A waterproof lens preparation process and waterproof lens

Through the process of plating an anti-reflection film layer and a waterproof film layer on the lens base, combined with a high-energy ion source assisted process and a steam-retardant method, the problem of a small hydrophobic angle of the waterproof lens is solved, and a hydrophobic angle of greater than 100° and good Excellent waterproof performance to meet the high performance requirements of automotive visual systems.

CN110058331BActive Publication Date: 2024-10-15XINYANG SUNNY OPTICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910410795.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-05-17
Publication Date
2024-10-15
Estimated Expiration
2039-05-17

AI Technical Summary

Technical Problem

Waterproof lenses have a small hydrophobic angle and poor waterproof effect, making it difficult to meet the requirements of automotive visual systems for improving imaging clarity and quality.

Method used

The process of plating an anti-reflection film layer and a waterproof film layer on the lens base is adopted, including plating an auxiliary bonding layer on the anti-reflection film layer, and plating the waterproof film layer through a high-energy ion source assisted process and a steam-retardant method to ensure that the anti-reflection film layer is The water angle is greater than 100°, and the spectroscopic test, boiled film test, friction resistance test and salt spray resistance test are carried out.

Benefits of technology

The prepared waterproof lens has a hydrophobic angle greater than 100°, is durable in the natural environment, has good waterproof performance, wear resistance and corrosion resistance, and meets the needs of high-standard and high-performance automotive visual systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110058331B_ABST
    Figure CN110058331B_ABST
Patent Text Reader

Abstract

The present invention relates to a waterproof lens preparation process and a waterproof lens made by the process, wherein the waterproof lens preparation process comprises: S1, coating an anti-reflection film layer (2) on a lens substrate (1); S2, cleaning the lens substrate (1) after coating the anti-reflection film layer (2); S3, after cleaning, coating a waterproof film layer (3) on the anti-reflection film layer (2), and the lens made by the waterproof lens preparation process has a hydrophobic angle greater than 100°. The waterproof lens made by the waterproof lens preparation process of the present invention can ensure that the hydrophobic angle of the waterproof lens is above 118°, and the hydrophobic angle is still above 100° after being exposed to the natural environment for 12 months, and has good waterproof performance, and also has wear resistance and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a waterproof optical lens, and in particular to a waterproof lens preparation process and a waterproof lens made by the process. Background Art

[0002] With the development of society, cars have become an indispensable means of transportation for people. With this comes fierce competition in the industry, and the market pays more and more attention to the high specifications and high performance of products.

[0003] As a common visual system for cars, the requirements for reversing and detecting objects are getting higher and higher. How to provide image clarity, reduce imaging errors, and improve image quality have become the main research directions. As a major component of the visual system, how to increase the water-repellent angle of waterproof lenses and maintain a long-term durability has also become an urgent problem to be solved. Summary of the invention

[0004] The purpose of the present invention is to provide a waterproof lens preparation process and a waterproof lens, so as to solve the problem that the waterproof lens has a small water repellent angle and poor waterproof effect.

[0005] To achieve the above object, the present invention provides a process for preparing a waterproof lens, comprising:

[0006] S1, coating an anti-reflection film layer on a lens substrate;

[0007] S2, cleaning the lens substrate after being coated with the anti-reflection film layer;

[0008] S3, after cleaning, coating a waterproof film layer on the anti-reflection film layer;

[0009] The water repellency angle of the lens manufactured by the waterproof lens manufacturing process is greater than 100°.

[0010] According to one aspect of the present invention, in step S3, the waterproof film layer is plated by evaporation resistance, the coating vacuum degree is 1.0E-3Pa~1.5E-3Pa, and the thickness of the plated waterproof film layer is 45nm-50nm.

[0011] According to one aspect of the present invention, after step S2 and before step S3, the method further includes: coating an auxiliary bonding layer on the anti-reflection film layer, wherein the auxiliary bonding layer is made of silicon oxide and has a thickness of 2nm-5nm.

[0012] According to one aspect of the present invention, in step S1, the antireflection film layer is plated according to the structure of (X+Y)*n, wherein X represents a titanium compound material layer, Y represents a silicon oxide material layer, (X+Y)*n represents that the X material layer and the Y material layer are alternately plated n times, and n is an integer greater than or equal to 3.

[0013] According to one aspect of the present invention, in step S1, a high-energy ion source assisted process is adopted when coating the anti-reflection film layer, including ion cleaning of the lens substrate before coating the anti-reflection film layer, and assisting the coating of a titanium-containing compound material layer and an assisting the coating of a silicon oxide material layer during the coating of the anti-reflection film layer.

[0014] According to one aspect of the present invention, in the high-energy ion source assisted process, the ion source power of ion cleaning is set to a voltage of 500-800V and a current of 500-800A.

[0015] According to one aspect of the present invention, the ion source power for auxiliary plating of the titanium compound material layer is set to a voltage of 1100-1200V and a current of 1100-1200A.

[0016] According to one aspect of the present invention, the ion source power for auxiliary plating of the silicon-containing oxide material layer is set to a voltage of 1000-1200V and a current of 1000-1200A.

[0017] According to one aspect of the present invention, along a direction away from the lens substrate, the antireflection film layer includes a first titanium oxide layer, a first silicon oxide layer, a second titanium oxide layer, a second silicon oxide layer, a third titanium oxide layer and a third silicon oxide layer in sequence;

[0018] The thickness of the first titanium oxide layer is 10-30nm, the thickness of the first silicon oxide layer is 10-40nm, the thickness of the second titanium oxide layer is 30-70nm, the thickness of the second silicon oxide layer is 10-30nm, the thickness of the third titanium oxide layer is 20-50nm, and the thickness of the third silicon oxide layer is 80-110nm.

[0019] According to one aspect of the present invention, the maximum value of the surface reflectivity of the antireflection film layer in the wavelength range of 410nm-690nm is less than 0.5%.

[0020] According to one aspect of the present invention, before step S1, the lens substrate is further ultrasonically cleaned.

[0021] According to one aspect of the present invention, the waterproof lens preparation process further comprises: performing a spectroscopic test and a hydrophobic angle test on the lens after completing step S3.

[0022] According to one aspect of the present invention, the waterproof lens preparation process further comprises: after completing step S3, performing a water boiling film pulling test, a friction resistance test and a salt spray resistance test on the lens.

[0023] The present invention also provides a waterproof lens made by the above-mentioned waterproof lens preparation process, comprising a lens substrate and an anti-reflection film layer and a waterproof film layer sequentially plated on the lens substrate;

[0024] The water repellency angle of the waterproof lens is greater than 100°.

[0025] According to one aspect of the present invention, an auxiliary bonding layer is further provided between the anti-reflection film layer and the waterproof film layer of the waterproof lens.

[0026] According to one scheme of the present invention, a waterproof lens is prepared according to a process flow of coating an anti-reflection film layer on a lens substrate, then cleaning it, and then coating a waterproof film layer on the anti-reflection film layer after cleaning. It can be ensured that the water repellency angle of the manufactured waterproof lens is above 118°, and the water repellency angle is still above 100° after being exposed to the natural environment for 12 months. It has good waterproof performance, and also has wear resistance and corrosion resistance.

[0027] According to one solution of the present invention, a waterproof film layer is plated by evaporation resistance, the vacuum degree of the film is 1.0E-3Pa to 1.5E-3Pa, and the thickness of the plated waterproof film layer is 45nm to 50nm. This ensures that the plated waterproof film layer is more solid and not easy to fall off, and at the same time, the hydrophobic angle can be increased, and the waterproof performance is good.

[0028] According to one solution of the present invention, after the anti-reflection film layer is coated on the lens substrate to form a semi-finished product and before the waterproof film layer is coated, since it also includes a cleaning step for the semi-finished lens, it is beneficial to the subsequent coating of the waterproof film layer, ensuring the firmness of the coating of the waterproof film layer, increasing the hydrophobic angle, and improving the waterproof performance.

[0029] According to one solution of the present invention, since an auxiliary bonding layer is first plated on the anti-reflection film layer before the waterproof film layer is plated, the bonding energy between the waterproof film layer and the auxiliary bonding layer can be effectively improved, thereby ensuring the structural strength and protective performance of the waterproof film layer.

[0030] According to one solution of the present invention, in step S1, an anti-reflection film layer is plated according to the structure of (X+Y)*n, where n is an integer greater than or equal to 3. This is conducive to ensuring the firmness of the anti-reflection film layer and the lens substrate, and ensuring that the anti-reflection film layer can effectively reduce the surface light reflectivity. At the same time, a waterproof film layer is plated on the basis of the anti-reflection film layer structure, which is conducive to ensuring the waterproof performance of the waterproof film layer.

[0031] According to one solution of the present invention, when the anti-reflection film is plated according to the above structure, a high-energy ion source assisted process is adopted, including ion cleaning of the lens substrate before the anti-reflection film is plated, and assisting the plating of the titanium compound material layer and the silicon oxide material layer during the anti-reflection film plating process. In this way, the cleanliness of the lens substrate surface can be improved, and the bonding between the film layer and the lens substrate can be improved. At the same time, the density of the film layer can be improved, and the bonding strength between the film layers can be improved.

[0032] According to one solution of the present invention, the thickness of the plated first titanium oxide layer is set to 10-30nm, the thickness of the first silicon oxide layer is set to 10-40nm, the thickness of the second titanium oxide layer is set to 30-70nm, the thickness of the second silicon oxide layer is set to 10-30nm, the thickness of the third titanium oxide layer is set to 20-50nm, and the thickness of the third silicon oxide layer is set to 80-110nm. This is beneficial to control the surface reflectivity of the anti-reflection film layer of the present invention, so that the maximum value of the surface reflectivity of the anti-reflection film layer in the 410nm-690nm band is less than 0.5%.

[0033] According to one solution of the present invention, before step S1, ultrasonic cleaning is performed on the lens substrate to ensure the cleanliness of the lens substrate.

[0034] According to one solution of the present invention, after step S3, the waterproof lens is further subjected to a spectroscopic test, a hydrophobic angle test, a water boiling film test, a friction resistance test, and a salt spray resistance test. In this way, a performance test can be performed after the waterproof lens is subjected to the performance test to ensure that the various performances of the waterproof lens meet the requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 A schematic diagram showing the structure of a waterproof lens manufactured by using an embodiment of the process for manufacturing a waterproof lens of the present invention;

[0036] Figure 2 A diagram schematically showing a hydrophobic angle test of a waterproof lens according to an embodiment of the present invention;

[0037] Figure 3 A diagram schematically showing a spectroscopic test curve of a waterproof lens according to an embodiment of the present invention;

[0038] Figure 4 A diagram schematically showing the water repellency angle of a conventional lens after a friction resistance test;

[0039] Figure 5 A diagram schematically showing the hydrophobic angle of the waterproof lens of the present invention after the friction resistance test;

[0040] Figure 6 Schematic representation of the surface results of traditional lenses after salt spray test;

[0041] Figure 7 The surface result diagram of the waterproof lens of the present invention after the salt spray resistance test is schematically shown. DETAILED DESCRIPTION

[0042] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0043] When describing the embodiments of the present invention, the orientation or positional relationship expressed by the terms "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" are based on the orientation or positional relationship shown in the relevant drawings. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operate in a specific orientation. Therefore, the above terms should not be understood as limiting the present invention.

[0044] The present invention will be described in detail below in conjunction with the accompanying drawings and specific embodiments. The embodiments cannot be described one by one here, but the embodiments of the present invention are not therefore limited to the following embodiments.

[0045] Figure 1 Schematically shows the structure of a waterproof lens manufactured using one embodiment of the waterproof lens manufacturing process of the present invention. Figure 1 As shown, the waterproof lens of the present invention comprises a lens substrate 1 , an anti-reflection film layer 2 , and a waterproof film layer 3 .

[0046] Combination Figure 1 The waterproof lens preparation process of the present invention is described. The waterproof lens preparation process of the present invention includes S1, coating an anti-reflection film layer 2 on a lens substrate 1; S2, cleaning the lens substrate 1 after coating the anti-reflection film layer 2; S3, after cleaning, coating a waterproof film layer 3 on the anti-reflection film layer 2. The hydrophobic angle of the lens made by the waterproof lens preparation process of the present invention is greater than 100°. That is, the waterproof film preparation process of the present invention first coats an anti-reflection film layer 2 on the lens substrate 1. According to one embodiment of the present invention, the lens substrate 1 can be a transparent glass lens, and the refractive index is generally between 1.49-2.0. According to the concept of the present invention, the anti-reflection film layer 2 can be coated on any surface of the lens substrate 1, and the anti-reflection film layer 2 can also be coated on both surfaces of the lens substrate 1. Figure 1As shown, in this embodiment, an anti-reflection film layer 2 is plated on both surfaces of the lens substrate 1. The anti-reflection film layer 2 is used to reduce the surface emissivity of the lens and improve the transmittance of light.

[0047] After the anti-reflection film layer 2 is plated, the lens substrate 1 with the anti-reflection film layer 2 needs to be cleaned. At this time, the lens substrate 1 is plated with the anti-reflection film layer 2, which can be regarded as a semi-finished lens, that is, the semi-finished lens needs to be cleaned, and then the waterproof film layer 3 is plated on the anti-reflection film layer 2. According to the concept of the present invention, the waterproof film layer 3 is plated on at least one anti-reflection film layer 2. That is, if the anti-reflection film layer 2 is plated on both surfaces of the lens substrate 1, the waterproof film layer 3 is plated on at least one of the anti-reflection films 2. According to one embodiment of the present invention, Figure 1 As shown, the anti-reflection film layer 2 is plated on both surfaces of the lens substrate 1, and the waterproof film layer 3 is plated only on the upper anti-reflection film layer 2. In the actual plating process, the upper anti-reflection film layer 2 can be plated first, then the lower anti-reflection film layer 2 is plated, and then the waterproof film layer 3 is plated on the upper anti-reflection film layer 2.

[0048] The waterproof lens preparation process of the present invention can ensure that the water repellency angle of the waterproof lens is above 118°, and the water repellency angle is still above 100° after being exposed to the natural environment for 12 months. The waterproof lens has good waterproof performance and also has wear resistance and corrosion resistance.

[0049] In the present invention, in step S3, the waterproof film layer 3 is plated by the evaporation resistance method, the vacuum degree of the coating is 0.0015-0.001pa, and the thickness of the plated waterproof film layer 3 is 45nm-50nm. That is, the waterproof material is melted and vaporized and plated on the anti-reflection film layer 2 by resistance heating in a vacuum environment. The vacuum degree of the waterproof film layer 3 is 1.0E-3Pa~1.5E-3Pa, and the coating thickness is 45nm-50Nm. According to one embodiment of the present invention, the waterproof material can be selected from CEKO-TCD-063 or OR-112D material.

[0050] The waterproof lens preparation process of the present invention adopts the evaporation-resistance method to plate the waterproof film layer 3, the vacuum degree of the coating is 1.0E-3Pa to 1.5E-3Pa, and the thickness of the plated waterproof film layer is 45nm to 50nm. In this way, the plated waterproof film layer can be ensured to be more solid and not easy to fall off, and at the same time, the hydrophobic angle can be increased, and the waterproof performance is good.

[0051] In the present invention, after the anti-reflection film layer 2 is plated on the lens substrate 1 to form a semi-finished product and before the waterproof film layer 3 is plated, since a cleaning step for the semi-finished lens is also included, it is beneficial to the subsequent plating of the waterproof film layer 3, ensuring the firmness of the plating of the waterproof film layer 3, increasing the hydrophobic angle, and improving the waterproof performance.

[0052] In the invention, the anti-reflection film layer 2 and the waterproof film layer 3 are separately plated. As mentioned above, after the anti-reflection film layer 2 is plated, the semi-finished lens needs to be cleaned. And the method of the present invention also includes that after cleaning and before the waterproof film layer 3 is plated, an auxiliary bonding layer 4 needs to be plated on the anti-reflection film layer 2. In the invention, the auxiliary bonding layer 4 is made of silicon oxide material with a thickness of 2nm-5nm.

[0053] In the invention, since an auxiliary bonding layer 4 is firstly plated on the anti-reflection film layer 2 before the waterproof film layer 3 is plated, the bonding energy between the waterproof film layer 3 and the auxiliary bonding layer 4 can be effectively improved to ensure the structural strength and protective performance of the waterproof film layer 3.

[0054] In the present invention, in the step S1, the antireflection film layer 2 is plated according to the structure of (X+Y)*n, wherein X represents a titanium compound material layer, Y represents a silicon oxide material layer, (X+Y)*n represents that the X material layer and the Y material layer are alternately plated n times, and n is an integer greater than or equal to 3.

[0055] In the present invention, the anti-reflection film layer 2 is plated with the above structure, which is conducive to ensuring the firmness of the combination of the anti-reflection film layer 2 and the lens substrate 1, and ensuring that the anti-reflection film layer 2 can effectively reduce the surface light reflectivity. At the same time, based on the structure of the anti-reflection film layer 2, the waterproof film layer 3 is plated, which is conducive to ensuring the waterproof performance of the waterproof film layer 3.

[0056] In the present invention, when the anti-reflection film layer 2 is plated according to the above structure, a high-energy ion source assisted process is adopted, including ion cleaning of the lens substrate 1 before the anti-reflection film layer 2 is plated, and assisting the plating of the titanium compound material layer and the silicon oxide material layer during the plating of the anti-reflection film layer 2. In this way, the cleanliness of the surface of the lens substrate 1 can be improved, and the bonding between the film layer and the lens substrate 1 can be improved. At the same time, the density of the film layer can be improved, and the bonding strength between the film layers can be improved.

[0057] According to one embodiment of the present invention, in the high-energy ion source assisted process, the ion source power of ion cleaning is set to a voltage of 500-800V and a current of 500-800A, the ion source power of the titanium compound material layer assisted plating is set to a voltage of 1100-1200V and a current of 1100-1200A, and the ion source power of the silicon oxide material layer assisted plating is set to a voltage of 1000-1200V and a current of 1000-1200A. Within the above process parameter range, the effect of the high-energy ion source assisted process can be maximized.

[0058] According to one embodiment of the present invention, the structure of the plated antireflection film layer 2 is (X+Y)*n, n=3, X is titanium oxide, and Y is silicon oxide. That is, in this embodiment, along the direction away from the lens substrate 1, the antireflection film layer 2 includes a titanium oxide layer, a first silicon oxide layer, a second titanium oxide layer, a second silicon oxide layer, a third titanium oxide layer, and a third silicon oxide layer in sequence. The thickness of the plated first titanium oxide layer is 10-30nm, the thickness of the first silicon oxide layer is 10-40nm, the thickness of the second titanium oxide layer is 30-70nm, the thickness of the second silicon oxide layer is 10-30nm, the thickness of the third titanium oxide layer is 20-50nm, and the thickness of the third silicon oxide layer is 80-110nm. Of course, according to the concept of the present invention, the material layers of the antireflection film layer 2 can also have other embodiments, for example, X in the (X+Y)*n structure can be titanium dioxide, titanium pentoxide, etc. Y can be silicon monoxide or silicon dioxide, etc. Specifically, a suitable material can be selected according to the waterproof effect to be ultimately achieved.

[0059] In the present invention, coating each film layer of the anti-reflection film layer 2 according to the above film layer thickness range is beneficial to controlling the surface reflectivity of the anti-reflection film layer 2 of the present invention. Figure 3 As shown, in the present invention, the maximum value of the surface reflectivity of the antireflection film layer 2 in the wavelength range of 410nm-690nm is less than 0.5%.

[0060] The process for preparing a waterproof lens of the present invention further comprises, before step S1 , ultrasonically cleaning the lens substrate 1 to ensure the cleanliness of the lens substrate 1 .

[0061] The waterproof lens preparation process of the present invention further includes performing spectroscopic test, hydrophobic angle test, water boiling and film pulling test, friction resistance test and salt spray resistance test on the waterproof lens after the waterproof film layer 3 is plated.

[0062] The steps of the spectrophotometry test are as follows: select the surface of the waterproof lens to be tested, and use a reflectivity tester to measure the surface to be tested, such as Figure 3 As shown, if the maximum value of the surface reflectivity in the 410nm-690nm band is less than 0.5%, the requirement is met.

[0063] The hydrophobic test is as follows: select multiple waterproof lenses to test the surface hydrophobic angle, select the water drop size as 2μL, and measure the size of the hydrophobic angle. Figure 2 As shown, the hydrophobic angle of one of the waterproof lenses is 121.2°, which meets the requirements.

[0064] The boiling film test is as follows: use boiling water steam to boil the waterproof lens for two hours to confirm whether the film layer on the lens surface falls off. If not, it meets the requirements.

[0065] The friction resistance test is as follows: a sponge is added with a 1:10 Kanto mud solution and the wear resistance test is carried out under a load of 2.5N. Figure 4 and Figure 5 As shown, the film layer of the conventional waterproof lens may fall off after being worn for 50 times, while the waterproof lens of the present invention is still greater than 100° after being worn for 300 times and then subjected to a hydrophobic angle test.

[0066] Combination Figure 6 and Figure 7 As shown, the salt spray resistance test is as follows: the existing waterproof lens and the waterproof lens of the present invention are respectively subjected to a salt spray corrosion test in a sodium chloride solution at 35°C and 5% concentration. The existing waterproof lens suffers from film shedding corrosion after 96 hours, while the waterproof lens of the present invention still has no corrosion phenomenon after 288 hours.

[0067] As can be seen from the above, the overall process of the waterproof lens preparation process of the present invention is as follows: first, a lens substrate 1 is selected, and then the lens substrate 1 is ultrasonically cleaned, and then the lens substrate 1 is placed in an anti-reflection film layer 2 coating device, and the lens substrate 1 is subjected to high-energy ion-assisted cleaning in the device, and then the anti-reflection film layer 2 is coated according to the structure of (X+Y)*n, and then the lens substrate 1 after the anti-reflection film layer 2 is coated is taken out (semi-finished lens), and the waterproof film layer 3 is separately coated by a coating machine. Specifically, the auxiliary bonding layer 4 is first coated on the anti-reflection film layer 2, and then the waterproof film layer 3 is coated on the auxiliary bonding layer 4 to complete the preparation of the waterproof lens. After that, the waterproof lens is subjected to a spectroscopic test, a hydrophobic angle test, a water boiling and pulling film test, a friction resistance test, and a salt spray resistance test to check whether the coated waterproof lens meets the requirements. It should be noted that the spectroscopic test and the hydrophobic angle test will not cause damage to the lens, and can be tested sequentially, that is, the spectroscopic test (or hydrophobic angle test) can be performed first and then the hydrophobic angle test (or spectroscopic test) can be performed. The water boiling film test, friction resistance test and salt spray resistance test will damage the lens to a certain extent, so these tests should be conducted after the lens has undergone the hydrophobic angle test and spectrophotometry test. Of course, new lenses can also be selected for water boiling film test, friction resistance test and salt spray resistance test, that is, these tests can be conducted by sampling the prepared waterproof lenses.

[0068] The present invention also provides a waterproof lens made by the above method, referring to the plating process and attached Figure 1 The waterproof lens of the present invention comprises a lens substrate 1, an antireflection film layer 2 and a waterproof film layer 3.

[0069] The waterproof lens of the present invention has an anti-reflection film layer 2 on at least one surface of the lens substrate 1, and a waterproof film layer 3 on at least one anti-reflection film layer 2. The water repellency angle of the waterproof lens of the present invention is greater than 100°.

[0070] Specifically, the structure of the antireflection film layer 2 is (X+Y)*n, wherein X represents a titanium compound material layer, Y represents a silicon oxide material layer, (X+Y)*n represents that the X material layer and the Y material layer are alternately plated n times, and n is an integer greater than or equal to 3. According to one embodiment of the present invention, in a direction away from the lens substrate 1, the antireflection film layer 2 includes a first titanium oxide layer, a first silicon oxide layer, a second titanium oxide layer, a second silicon oxide layer, a third titanium oxide layer and a third silicon oxide layer in sequence. And the thickness of the first titanium oxide layer is 10-30nm, the thickness of the first silicon oxide layer is 10-40nm, the thickness of the second titanium oxide layer is 30-70nm, the thickness of the second silicon oxide layer is 10-30nm, the thickness of the third titanium oxide layer is 20-50nm, and the thickness of the third silicon oxide layer is 80-110nm. The maximum value of the surface reflectivity of the antireflection film layer 2 in the 410nm-490nm band is less than 0.5%.

[0071] In the waterproof lens of the present invention, the waterproof film layer 3 has a thickness of 45nm-50nm. An auxiliary bonding layer 4 is provided between the anti-reflection film layer 2 and the waterproof film layer 3. The auxiliary bonding layer 4 is made of silicon oxide material and has a thickness of 2nm-5nm.

[0072] The above contents are merely examples of specific solutions of the present invention. For devices and structures not described in detail therein, it should be understood that they can be implemented by adopting general devices and general methods available in the art.

[0073] The above is only one solution of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A process for preparing a waterproof lens, characterized in that: include: S1, coating an anti-reflection film layer (2) on a lens substrate (1); S2, cleaning the lens substrate (1) after coating the anti-reflection film layer (2); S3, after cleaning, coating a waterproof film layer (3) on the anti-reflection film layer (2); The water repellency angle of the lens manufactured by the waterproof lens manufacturing process is greater than 100°; Along a direction away from the lens substrate (1), the antireflection film layer (2) comprises in sequence a first titanium oxide layer, a first silicon oxide layer, a second titanium oxide layer, a second silicon oxide layer, a third titanium oxide layer and a third silicon oxide layer; The thickness of the first titanium oxide layer is 10-30 nm, the thickness of the first silicon oxide layer is 10-40 nm, the thickness of the second titanium oxide layer is 30-70 nm, the thickness of the second silicon oxide layer is 10-30 nm, the thickness of the third titanium oxide layer is 20-50 nm, and the thickness of the third silicon oxide layer is 80-110 nm; In the step S3, the waterproof film layer (3) is plated by a vapor resistance method, the vacuum degree of the coating is 1.0E-3Pa~1.5E-3Pa, and the thickness of the plated waterproof film layer (3) is 45nm-50nm; After step S2 and before step S3, the method further comprises: plating an auxiliary bonding layer (4) on the third silicon oxide layer, wherein the auxiliary bonding layer (4) is made of silicon oxide and has a thickness of 2 nm to 5 nm.

2. The process for preparing a waterproof lens according to claim 1, characterized in that: In the step S1, a high-energy ion source assisted process is adopted when coating the anti-reflection film layer (2), including ion cleaning of the lens substrate (1) before coating the anti-reflection film layer (2), and assisting the coating of a titanium compound material layer and assisting the coating of a silicon oxide material layer during the coating process of the anti-reflection film layer (2).

3. The process for preparing a waterproof lens according to claim 2, characterized in that: In the high-energy ion source assisted process, the ion source power of ion cleaning is set to a voltage of 500-800V and a current of 500-800A.

4. The process for preparing a waterproof lens according to claim 2, characterized in that: The power of the ion source for auxiliary plating of the titanium compound material layer is set to a voltage of 1100-1200V and a current of 1100-1200A.

5. The process for preparing a waterproof lens according to claim 2, characterized in that: The power of the ion source for auxiliary plating of the silicon-containing oxide material layer is set to a voltage of 1000-1200V and a current of 1000-1200A.

6. The process for preparing a waterproof lens according to any one of claims 1 to 5, characterized in that: The maximum value of the surface reflectivity of the antireflection film layer (2) in the wavelength range of 410nm-690nm is less than 0.5%.

7. The process for preparing a waterproof lens according to claim 1, characterized in that: Before step S1, the lens substrate (1) is also ultrasonically cleaned.

8. The process for preparing a waterproof lens according to claim 1, characterized in that: The waterproof lens preparation process further includes: after completing step S3, performing a spectroscopic test and a hydrophobic angle test on the lens.

9. The process for preparing a waterproof lens according to claim 8, characterized in that: The waterproof lens preparation process further includes: after completing step S3, performing a water boiling film pulling test, a friction resistance test and a salt spray resistance test on the lens.

10. A waterproof lens made by using the waterproof lens preparation process according to any one of claims 1 to 9.