Long hole heat exchange channel at the interface of explosive composite plate and its manufacturing method
By prefabricating micropores on the substrate and reaming the holes after explosion and composite, the holes are formed in long hole heat exchange channels are solved, the problem of opening holes at the interface is improved, the heat exchange efficiency and structural strength are improved, and it is suitable for high-temperature and high-pressure places.
Patent Information
- Application Number
- CN201910440559.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-05-24
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2039-05-24
AI Technical Summary
It is difficult to effectively open long hole heat exchange channels at the interface of the explosive composite panel. The traditional method is complex and difficult to achieve, affecting the heat exchange efficiency and structural strength.
Micro elongated holes are prefabricated on one side of the substrate, and then exploded and then reamed through wire cutting to form a long hole heat exchange channel across the interface of the composite plate, using circular or elliptical micro-holes to disperse and protect the hole structure with stress.
It realizes high-efficiency heat exchange, high structural strength and easy operation of long hole heat exchange channels, suitable for high-temperature and high-pressure environments.
Smart Images

Figure CN110238505B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of explosion composite and heat exchangers, and in particular to a long hole heat exchange channel at the interface of an explosion composite plate and a manufacturing method thereof. Background Art
[0002] Heat exchanger is a device that realizes heat transfer between two or more fluids at different temperatures. It is one of the main equipment that transfers heat from a higher temperature fluid to a lower temperature fluid, so that the fluid temperature reaches the specified index of the process to meet the needs of process conditions and improve energy utilization. The heat exchanger industry involves nearly 30 industries such as HVAC, pressure vessels, and reclaimed water treatment equipment, forming an industrial chain.
[0003] Heat exchangers are usually manufactured using traditional fusion welding, expansion welding and other methods. Automatic argon arc welding, manual argon arc welding, manual arc welding and other methods should be used as welding processes. In the 1970s, my country began to try to use the explosive composite method to make heat exchangers. In tube-tube sheets, more and more traditional fusion welding methods are abandoned and explosive welding methods are used. This is because the explosive welding method does not require highly skilled tube welding skills, and the performance of the plate materials is similar or very different, and welding can be achieved. It does not require a special atmosphere, and the size requirements are not as strict as the fusion welding method. At present, the heat transfer channel is often simply in the same metal. With the increasing requirements for heat exchangers, the heat exchanger is required to have both efficient heat exchange and high strength. If a hole can be made at the interface of the composite plate to make a heat exchange channel, it is bound to achieve better results. For example, some devices in nuclear fusion devices use grooves at the copper-steel composite interface.
[0004] If the explosive composite plate is punched and slotted at the side interface, it can be achieved if the distance is short, but it is difficult to achieve if the distance is long. If a slot is made on one side of the explosive composite plate, it is opened to the interface, and then the slot is sealed to form a heat exchange channel at the interface, it can be achieved, but the process is more complicated. Therefore, it is very important to find a method to open a long hole at the explosive composite interface. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a long hole heat exchange channel at the interface of an explosive composite plate and a manufacturing method thereof. Before the explosive composite, a micro long hole is prefabricated on one side of the substrate, and then the explosive composite is performed. After the explosive composite, the microhole is enlarged to form a long hole heat exchange channel at the interface of the composite plate. The obtained heat exchange channel has good heat exchange effect, high structural strength and is more convenient to operate.
[0006] In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a long hole heat exchange channel at the interface of an explosive composite plate, comprising a base plate and a cover plate, the lower surface of the cover plate and the upper surface of the base plate are explosively composited, and a long hole heat exchange channel spanning the base plate and the cover plate is opened at the junction of the base plate and the cover plate. By setting the long hole heat exchange channel, and the heat exchange channel spanning the composite part of the base plate and the cover plate, the heat exchange channel has a good heat exchange effect and a high structural strength.
[0007] Furthermore, the long hole heat exchange channel is located near the interface of the explosive composite plate, and the extension direction of the long hole heat exchange channel is perpendicular to the side of the substrate. The long hole heat exchange channel is located near the interface of the explosive composite plate, which is conducive to the formation of the channel during explosive composite.
[0008] Furthermore, the length of the long hole heat exchange channel is not greater than 800 mm, there are multiple long hole heat exchange channels, and the multiple long hole heat exchange channels are evenly and parallelly arranged along the side of the substrate where the long hole heat exchange channel is located.
[0009] The long hole heat exchange channel of the present application can be up to 800 mm in length, which is conducive to heat exchange and improves the efficiency of heat exchange.
[0010] The present invention further discloses a method for preparing the long hole heat exchange channel at the interface of the explosive composite plate, comprising the following steps: 1. Pretreatment of the substrate: 1) preparing the substrate and the cover plate to a certain size, cutting a 2-3 mm slit on one side of the substrate in a direction parallel to the substrate by wire cutting, and then cutting a micro hole at the end;
[0011] 2) Use surfacing welding to seal one side of the cut, grind it flat, then fill the micropores with water, and seal both ends of the micropores with high-temperature resistant sealant; set the cut to facilitate the opening of micropores. If no cut is set, there is no way to open the micropores, and then weld the cut flat so as not to affect its explosive compounding.
[0012] 2. Explosive compounding: 3) Clean the side of the substrate with the cutouts and clean one side of the cover plate;
[0013] 4) placing the substrate and the cover plate in an explosion field for explosive bonding, the two surfaces cleaned in step 3) being the explosive bonding surfaces;
[0014] 3. Micropore expansion: 5) After the explosive composite, the composite plate is leveled and heat treated to make the explosive composite plate flat;
[0015] 6) Remove the blockages at both ends of the micropores and release water to make the micropores unobstructed;
[0016] 7) The composite plate processed in step 6) is placed on a wire cutting workbench, and the micropores are expanded to the interface of the composite plate by wire cutting to obtain a heat exchange channel.
[0017] The wire cutting method is specifically as follows: a molybdenum wire is inserted into a microhole to expand the hole, so that the hole is expanded to cross the composite plate bonding interface, that is, a heat exchange channel is formed at the composite interface.
[0018] Furthermore, in step 1), the micropores are circular micropores with a diameter of 3 to 8 mm and a length of no more than 800 mm. The micropores can be circular, and circular holes can disperse stress, withstand greater pressure, and avoid high temperature and high pressure from damaging the micropores during the explosion of explosives, thereby protecting the micropores. If the micropores are too large, the explosion of explosives will cause the holes to collapse, and if they are too small, it will be inconvenient for the molybdenum wire to pass through in the later stage, as well as the expansion of the micropores.
[0019] Furthermore, in step 1), the micropores are elliptical micropores with a long diameter of 3 to 8 mm and a length of no more than 800 mm, and the long diameter of the elliptical micropores is perpendicular to the substrate. The long diameter of the elliptical micropore is perpendicular to the substrate. The long diameter of the elliptical micropore is perpendicular to the substrate, which is conducive to dispersing stress, protecting the micropores from damage, and ensuring the integrity of the pores.
[0020] Furthermore, after the micro-holes are opened, the wire cutting cracks left on the opening surface should be sealed with the same metal surfacing and polished flat. During the explosive compounding, the side with the micro-holes opened should be placed on the inner side of the explosive compounding. The wire cutting cracks left on the opening surface should be sealed with the same metal surfacing and polished flat in preparation for explosive welding.
[0021] The beneficial effects brought by the present invention are as follows: (1) the difficult problem of opening a long hole at the composite interface is solved by combining wire cutting with explosive composite;
[0022] (2) The micropores are circular or elliptical, which is conducive to the diffusion of stress during explosive compounding and protects the micropores from being collapsed or damaged;
[0023] (3) During the explosive compounding, the micropores are filled with water. Since water is an incompressible liquid, the micropores are intact and will not be blocked during the explosive compounding, thus preparing for the wire cutting hole expansion;
[0024] (4) The heat exchange channel produced by this method has high heat exchange efficiency and strong structural strength, and can be used in high temperature and high pressure places. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Schematic diagram of a substrate with micropores.
[0026] Figure 2 Schematic diagram of a substrate with surface cuts eliminated.
[0027] Figure 3 Schematic diagram of the explosive composite device.
[0028] Figure 4 Schematic diagram of the explosive plate after hole expansion.
[0029] Among them, 1-cut; 2-micropore; 3-welding liquid; 4-base plate; 5-composite plate; 6-gap; 7-detonator; 8-explosive; 9-colloidal water; 10-sand base; 11-heat exchange channel; 12-weld. DETAILED DESCRIPTION
[0030] The present invention is described in detail below with reference to specific embodiments.
[0031] The explosive used in the present invention is explosive fiber or strip explosive, and has no special requirements on the type and detonation velocity. No matter single substance, mixed explosive, low detonation velocity or high detonation velocity explosive, it can be used.
[0032] Embodiment 1:
[0033] like Figure 1 As shown, 1) a stainless steel plate is selected as a substrate 4, the size of the substrate 4 is 600mm×300mm×16mm, and a 2mm deep slit 1 is cut into the substrate along the 600mm side length direction by wire cutting, and then a circular microhole 2 with a diameter of 4mm and a length of 600mm is cut toward the inside of the plate;
[0034] 2) If Figure 2 As shown, the slit 1 is sealed by surfacing welding, the gap of the slit 1 is filled with welding liquid 3, the surface slit is eliminated, the surface is polished and smoothed, and then the micropore 2 is filled with water, and both ends are sealed with high temperature resistant sealant, so that the slit of the substrate 4 and both ends of the hole are sealed;
[0035] 3) Clean the side of the substrate 4 with the cut 1 after the above steps, select chromium zirconium copper as the cover plate 5, the size of the cover plate 5 is 600mm×300mm×8mm, clean one side of the cover plate 5, place the substrate 4 and the cover plate 5 in the explosion field for explosion composite, and the cleaned two sides are the explosion composite bonding surface. The specific operation method is as follows: Figure 3 As shown, the base plate 4 and the composite plate 5 are placed on the sand base 10 of the special blasting field, leaving a certain gap 6 in the middle, adding a protective layer on the cover plate 5, covering the protective layer with explosives 8, and placing the detonator 7 into the explosives from one end, and adding colloidal water 9 on the explosives 8. After the preparation is completed, the wires are connected, charged, detonated, and the composite plate is recovered;
[0036] 4) After the explosive composite, the periphery of the composite plate is cut neatly, leveled and heat treated to make the explosive composite plate flat, and the blockages at both ends of the micropores are removed to make the micropores unobstructed;
[0037] 5) If Figure 4 As shown, the composite plate is placed on a wire cutting workbench, and a molybdenum wire is inserted into the microhole for hole expansion, so that the hole is expanded to cross the composite plate bonding interface and the weld 1 of the explosive composite plate, thereby forming a heat exchange channel 11 after the hole expansion at the composite interface.
[0038] Embodiment 2:
[0039] 1) If Figure 1 As shown, a stainless steel plate is selected as the substrate 4, and the size of the substrate 4 is 500mm×200mm×16mm. The substrate 4 is cut into a 3mm deep slit 1 along the length direction of the 500mm side by a wire cutting method, and then an elliptical microhole 2 with a long diameter of 4mm, a short diameter of 3, and a length of 800mm is cut toward the inside of the plate, and the long diameter direction is consistent with the slit direction;
[0040] 2) If Figure 2 As shown, the cut seam 1 is sealed by surfacing welding, the gap is filled with welding liquid 3, the surface cut seam is eliminated, the surface is polished and smoothed, and then the micropores 2 are filled with water, and the two ends are sealed with high temperature resistant sealant, so that the cut seam on the stainless steel plate and the two ends of the hole are sealed;
[0041] 3) Clean the side of the substrate 4 with the slit 1 after the above steps, select an aluminum plate as the cover plate 5, the size of which is 500mm×200mm×6mm, clean one side of the cover plate 5, place the substrate 4 and the cover plate 5 in the explosion field for explosion compounding, and the cleaned two sides are the explosion compounding bonding surfaces. The specific operation of the explosion compounding is as follows: Figure 3 As shown, a base plate 4 and a cover plate 5 are placed on a sand base 10 of a special blasting field, leaving a certain gap 6 in the middle, a protective layer is added on the cover plate 5, and explosives 8 are spread on the protective layer. Detonators 7 are placed into the explosives from one end, and colloidal water 9 is added to the explosives 8. After preparation is completed, the wires are connected, charged, detonated, and the composite plate is recovered.
[0042] 4) After the explosive composite, the periphery of the composite plate is cut neatly, leveled and heat treated to make the explosive composite plate flat, and the blockages at both ends of the micropores are removed to make the micropores unobstructed;
[0043] 5) If Figure 4 As shown, the composite plate is placed on a wire cutting workbench, and a molybdenum wire is inserted into the microhole for hole expansion, so that the hole is expanded to cross the composite plate bonding interface, that is, to cross the weld 12 of the explosive composite plate, thereby forming a heat exchange channel 11 after the hole expansion at the composite interface.
[0044] The above shows and describes the basic principles, main features and characteristics of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of the present invention to be protected is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a long hole heat exchange channel at the interface of an explosive composite plate, characterized in that: The long hole heat exchange channel at the interface of the explosive composite plate comprises a base plate (4) and a cover plate (5), the lower surface of the cover plate (5) and the upper surface of the base plate (4) are explosively composited, and a long hole heat exchange channel (11) spanning the base plate (4) and the cover plate (5) is opened at the junction of the base plate (4) and the cover plate (5); The process includes the following steps:
1. Pretreatment of the substrate: 1) Prepare the substrate and cover plate to a certain size, cut a 2-3 mm slit on one side of the substrate in a direction parallel to the substrate using wire cutting, and then cut a micro hole at the end; 2) Use surfacing welding to seal one side of the cut, grind it flat, then fill the micropores with water, and seal both ends of the micropores with high temperature resistant sealant; 2. Explosive compounding: 3) Clean the side of the substrate with the cutouts and clean one side of the cover plate; 4) placing the substrate and the cover plate in the explosion field for explosion bonding, and the two surfaces cleaned in step 3) are the explosion bonding surfaces; 3. Micropore expansion: 5) After the explosive composite, the composite plate is leveled and heat treated to make the explosive composite plate flat; 6) Remove the blockages at both ends of the micropores and release water to make the micropores unobstructed; 7) Place the composite plate processed in step 6) on a wire cutting workbench, and use wire cutting to expand the micropores to the interface of the composite plate to obtain a heat exchange channel.
2. The method for preparing the long hole heat exchange channel at the interface of the explosive composite plate according to claim 1, characterized in that: The long hole heat exchange channel (11) is located at the proximal end of the interface of the explosion composite plate, and the extension direction of the long hole heat exchange channel (11) is perpendicular to the side of the base plate (4).
3. The method for preparing the long hole heat exchange channel at the interface of the explosive composite plate according to claim 1, characterized in that: The length of the long hole heat exchange channel (11) is not greater than 800 mm.
4. The method for preparing the long hole heat exchange channel at the interface of the explosive composite plate according to claim 1, characterized in that: There are a plurality of the long hole heat exchange channels (11), and the plurality of long hole heat exchange channels (11) are evenly and parallelly arranged along the side of the substrate (4) where the long hole heat exchange channels (11) are located.
5. The method for preparing the long hole heat exchange channel at the interface of the explosive composite plate according to claim 1, characterized in that: Step 1) The micropores are circular micropores with a diameter of 3 to 8 mm and a length of no more than 800 mm.
6. The method for preparing the long hole heat exchange channel at the interface of the explosive composite plate according to claim 1, characterized in that: In step 1), the micropores are elliptical micropores with a long diameter of 3 to 8 mm and a length of no more than 800 mm, and the long diameter of the elliptical micropores is perpendicular to the substrate.
7. The method for preparing the long hole heat exchange channel at the interface of the explosive composite plate according to claim 1, characterized in that: After the micropores are opened, the wire cutting cracks left on the opening surface are sealed with the same metal by surfacing welding and polished to make it smooth. During the explosive composite, the side with the micropores opened is placed on the inner side of the explosive composite.
8. The method for preparing the long hole heat exchange channel at the interface of the explosive composite plate according to any one of claims 1 to 7, characterized in that: The wire cutting method described in step 7) is specifically as follows: inserting a molybdenum wire into the microhole to expand the hole so that the hole is expanded to cross the composite plate bonding interface, that is, forming a heat exchange channel at the composite interface.