Back contact solar cell and preparation method thereof

By adopting specific structures and processes of P-type crystalline silicon substrates in back contact solar cells, including tunneling oxide layers, n+ doped polysilicon regions, laser grooves and passivation films, the insufficient coverage of metal electrodes on the back surface and the preparation cost are solved. High-quality problems achieve high-efficiency energy conversion and low-cost production.

CN108110065BActive Publication Date: 2024-11-29JOLYWOOD (TAIZHOU) SOLAR TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN201810067107.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-01-24
Publication Date
2024-11-29
Estimated Expiration
2038-01-24

AI Technical Summary

Technical Problem

The existing back contact solar cells are costly during the preparation process, and the metal electrode coverage area on the back surface is insufficient, which affects the energy conversion efficiency of the battery.

Method used

The back surface structure of the P-type crystal silicon matrix is ​​adopted, including tunneled oxide layer, alternating n+ doped polysilicon region, laser grooved region, passivation film and metal electrode, and the process is simplified through the ohmic contact between silver electrode and aluminum electrode. Process and reduce costs.

Benefits of technology

The passivation contact and field passivation effects of the back surface are realized, the recombination rate is reduced, the open circuit voltage and short circuit current is improved, the manufacturing cost is reduced, and the quantum efficiency in the short-band is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN108110065B_ABST
    Figure CN108110065B_ABST
Patent Text Reader

Abstract

The invention relates to a back contact solar cell, comprising a P-type crystalline silicon substrate, the back surface of which includes a tunneling oxide layer, an alternating back surface n+ doped polysilicon region and a laser grooved region, a passivation film and a metal electrode from the inside to the outside; the metal electrode includes a silver electrode in ohmic contact with the back surface n+ doped polysilicon region and an aluminum electrode in ohmic contact with the back surface laser grooved region; the front surface includes a p+ doped region and a front surface passivation anti-reflection film from the inside to the outside. The beneficial effects are: the emitter region on the back surface of the P-type crystalline silicon substrate adopts an n+ doped polysilicon passivation layer, the back surface is formed by an aluminum paste electrode to form a p+ region and is passivated by an aluminum oxide film, the passivation contact and field passivation effect of the back surface are realized, the recombination rate of the back surface of the battery is reduced, and the open circuit voltage and short circuit current are improved; and the back p+ region is formed by aluminum paste, which reduces one diffusion doping step compared with the traditional process, simplifies the process flow, and saves the battery cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cells, and in particular to a back-contact solar cell and a preparation method thereof. Background Art

[0002] Solar cells are semiconductor devices that convert light energy into electrical energy. Low production costs and high energy conversion efficiency have always been the goals pursued by the solar cell industry. For current conventional solar cells, the p+ doped region contact electrode and the n+ doped region contact electrode are located on the front and back sides of the cell, respectively. The front side of the cell is the light-receiving side, and the coverage of the front metal contact electrode will inevitably cause a portion of the incident sunlight to be blocked and reflected by the metal electrode, resulting in some optical loss. The coverage area of ​​the front metal electrode of an ordinary crystalline silicon solar cell is about 7%. Reducing the front coverage of the metal electrode can directly improve the energy conversion efficiency of the cell.

[0003] A back-contact battery is a battery in which both the p+ doped region and the n+ doped region are placed on the back side of the battery (non-light-receiving side). The light-receiving side of the battery is not blocked by any metal electrode, which effectively increases the short-circuit current of the battery cell and improves the energy conversion efficiency of the battery cell.

[0004] The solar cell with back contact structure is the one with the highest energy conversion efficiency among the crystalline silicon solar cells currently mass-produced by solar energy industry. Its high conversion efficiency and low component packaging cost have always been favored by people. However, the back surface of the common back contact cell is an N-type silicon substrate, p+ and n+ type doped layers, on which SiN is generally used. x or SiO2 / SiN x As a passivation layer, a burn-through silver paste is then used to penetrate the passivation layer and form an ohmic contact with silicon. The back metal electrode accounts for about 5%-8% of the back surface area, which means that more than 5% of the silicon surface is not covered by the passivation layer, and these areas have serious metal recombination. In addition, the multi-step diffusion and silver paste printing in the preparation process of the back contact battery is an important factor leading to the relatively high cost of the high-efficiency battery. Therefore, a new type of battery that can form a good contact between the metal electrode and the silicon substrate, maintain the integrity of the passivation film, and reduce the manufacturing cost of the back contact battery is a development trend in the field of solar cells. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a back-contact solar cell.

[0006] A back contact solar cell of the present invention has the following technical solution:

[0007] A back-contact solar cell, characterized in that: it includes a P-type crystalline silicon substrate, the back surface of the P-type crystalline silicon substrate includes, from the inside to the outside, a tunneling oxide layer, an alternating back surface n+ doped polysilicon region and a back surface laser grooved region, a back surface passivation film and a back surface metal electrode; the back surface metal electrode includes a first back silver electrode in ohmic contact with the back surface n+ doped polysilicon region and a second back electrode in ohmic contact with the back surface laser grooved region; the front surface of the P-type crystalline silicon substrate includes, from the inside to the outside, a p+ doped region and a front surface passivation anti-reflection film.

[0008] The present invention provides a back-contact solar cell, which also includes the following subsidiary technical solutions:

[0009] Wherein, the front surface of the P-type crystalline silicon substrate is a front surface field formed by a boron-doped region and a front surface passivation anti-reflection film; or, the front surface of the P-type crystalline silicon substrate is a passivation contact front surface field formed by an oxide layer, a p+ doped polysilicon layer and a front surface passivation anti-reflection film.

[0010] Wherein, the front surface passivation anti-reflection film is SiN x , with a thickness of 40 to 80 nm; the oxide layer is SiO2 and / or Al2O3; or the back surface passivation film includes an Al2O3 dielectric film and a SiN x The dielectric film has a thickness of 2 to 10 nm, and the SiN x The thickness of the dielectric film is 40 to 80 nm. ;.

[0011] Wherein, the first back electrode is a silver electrode, and the second back electrode is an aluminum electrode.

[0012] The present invention also provides a method for preparing a back-contact solar cell, comprising the following steps:

[0013] (1) Selecting a P-type crystalline silicon substrate and performing a texturing treatment on the P-type crystalline silicon substrate;

[0014] (2) performing doping treatment on the back surface and the front surface of the P-type crystalline silicon substrate after the treatment in step (1); wherein the doping treatment method for the back surface of the P-type crystalline silicon substrate is: growing a tunneling oxide layer on the back surface of the P-type crystalline silicon substrate, and growing an intrinsic polycrystalline silicon layer or an intrinsic amorphous silicon layer on the tunneling oxide layer, and then injecting phosphorus ions into the intrinsic polycrystalline silicon layer or the intrinsic amorphous silicon layer; and the doping treatment method for the front surface of the P-type crystalline silicon substrate is: injecting boron ions by boron diffusion or ion implantation.

[0015] (3) The P-type crystalline silicon substrate treated in step (2) is subjected to high-temperature annealing treatment, wherein the peak annealing temperature is 800-1100°C and the annealing time is 30-200 minutes. After the annealing is completed, a doped p+ region is formed on the front surface of the P-type crystalline silicon substrate, and an n+ doped emitter is formed on the back surface of the P-type crystalline silicon substrate.

[0016] (4) forming a front surface passivation anti-reflection film on the front surface of the P-type crystalline silicon substrate after the treatment in step (3), and forming a back surface passivation film on the back surface of the P-type crystalline silicon substrate;

[0017] (5) After the treatment in step (4), the back surface of the P-type crystalline silicon substrate is laser grooved, and an aluminum electrode is printed in the laser grooved area to form an ohmic contact with the p+ area, and a silver electrode is printed in the n+ doped area of ​​the back surface to form an ohmic contact with the n+ doped area, thereby completing the production of a back contact solar cell.

[0018] The present invention provides a method for preparing a back-contact solar cell, which also includes the following subsidiary technical solutions:

[0019] Wherein, in step (1), the front surface and the back surface of the P-type crystalline silicon substrate are subjected to texturing treatment; the resistivity of the P-type crystalline silicon substrate is 0.5 to 15Ω·cm, and the thickness is 50 to 300μm.

[0020] Wherein, in step (2), the back surface tunneling oxide layer is SiO2, and its thickness is 1-3nm, and the growth method of SiO2 is high temperature thermal oxidation method, nitric acid oxidation method, ozone oxidation method or CVD deposition method; the method of growing an intrinsic polycrystalline silicon layer or an intrinsic amorphous silicon layer on the back surface tunneling oxide layer is: placing a P-type crystalline silicon substrate in an LPCVD device, and growing an intrinsic polycrystalline silicon layer or an intrinsic amorphous silicon layer on the back surface tunneling oxide layer; and implanting phosphorus atoms into the intrinsic polycrystalline silicon layer or the intrinsic amorphous silicon layer by ion implantation method, and the implantation dose is 1×10 15 cm -2 ~8×10 15 cm -2 The doping treatment method of the front surface of the P-type crystalline silicon substrate is as follows: ion implantation is performed on the front surface, and the implanted elements include phosphorus, and the phosphorus ion implantation dose is 1×10 15 cm -2 ~4×10 15 cm -2 .

[0021] Wherein, in step (3), the peak temperature of the annealing treatment is 800-1100°C, the annealing time is 30-200 min, and the ambient gas source is N2 and O2.

[0022] In step (4), the preparation method of the front surface passivation anti-reflection film is: firstly deposit a layer of SiO with a thickness of 5 to 30 nm on the front surface of the P-type crystalline silicon substrate by using a PECVD device; x The dielectric film is then x A layer of SiN with a thickness of 40 to 80 nm is deposited on the dielectric film. x The preparation method of the back surface passivation film is: first depositing a layer of Al2O3 dielectric film with a thickness of 2 to 20 nm on the back surface of the P-type crystalline silicon substrate using an ALD device, and then depositing a layer of SiN with a thickness of 40 to 80 nm on the Al2O3 dielectric film. x Dielectric film.

[0023] Among them, in step (5), the preparation method of the metal electrode is: printing silver paste on the n+ doped area on the back surface of the P-type crystalline silicon substrate treated in step (4) by screen printing, printing aluminum paste on the laser grooved area, and then sintering.

[0024] The implementation of the present invention includes the following technical effects:

[0025] The present invention provides a back-contact solar cell, in which the emitter region on the back surface of the P-type crystalline silicon substrate adopts an n+ doped polysilicon passivation layer, and the p+ region formed by the aluminum paste electrode on the back surface adopts an aluminum oxide film passivation, realizing the passivation contact and field passivation effect of the back surface, greatly reducing the recombination rate of the back surface of the battery, and improving the open circuit voltage and short circuit current; on the other hand, the back p+ region formed by the aluminum paste reduces one diffusion doping step compared to the traditional process, simplifies the process flow, and saves battery costs. In addition, after the back and back surfaces of the back-contact solar cell provided by the present invention are covered with the passivation film, its implied open circuit voltage (Implied Voc) can reach more than 700mV, and the dark saturation current density J0<20fAcm -2 After the printed electrode is made into a back-junction contact battery, its internal quantum efficiency in the short-wave band reaches more than 98%. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic cross-sectional diagram of the cell structure after step 1 of the method for preparing a back-contact solar cell in an embodiment of the present invention.

[0027] Figure 2 It is a schematic cross-sectional diagram of the cell structure after step 2 of the method for preparing a back-contact solar cell in an embodiment of the present invention.

[0028] Figure 3 It is a schematic cross-sectional diagram of the cell structure after step three of the method for preparing a back-contact solar cell in an embodiment of the present invention.

[0029] Figure 4It is a schematic cross-sectional diagram of the cell structure after step 4 of the method for preparing a back-contact solar cell in an embodiment of the present invention.

[0030] Figure 5 It is a schematic cross-sectional diagram of the cell structure after step five of the method for preparing a back-contact solar cell in an embodiment of the present invention.

[0031] Figure 6 Schematic diagram of the cross-section of the cell structure after step six of the method for preparing a back-contact solar cell in an embodiment of the present invention.

[0032] Figure 7 It is a schematic cross-sectional view of the cell structure after step seven of the method for preparing a back-contact solar cell in an embodiment of the present invention.

[0033] Figure 8 Schematic diagram of the cross-section of the cell structure after step eight of the method for preparing a back-contact solar cell in an embodiment of the present invention. DETAILED DESCRIPTION

[0034] The present invention will be described in detail below in conjunction with embodiments and drawings. It should be pointed out that the described embodiments are only intended to facilitate the understanding of the present invention and do not have any limiting effect on the present invention.

[0035] See also Figures 1 to 8 As shown, the present embodiment provides a method for preparing a back contact solar cell, comprising the following steps:

[0036] (1) Select a P-type crystalline silicon substrate 10, and perform a texturing treatment on the front and back surfaces of the P-type crystalline silicon substrate 10; the resistivity of the P-type crystalline silicon substrate 10 is 0.5 to 15 Ω·cm, preferably 1 to 5 Ω·cm; the thickness of the P-type crystalline silicon substrate 10 is 50 to 300 μm, preferably 120 to 200 μm; the battery structure after completing this step is as follows Figure 1 shown.

[0037] (2) A tunneling oxide layer 20 is grown on the back surface of the P-type crystalline silicon substrate 10 after being treated in step (1). In this embodiment, the tunneling oxide layer 20 is a SiO2 layer. Methods for growing the tunneling oxide layer 20 include high-temperature thermal oxidation, nitric acid oxidation, ozone oxidation or CVD deposition (chemical vapor deposition) and the like. This embodiment adopts a wet ozone oxidation method, wherein the P-type crystalline silicon substrate 10 is placed in deionized water, and then ozone is introduced into the deionized water so that the ozone concentration reaches 20-50ppm, the reaction temperature is 30-50°C, the reaction time is 5-20min, and the thickness of the grown tunneling oxide layer 20 is 1-3nm. The battery structure after completing this step is as follows: Figure 2 shown.

[0038] (3) Place the P-type crystalline silicon substrate 10 treated in step (2) into the LPCVD device, and grow an intrinsic polysilicon layer or an intrinsic amorphous silicon layer 11 on its back surface. The thickness of the intrinsic polysilicon layer or the intrinsic amorphous silicon layer is 100-200nm. The battery structure after completing this step is as follows: Figure 3 shown.

[0039] (4) Phosphorus atoms are implanted into the intrinsic polysilicon layer or the intrinsic amorphous silicon layer 11 of the P-type crystalline silicon substrate 10 after the treatment in step (3) by ion implantation, and the implantation dose of phosphorus atoms is 1×10 15 cm -2 ~8×10 15 cm -2 , and then put it into an annealing furnace for high temperature annealing. The peak temperature of the annealing treatment is 800-1100°C, the annealing time is 30-200 minutes, and the ambient gas source is N2 and O2. After the annealing treatment, the intrinsic polysilicon layer or the intrinsic amorphous silicon layer 11 is converted into an n+ doped polysilicon region 12. The battery structure after completing this step is as follows Figure 4 shown.

[0040] (5) Laser grooves are performed on the P-type crystalline silicon substrate 10 after the treatment in step (4), and the width of the linear opening pattern of the grooves is 50 to 400 μm, preferably 100 to 300 μm. The battery structure after the grooves are completed in this step is as shown in FIG. Figure 5 shown.

[0041] (6) The P-type crystalline silicon substrate 10 treated in step (5) is implanted with boron atoms by ion implantation, and the implantation dose of boron atoms is 1×10 15 cm -2 ~4×10 15 cm -2 , and then put it into an annealing furnace for high temperature annealing. The peak temperature of the annealing treatment is 800-1100°C, the annealing time is 30-200min, and the ambient gas source is N2 and O2. After annealing, a p+ front surface 14 is formed. Or, the P-type crystalline silicon substrate 10 treated in step (5) is placed in an industrial diffusion furnace to diffuse boron on the textured surface to form a p+ doped area on the front surface. The boron source is boron tribromide, the diffusion temperature is 900-1000°C, the time is 60-180 minutes, and the square resistance after boron diffusion is 40-200Ω / sqr. The battery structure after completing this step is as follows Figure 6 shown.

[0042] (7) A passivation film 21 and a passivation anti-reflection film 22 are grown on the front surface of the P-type crystalline silicon substrate 10 after the treatment in step (6). The passivation film 21 can be one or more of SiO2 and Al2O3 dielectric films, and the passivation anti-reflection film can be SiN xThe film has a thickness of 40 to 80 nm; a passivation film 23 and 24 are grown on the back surface of the P-type crystalline silicon substrate 10, the passivation film 23 is Al2O3, and the passivation film 24 is SiN x Dielectric film: A 2-10 nm thick Al2O3 dielectric film is first deposited using ALD equipment, and then a 40-80 nm thick SiN layer is deposited on the Al2O3 dielectric film. x The dielectric film 24. After completing this step, the battery structure is as follows Figure 7 shown.

[0043] (8) A metal electrode 30 is printed on the n+ doped area on the back surface of the P-type crystalline silicon substrate 10 using silver paste and then dried, and a metal electrode 31 is printed on the grooved area using aluminum paste and then dried. Both the silver paste and the aluminum paste are the types commonly used in the existing P-type battery process. The battery structure after completing this step is as follows: Figure 8 shown.

[0044] (9) The P-type crystalline silicon substrate 10 processed in step (8) is transferred into a belt sintering furnace for sintering. The sintering peak temperature is 850-950° C., thereby completing the preparation of a back-contact solar cell.

[0045] Preferably, the front surface of the P-type crystalline silicon substrate can be a front surface field formed by a boron-doped region and a passivation anti-reflection film, or can be a passivation contact front surface field formed by an oxide layer, a p+-doped polysilicon layer and a passivation anti-reflection film.

[0046] See also Figure 8 As shown, a back-contact solar cell provided in this embodiment includes a P-type crystalline silicon substrate 10, the back surface of the P-type crystalline silicon substrate 10 includes, from the inside to the outside, a tunneling oxide layer 20, alternatingly arranged back surface n+ doped polysilicon regions 12 and back surface laser grooved regions, a back surface passivation film and a back surface metal electrode; the back surface metal electrode includes a first back electrode 30 in ohmic contact with the back surface n+ doped polysilicon region 12 and a second back electrode 31 in ohmic contact with the back surface laser grooved region; the front surface of the P-type crystalline silicon substrate includes, from the inside to the outside, a p+ doped region 14 and a front surface passivation anti-reflection film.

[0047] Preferably, the first back electrode 30 is a back silver electrode, and the second back electrode 31 is a back aluminum electrode. The passivation film 21 on the front surface can be one or more of SiO2 and Al2O3 dielectric films, and the passivation anti-reflection film is SiN xThe passivation film 23 and 24 are grown on the back surface of the P-type crystalline silicon substrate 10. The passivation film 23 is Al2O3. A layer of Al2O3 dielectric film 23 with a thickness of 2 to 10 nm is first deposited by ALD equipment, and then a layer of SiN with a thickness of 40 to 80 nm is deposited on the Al2O3 dielectric film. x The dielectric film 24 .

[0048] After the back contact solar cell with the above structure is passivated on the front and back surfaces, it is tested that its implied open circuit voltage (Implied Voc) can reach more than 700mV and the dark saturation current density J0<20fA﹒cm -2 After the back-contact battery is made of printed electrodes, its internal quantum efficiency in the short-wave band reaches more than 98%.

[0049] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A back contact solar cell, Features: The invention comprises a P-type crystalline silicon substrate, wherein the back surface of the P-type crystalline silicon substrate comprises, from the inside to the outside, a tunneling oxide layer, an alternately arranged back surface n+ doped polysilicon region and a back surface laser grooved region, a back surface passivation film and a back surface metal electrode; the back surface metal electrode comprises a first back electrode in ohmic contact with the back surface n+ doped polysilicon region and a second back electrode in ohmic contact with the back surface laser grooved region; the front surface of the P-type crystalline silicon substrate comprises, from the inside to the outside, a p+ doped region and a front surface passivation anti-reflection film; The back surface passivation film includes Al 2 O 3 Dielectric film and deposited on Al 2 O 3 SiN on the back surface of the dielectric film x Dielectric film; The first back electrode is a silver electrode, and the second back electrode is an aluminum electrode; The tunnel oxide layer is SiO 2 .

2. A back contact solar cell according to claim 1, Features: The front surface of the P-type crystalline silicon substrate is a front surface field formed by a boron-doped region and a front surface passivation anti-reflection film; or, the front surface of the P-type crystalline silicon substrate is a passivation contact front surface field formed by an oxide layer, a p+ doped polysilicon layer and a front surface passivation anti-reflection film.

3. A back contact solar cell according to claim 2, Features: The front surface passivation anti-reflection film is SiN x , with a thickness of 40 to 80 nm; the oxide layer is SiO 2 and / or Al 2 O 3 ; or, the Al 2 O 3 The thickness of the dielectric film is 2 to 10 nm. x The thickness of the dielectric film is 40 to 80 nm.

4. The method for preparing a back contact solar cell according to claim 1, It is characterized in that The following steps are involved: (1) Selecting a P-type crystalline silicon substrate and performing a texturing treatment on the P-type crystalline silicon substrate; (2) performing doping treatment on the back surface and the front surface of the P-type crystalline silicon substrate after the treatment in step (1); wherein the doping treatment method of the back surface of the P-type crystalline silicon substrate is: growing a tunneling oxide layer on the back surface of the P-type crystalline silicon substrate, growing an intrinsic polycrystalline silicon layer or an intrinsic amorphous silicon layer on the tunneling oxide layer, and then injecting phosphorus ions into the intrinsic polycrystalline silicon layer or the intrinsic amorphous silicon layer; the doping treatment method of the front surface of the P-type crystalline silicon substrate is: injecting boron ions by boron diffusion or ion implantation; (3) subjecting the P-type crystalline silicon substrate treated in step (2) to a high temperature annealing treatment, wherein the peak annealing temperature is 800 to 1100° C. and the annealing time is 30 to 200 min. After the annealing is completed, a doped p+ region is formed on the front surface of the P-type crystalline silicon substrate, and an n+ doped emitter is formed on the back surface of the P-type crystalline silicon substrate; (4) forming a front surface passivation anti-reflection film on the front surface of the P-type crystalline silicon substrate after the treatment in step (3), and forming a back surface passivation film on the back surface of the P-type crystalline silicon substrate; (5) After the treatment in step (4), the back surface of the P-type crystalline silicon substrate is laser grooved, and an aluminum electrode is printed in the laser grooved area to form an ohmic contact with the p+ area, and a silver electrode is printed in the n+ doped area of ​​the back surface to form an ohmic contact with the n+ doped area, thereby completing the production of a back contact solar cell.

5. A method for preparing a back contact solar cell according to claim 4, Features: In step (1), the front surface and the back surface of the P-type crystalline silicon substrate are textured; the resistivity of the P-type crystalline silicon substrate is 0.5 to 15 Ω·cm, and the thickness is 50 to 300 μm.

6. A method for preparing a back contact solar cell according to claim 4 or 5, Features: In step (2), the back surface tunneling oxide layer is SiO 2 , with a thickness of 1-3nm, SiO 2 The growth method is a high temperature thermal oxidation method, a nitric acid oxidation method, an ozone oxidation method or a CVD deposition method; the method for growing an intrinsic polycrystalline silicon layer or an intrinsic amorphous silicon layer on the back surface tunneling oxide layer is as follows: placing a P-type crystalline silicon substrate into an LPCVD device, growing an intrinsic polycrystalline silicon layer or an intrinsic amorphous silicon layer on the back surface tunneling oxide layer; and implanting phosphorus atoms into the intrinsic polycrystalline silicon layer or the intrinsic amorphous silicon layer by ion implantation, wherein the implantation dose is 1×10 15 cm -2 ~8×10 15 cm -2 The doping treatment method of the front surface of the P-type crystalline silicon substrate is as follows: ion implantation is performed on the front surface, and the implanted elements include phosphorus, and the phosphorus ion implantation dose is 1×10 15 cm -2 ~4×10 15 cm -2 .

7. The method for preparing a back contact solar cell according to claim 4, Features: In step (3), the peak temperature of the annealing treatment is 800-1100°C, the annealing time is 30-200 min, and the ambient gas source is N 2 and O 2 .

8. A method for preparing a back contact solar cell according to claim 4, 5 or 7, Features: In step (4), the preparation method of the front surface passivation anti-reflection film is: firstly deposit a layer of SiO with a thickness of 5 to 30 nm on the front surface of the P-type crystalline silicon substrate by using a PECVD device; x The dielectric film is then x A layer of SiN with a thickness of 40 to 80 nm is deposited on the dielectric film. x The back surface passivation film is prepared by first depositing a layer of Al with a thickness of 2 to 20 nm on the back surface of the P-type crystalline silicon substrate using an ALD device. 2 O 3 Dielectric film, then Al 2 O 3 A layer of SiN with a thickness of 40 to 80 nm is deposited on the dielectric film. x Dielectric film.

9. A method for preparing a back-contact solar cell according to any one of claims 4 to 5 and 7, Features: In step (5), the metal electrode is prepared by printing silver paste on the n+ doped area on the back surface of the P-type crystalline silicon substrate treated in step (4) by screen printing, printing aluminum paste on the laser grooved area, and then sintering.

Citation Information

Patent Citations

  • Back contact solar cell

    CN207705205U

  • A method of fabricating a heterojunction all-back-contact solar cell

    WO2017111697A1