A cold-drawn tube blank and cold-drawing process for buffering high-strength steel cold-drawing impact
By designing the transition zone and finished product zone in the high-strength steel cold-drawn tube blank to buffer the deformation of the cold-drawn tail and achieve smooth tube removal, the problems of cold-drawn impact and noise of high-strength steel in the traditional cold-drawing process are solved, and the stability of the process is improved. and versatility.
Patent Information
- Application Number
- CN201811074511.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-09-14
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2038-09-14
AI Technical Summary
The traditional cold drawing process causes large deformation during the cold drawing process of high-strength steel, requires a large drawing force, causes a large cold drawing impact force, and cannot effectively solve the noise problem during cold drawing and pipe removal, affecting the cold drawing machine and spare parts.
Design a cold-drawn tube blank that buffers the cold-drawing impact of high-strength steel. It includes a cylindrical main body. The end of the main body is equipped with a transition zone and a finished product zone. A tapered transition surface is formed by turning, and the inner mold is formed along the drawing direction. The plastic deformation is completed under the action of the external mold, buffering the deformation of the tail and achieving smooth de-tubing.
By preprocessing the transition zone and finished product area of the cold-drawn tube blank, the drawing force at the end of the cold drawing is reduced, the noise and impact force during tube removal are reduced, and smooth tube removal at the end of cold drawing is achieved, which enhances the versatility and stability of the process. sex.
Smart Images

Figure CN109048230B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel pipe production, in particular to a cold-drawn pipe blank and a cold-drawing process for buffering the cold-drawing impact of high-strength steel. Background Art
[0002] The traditional production method of cold-drawn tubes in the industry is to directly draw the cold-drawn blanks, and the wall reduction is consistent throughout the drawing process. However, for high-strength steel, a large drawing force is required to produce deformation, and the deformation is greater towards the end of the cold-drawn tube, resulting in a greater cold-drawing impact force. This cold-drawing process cannot solve the noise problem during cold-drawing tube removal, nor can it avoid the impact on the cold-drawing machine and its spare parts during tube removal. Summary of the invention
[0003] In order to solve the above technical problems, the present invention discloses a cold-drawn tube blank and a cold-drawing process for buffering the impact of cold drawing of high-strength steel. The new cold-drawn tube can solve the noise problem when the high-strength steel is cold-drawn and removed from the tube, and avoid the large drawing force when removing the tube from causing excessive impact on the cold drawing machine and its spare parts.
[0004] The present invention is achieved through the following technical scheme: a cold-drawn tube blank for buffering the cold-drawing impact of high-strength steel comprises a cylindrical main tube, the end of which is provided with a transition zone and a finished product zone from the inside to the outside; the inner diameter and the outer diameter of the finished product zone are the same as the cold-drawing forming size; the transition zone uniformly transitionally connects the main tube and the finished product zone.
[0005] Further, one end of the main pipe body is provided with a transition zone and a finished product zone, or both ends of the main pipe body are provided with a transition zone and a finished product zone.
[0006] The finished product area is cylindrical, the inner diameter of the finished product area is larger than the inner diameter of the main body, and the outer diameter of the finished product area is smaller than the outer diameter of the main body; the inner and outer surfaces of the transition area are conical surfaces that evenly transitionally connect the main body and the finished product area.
[0007] A cold drawing process for buffering the cold drawing impact of high-strength steel comprises the following steps:
[0008] ① Process the blank into the following shape of cold drawn tube blank;
[0009] The cold-drawn tube blank comprises a cylindrical main tube body, and a transition zone and a finished product zone are sequentially arranged at the end of the main tube body from the inside to the outside; the inner diameter and the outer diameter of the finished product zone are the same as the cold-drawn forming size; the transition zone uniformly transitionally connects the main tube body and the finished product zone;
[0010] ② Along the drawing direction, the cold drawn tube blank is plastically deformed under the constraints of the inner and outer dies to reach the predetermined size.
[0011] Further, one end of the main pipe body is provided with a transition zone and a finished product zone, or both ends of the main pipe body are provided with a transition zone and a finished product zone.
[0012] The finished product area is cylindrical, the inner diameter of the finished product area is larger than the inner diameter of the main body, and the outer diameter of the finished product area is smaller than the outer diameter of the main body; the inner and outer surfaces of the transition area are conical surfaces that evenly transitionally connect the main body and the finished product area.
[0013] When processing the blank into a cold drawn tube:
[0014] The first step is to complete the processing of the outer circumference of the finished product area by turning;
[0015] The second step is to complete the processing of the inner circumference of the finished product area by turning;
[0016] The third step is to complete the processing of the outer conical surface of the transition zone by turning;
[0017] The fourth step is to complete the processing of the tapered surface in the transition zone by turning.
[0018] The cold-drawn tube blank of the present invention is provided with a cold-drawn transition zone. When the high-strength steel cold drawing is about to end, the deformation is pre-transitioned to the cold-drawn finished product specification, and the large drawing force at the end of the cold drawing is buffered, thereby reducing the cold-drawing impact caused by excessive drawing force, and reducing the impact on the cold-drawing machine and its spare parts when the tube is removed. The cold-drawn tube blank is also provided with a finished product zone. When the tube is removed, there is no deformation in the cold-drawn finished product zone, and the drawing force is further stabilized, so that the tube is smoothly removed at the end of the cold drawing, and the noise of the tube removal is reduced.
[0019] Compared with the prior art, the beneficial effects of the present invention are: the processing method of the present invention is simple and easy, does not affect the length of the cold-drawn finished product, and only pre-processes the cold-drawn transition zone and the cold-drawn finished product zone at the tail of the billet tube to achieve smooth cold-drawing tube removal without large noise and impact force, and has strong versatility. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is a schematic structural diagram of Embodiment 1 of the present invention;
[0021] Figure 2 Schematic diagram of cold drawing of a cold drawn tube blank according to the second embodiment of the present invention;
[0022] In the figure: 1. Main body; 2. Transition zone; 3. Finished product zone; 4. Inner mold; 5. Outer mold. DETAILED DESCRIPTION
[0023] The following are specific embodiments of the present invention, which will be further described in conjunction with the accompanying drawings.
[0024] Embodiment 1
[0025] Combination Figure 1As shown, a cold-drawn tube blank for buffering the cold-drawing impact of high-strength steel comprises a cylindrical main body 1, a transition zone 2 and a finished product zone 3 are provided at one end of the main body 1, or a transition zone 2 and a finished product zone 3 are provided at both ends of the main body 1. The inner diameter and outer diameter of the finished product zone 3 are the same as the cold-drawing forming size; the transition zone 2 evenly transitions and connects the main body 1 and the finished product zone 3.
[0026] In this embodiment, the finished product area 3 is cylindrical, the inner diameter of the finished product area 3 is larger than the inner diameter of the main body 1, and the outer diameter of the finished product area 3 is smaller than the outer diameter of the main body 1; the inner and outer surfaces of the transition area 2 are conical surfaces that evenly transitionally connect the main body 1 and the finished product area 3.
[0027] Embodiment 2
[0028] Combination Figure 2 As shown, a cold drawing process for buffering the cold drawing impact of high-strength steel comprises the following steps:
[0029] ① Processing the cylindrical blank into the cold drawn tube blank as described in Example 1;
[0030] When processing the blank into a cold drawn tube:
[0031] The first step is to complete the processing of the outer circumference of the finished product area 3 by turning;
[0032] The second step is to complete the processing of the inner circumference of the finished product area 3 by turning;
[0033] The third step is to complete the processing of the outer conical surface of the transition zone 2 by turning;
[0034] The fourth step is to complete the processing of the tapered surface in the transition zone 2 by turning.
[0035] ② Along the drawing direction, the cold drawn tube blank is plastically deformed under the constraints of the inner and outer dies to reach the predetermined size.
[0036] The blank size in this embodiment is Φ351×19×L=12000mm, and is cold drawn to Φ350×16. Under the drawing force of the hydraulic cylinder, the main body 1 completes plastic deformation along the drawing direction through the restraint of the inner die 4 and the outer die 5, thereby achieving the specified size requirements.
[0037] Transition zone: In this example, the length of the transition zone is 100mm. The inner and outer diameters of the blank are pre-processed by wall reduction. During the equal diameter drawing process, the deformation gradually decreases. Under the action of the cold drawing transition zone at the end of the tube, due to the transition of the inner and outer diameters of the steel tube to the finished product specifications, the large drawing force required for cold drawing of high-strength steel to the end of the tube is buffered, thereby reducing the cold drawing impact caused by excessive drawing force and slowing down the impact on the cold drawing machine and its spare parts when the tube is removed.
[0038] Finished product area: In this example, the length of the pre-processed finished product area is 20mm. The inner and outer diameters of the blank in this area are consistent with the specifications of the cold-drawn finished product. Therefore, there is no deformation when cold-drawing to this area. In the cold-drawn finished product area at the end of the tube, there is no deformation in the cold-drawn finished product area when the tube is removed, and the drawing force is further stabilized. Without affecting the length of the cold-drawn finished product, the tube is smoothly removed at the end of cold drawing, reducing the noise of tube removal.
[0039] In this embodiment, the length of the transition zone and the length of the finished product zone are relatively short, which is much smaller than that of the cold-drawn blank and hardly affects the length of the cold-drawn finished product. Through this process method, the tube can be smoothly removed at the end of cold drawing without affecting the length of the cold-drawn tube, eliminating the tube removal noise, and playing a buffering role for the impact generated during the cold drawing process of high-strength steel.
Claims
1. A cold-drawn tube blank for buffering the impact of cold drawing of high-strength steel, comprising a cylindrical main tube body (1), characterized in that: The end of the main pipe (1) is provided with a transition zone (2) and a finished product zone (3) in sequence from the inside to the outside; the inner diameter and outer diameter of the finished product zone (3) are the same as the cold-drawn forming dimensions; the transition zone (2) uniformly transitionally connects the main pipe (1) and the finished product zone (3); Both ends of the main pipe body (1) are provided with a transition area (2) and a finished product area (3).
2. The cold-drawn tube blank for buffering the cold-drawing impact of high-strength steel according to claim 1, characterized in that: The finished product area (3) is cylindrical, the inner diameter of the finished product area (3) is larger than the inner diameter of the main body (1), and the outer diameter of the finished product area (3) is smaller than the outer diameter of the main body (1); the inner and outer surfaces of the transition area (2) are conical surfaces that evenly transitionally connect the main body (1) and the finished product area (3).
3. A cold drawing process for buffering the cold drawing impact of high-strength steel, comprising the following steps: ① Process the blank into the following shape of cold drawn tube blank; The cold-drawn tube blank comprises a cylindrical main tube body (1), the end of the main tube body (1) being provided with a transition zone (2) and a finished product zone (3) in sequence from the inside to the outside; the inner diameter and outer diameter of the finished product zone (3) are the same as the cold-drawn forming dimensions; the transition zone (2) uniformly transitionally connects the main tube body (1) and the finished product zone (3); ② Along the drawing direction, the cold drawn tube blank is plastically deformed under the constraints of the inner and outer dies to reach the predetermined size; Both ends of the main pipe body (1) are provided with a transition area (2) and a finished product area (3).
4. The cold drawing process for buffering the cold drawing impact of high-strength steel according to claim 3, characterized in that: The finished product area (3) is cylindrical, the inner diameter of the finished product area (3) is larger than the inner diameter of the main body (1), and the outer diameter of the finished product area (3) is smaller than the outer diameter of the main body (1); the inner and outer surfaces of the transition area (2) are conical surfaces that evenly transitionally connect the main body (1) and the finished product area (3).
5. The cold drawing process for buffering the cold drawing impact of high-strength steel according to claim 4, characterized in that: When processing the blank into a cold drawn tube: The first step is to complete the processing of the outer circumference of the finished product area (3) by turning; The second step is to complete the processing of the inner circumference of the finished product area (3) by turning; The third step is to complete the processing of the outer conical surface of the transition zone (2) by turning; The fourth step is to complete the machining of the inner conical surface of the transition zone (2) by turning.