soil sample is required. Place geotextiles on the top and bottom of the soil sample respectively. The contact surface between the geotextile and the soil sample should be the same as in the engineering application to simulate the working state of the geotextile; Step 2: Install the sample: Place the guard ring into the shallow groove of the water tank, place the permeable plate with a slightly larger diameter into the guard ring, apply a layer of vaseline on the outer wall of the ring cutter, place the cutting edge downward into the guard ring until it contacts the bottom permeable plate, and place the top permeable plate and the sample cover on the sample in sequence; Step 3: Connect the axial pressure device: The axial pressure device is connected to the steel ball on the sample cover to ensure that the force direction of the sample is perpendicular to its cross section; Step 4: Install the deformation measuring device: Use the axial pressure device to apply a pre-pressure of 1 kPa to the sample to make all parts in close contact, wrap the sample with moisturizing material and keep it moisturized during the entire test process, install a dial indicator or displacement sensor, unload, and adjust the deformation reading to zero; Step 5: Apply axial pressure: Design the axial load sequence according to the strength of the soil and the test requirements. For soil with high water content and low strength, a vertical load of 1 to 5 kPa should be applied first. After the load is applied, the deformation of the sample at different times, that is, the height change, is recorded. The deformation stability standard is that the deformation in the last hour does not exceed 0.001 to 0.01 mm. After the deformation is stable, the load is applied step by step according to the load sequence. Step 6: After the test, unload, remove the sample, peel off the geotextile, remove the surface soil, quickly put a piece of geotextile into the permeameter, and measure its vertical permeability coefficient according to the vertical permeability test method of geotextile. After the piece of geotextile is air-dried, weigh it; Step 7. Calculation: Calculate the amount of retained soil and the reduction in the vertical permeability coefficient of geotextiles.
2. The geotextile axial compression clogging test method according to claim 1, characterized in that The dial indicator has a measuring range of 10 to 20 mm and a minimum division of 0.01 mm.
3. The geotextile axial compression clogging test method according to claim 1, characterized in that The displacement sensor adopts a zero-order displacement sensor.
4. The geotextile axial compression clogging test method according to claim 1, characterized in that The axial pressure device is a hydraulic, pneumatic, lever or scale type device.
5. The geotextile axial compression clogging test method according to claim 1, characterized in that The thickness measurement step is also included between step 6 and step 7, which is as follows: It is necessary to calculate the comprehensive permeability coefficient of the sample, the consolidation coefficient of the soil sample, and the compression modulus parameters of the soil sample. If the change of the thickness of the geotextile with the load cannot be ignored, it is also necessary to cut the geotextile and measure its thickness according to the axial load sequence of the test according to the geotextile thickness measurement test method. The height change of the soil sample is calculated based on the deformation of the sample and the change of the geotextile thickness. The calculation formula of soil sample deformation under a certain load level is: H=(h0-h1)-(t0-t1) Where H is the deformation of the soil sample under a certain level of load, mm; h0 is the height of the sample at the end of the previous level of load, mm; h1 is the height of the sample at the end of a certain level of load, mm; t0 is the thickness of the geotextile under the previous level of load, mm; t1 is the thickness of the geotextile under a certain level of load, mm.
6. The geotextile axial compression clogging test method according to claim 5, characterized in that The calculation formula of the amount of retained soil in step 7 is: Where η is the amount of soil retained by the geotextile, g / cm 2 ; m0 is the mass of geotextile, g; m1 is the mass of geotextile and soil after the test, g; A is the area of geotextile, cm 2 ; The calculation formula for the reduction of vertical permeability coefficient of geotextiles is: Where K is the reduced vertical permeability coefficient of geotextile; k0 is the initial vertical permeability coefficient of geotextile, cm / s; k1 is the vertical permeability coefficient of geotextile after the test, cm / s.