A welding method for spot welding of mobile phone antenna contacts
Through the methods of die-casting molding of mobile phone cases, injection molding of plastic parts, CNC treatment, spraying and spot welding, the problem of insufficient conductivity of traditional mobile phone antennas is solved, high strength and stability are achieved, 5G technology needs are met, and production is improved Efficiency and product quality.
Patent Information
- Application Number
- CN201910442081.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-05-24
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2039-05-24
AI Technical Summary
The conductivity of traditional mobile phone antennas is insufficient, especially in the application of 5G technology. The oxidation of antenna contacts leads to poor signal, and the prior art is difficult to ensure the stable conduction of the antenna.
Using a method including die-casting molding of mobile phone cases, injection molding of plastic parts, CNC treatment, spraying and spot welding, through high-temperature treated alloy raw materials and copper sheet spot welding technology, ensure high strength and stability of antenna contacts, and achieve efficient welding.
It improves the conductivity and product quality of mobile phone antennas, meets the needs of 5G technology, improves production efficiency, and reduces environmental pollution, and has significant economic and social value.
Smart Images

Figure CN110340610B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mobile phone shell design, and in particular to a welding method for spot welding of mobile phone antenna contacts. Background Art
[0002] With the continuous development of science and technology, people have higher and higher requirements for mobile phone network signals, and the disadvantages of traditional FPC antennas have begun to emerge, such as failure and falling off due to long-term glue. With the application and development of 5G technology, die-cast alloys have replaced TPC antennas, which also cause poor antenna conduction signals due to oxidation at the antenna contacts. The antenna performance of products is required to be higher, and only the stability of the antenna signal can ensure data transmission. Then the conductivity of the antenna is particularly important. At the current price range, the antennas of many mobile phone products are replaced by metal mold injection instead of traditional FPC antennas, but the contact point between the alloy and the motherboard contact is laser engraved. After a long time, the surface will oxidize and the effective conduction of the antenna cannot be guaranteed. Therefore, further improvement is needed. Summary of the invention
[0003] In view of the deficiencies of the above-mentioned prior art, the present invention provides a welding method for spot welding of mobile phone antenna contacts which is easy to operate, has a high yield rate, and can meet the requirements of 5G technology.
[0004] The technical solution adopted by the present invention to solve the above problems is:
[0005] The present invention provides a method for spot welding of mobile phone antenna contacts, comprising the following steps: (1) die-casting a mobile phone shell;
[0006] An initial alloy raw material of the mobile phone shell is prepared according to the composition ratio of the mobile phone shell, and the initial alloy raw material is fed into a die-casting mold through a feeding device after high-temperature treatment for die-casting to obtain a mobile phone shell body;
[0007] (2) Plastic injection molding
[0008] The mobile phone housing obtained in step (1) is subjected to plastic part injection molding operation through an injection mold and an injection molding device, wherein the plastic part injection molding includes a plastic part heating step and a plastic part cooling step, to form an initial mobile phone housing;
[0009] (3) CNC processing
[0010] The initial mobile phone shell obtained in step (2) is subjected to surface treatment so that the shell surface has gloss, which comprises the following steps:
[0011] Step (3.1) Line grinding and polishing: polishing the initial mobile phone housing surface;
[0012] Step (3.2) sandblasting the polished surface to give the polished surface a grainy feel;
[0013] Step (3.3) Remove grease from the surface of the phone case and remove residual liquid:
[0014] Step (3.4) is further polishing and cleaning to make the product surface clean.
[0015] (4) Spraying
[0016] The steps include:
[0017] Step (4.1) Surface dust removal: electrostatically remove dust from the product surface, and then spray the surface;
[0018] Step (4.2) applying primer, spraying the primer onto the mobile phone plastic part in a quantitative, uniform and continuous manner, and forming a uniform and continuous primer layer on the surface of the mobile phone plastic part after the primer is cured, so that the mobile phone plastic part presents the desired color effect;
[0019] Step (4.3) applying topcoat so that the topcoat evenly covers the primer layer to form a uniform and continuous topcoat layer;
[0020] Step (4.4) leveling treatment, leveling the mobile phone shell sprayed with topcoat;
[0021] (5) Spot welding
[0022] Step (5.1): Clean the antenna contacts in the phone case to prevent dust from entering;
[0023] Step (5.2): preparing copper sheets, and processing the required copper sheets according to the workpieces to be welded;
[0024] Step (5.3): Use a fixture to fit one side of the copper sheet tightly against the antenna contact, then apply the electrode cap of the welding gun directly to the copper sheet, and conduct heat to the surface of the antenna contact to be welded through the copper sheet to complete spot welding.
[0025] Furthermore, the components of the initial alloy raw material and the weight percentage of each component are: 1.0-3.0% manganese, 2.0-6.0% zinc, 0.1-1.0% magnesium, 0.01-2.0% titanium, 0.01%-1.0% tin, 0.8-1.2% silicon, 0.2-0.3% copper, and the balance is aluminum.
[0026] Furthermore, in the plastic part injection molding step of step (2), the injection mold comprises a front injection mold and a rear injection mold.
[0027] In the plastic part heating step, the mold temperature before injection molding is set to 80-120°C.
[0028] The mold temperature after injection molding is set at 80-120°C.
[0029] The holding time of the plastic part is set to 0.5 to 10 seconds.
[0030] Keep the pressure set at 50~200Mpa,
[0031] The cooling time in the plastic part cooling step is set to 1 to 50 seconds.
[0032] Furthermore, the primer layer in step (4.2) is prepared according to the ratio of primer crude oil: diluent = 1: (0.1-1).
[0033] Furthermore, the topcoat layer in step (4.3) is an ultraviolet-curable UV topcoat, which is prepared in a ratio of full-gloss UV topcoat: matte UV topcoat: diluent = 2:6: (8-9).
[0034] Furthermore, the thickness of the topcoat layer in step (4.2) is 5 to 10 μm.
[0035] Furthermore, the size of the copper sheet is (1-3) mm*(2-5) mm.
[0036] Furthermore, spot welding points are arranged on the copper sheet.
[0037] The beneficial effects of the present invention are:
[0038] The welding method for spot welding of mobile phone antenna contacts provided by the present invention has the advantages of convenient operation, high yield rate, and meeting the requirements of 5G technology. At the same time, the alloy of the mobile phone case prepared in this application can simultaneously achieve the comprehensive properties of high strength, anodization, and die-casting. The welding method for spot welding of mobile phone antenna contacts provided by this application effectively guarantees the quality of the product, while also improving production efficiency and reducing environmental pollution, and has great economic and social value. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a work flow chart of a welding method for spot welding of mobile phone antenna contacts of the present invention;
[0040] Figure 2 The present invention is a copper sheet structure diagram of a welding method for spot welding of mobile phone antenna contacts. DETAILED DESCRIPTION
[0041] The following specifically describes the embodiments of the present invention in conjunction with the accompanying drawings, which are only for reference and illustration and do not constitute a limitation on the scope of patent protection of the present invention.
[0042] Example 1
[0043] like Figure 1As shown, the present invention provides a welding method for spot welding of mobile phone antenna contacts, comprising the following steps: (1) die-casting of a mobile phone shell
[0044] An initial alloy raw material of the mobile phone shell is prepared according to the composition ratio of the mobile phone shell, and the initial alloy raw material is fed into a die-casting mold through a feeding device after high-temperature treatment for die-casting to obtain a mobile phone shell body;
[0045] (2) Plastic injection molding
[0046] The mobile phone housing obtained in step (1) is subjected to plastic part injection molding operation through an injection mold and an injection molding device, wherein the plastic part injection molding includes a plastic part heating step and a plastic part cooling step, to form an initial mobile phone housing;
[0047] (3) CNC processing
[0048] The initial mobile phone shell obtained in step (2) is subjected to surface treatment so that the shell surface has gloss, which comprises the following steps:
[0049] Step (3.1) Line grinding and polishing: polishing the initial mobile phone housing surface;
[0050] Step (3.2) sandblasting the polished surface to give the polished surface a grainy feel;
[0051] Step (3.3) Remove grease from the surface of the phone case and remove residual liquid:
[0052] Step (3.4) is further polishing and cleaning to make the product surface clean.
[0053] (4) Spraying
[0054] The steps include:
[0055] Step (4.1) Surface dust removal: electrostatically remove dust from the product surface, and then spray the surface;
[0056] Step (4.2) applying primer, spraying the primer onto the mobile phone plastic part in a quantitative, uniform and continuous manner, and forming a uniform and continuous primer layer on the surface of the mobile phone plastic part after the primer is cured, so that the mobile phone plastic part presents the desired color effect;
[0057] Step (4.3) applying topcoat so that the topcoat evenly covers the primer layer to form a uniform and continuous topcoat layer;
[0058] Step (4.4) leveling treatment, leveling the mobile phone shell sprayed with topcoat;
[0059] (5) Spot welding
[0060] Step (5.1): Clean the antenna contacts in the phone case to prevent dust from entering;
[0061] Step (5.2): preparing copper sheets, and processing the required copper sheets according to the workpieces to be welded;
[0062] Step (5.3): Use a fixture to fit one side of the copper sheet tightly against the antenna contact, then apply the electrode cap of the welding gun directly to the copper sheet, and conduct heat to the surface of the antenna contact to be welded through the copper sheet to complete spot welding.
[0063] In this embodiment, the components of the initial alloy raw material and the weight percentage of each component are: 1.5% manganese, 5% zinc, 0.5% magnesium, 1% titanium, 0.5% tin, 1% silicon, 2.5% copper, and the balance is aluminum.
[0064] In this embodiment, the injection mold in the plastic part injection molding step of step (2) includes a front injection mold and a rear injection mold.
[0065] In the plastic part heating step, the mold temperature before injection molding is set to 80°C.
[0066] The mold temperature after injection molding is set to 80°C.
[0067] The holding time of the plastic part is set to 1s.
[0068] Keep the pressure set to 60Mpa,
[0069] The cooling time in the plastic part cooling step is set to 35 seconds.
[0070] In this embodiment, the primer layer in step (4.2) is prepared according to the ratio of primer crude oil: diluent = 1:2.
[0071] In this embodiment, the topcoat layer in step (4.3) is an ultraviolet-curable UV topcoat, which is prepared in a ratio of full-gloss UV topcoat: matte UV topcoat: diluent = 2:6: (8-9).
[0072] In this embodiment, the thickness of the topcoat layer in step (4.2) is 5 μm.
[0073] In this embodiment, the size of the copper sheet is 2mm*3mm.
[0074] like Figure 1 As shown, in this embodiment, spot welding points are arranged on the copper sheet.
[0075] Example 2
[0076] The present invention provides a method for spot welding of mobile phone antenna contacts, comprising the following steps: (1) die-casting a mobile phone shell;
[0077] An initial alloy raw material of the mobile phone shell is prepared according to the composition ratio of the mobile phone shell, and the initial alloy raw material is fed into a die-casting mold through a feeding device after high-temperature treatment for die-casting to obtain a mobile phone shell body;
[0078] (2) Plastic injection molding
[0079] The mobile phone housing obtained in step (1) is subjected to plastic part injection molding operation through an injection mold and an injection molding device, wherein the plastic part injection molding includes a plastic part heating step and a plastic part cooling step, to form an initial mobile phone housing;
[0080] (3) CNC processing
[0081] The initial mobile phone shell obtained in step (2) is subjected to surface treatment so that the shell surface has gloss, which comprises the following steps:
[0082] Step (3.1) Line grinding and polishing: polishing the initial mobile phone housing surface;
[0083] Step (3.2) sandblasting the polished surface to give the polished surface a grainy feel;
[0084] Step (3.3) Remove grease from the surface of the phone case and remove residual liquid:
[0085] Step (3.4) is further polishing and cleaning to make the product surface clean.
[0086] (4) Spraying
[0087] The steps include:
[0088] Step (4.1) Surface dust removal: electrostatically remove dust from the product surface, and then spray the surface;
[0089] Step (4.2) applying primer, spraying the primer onto the mobile phone plastic part in a quantitative, uniform and continuous manner, and forming a uniform and continuous primer layer on the surface of the mobile phone plastic part after the primer is cured, so that the mobile phone plastic part presents the desired color effect;
[0090] Step (4.3) applying topcoat so that the topcoat evenly covers the primer layer to form a uniform and continuous topcoat layer;
[0091] Step (4.4) leveling treatment, leveling the mobile phone shell sprayed with topcoat;
[0092] (5) Spot welding
[0093] Step (5.1): Clean the antenna contacts in the phone case to prevent dust from entering;
[0094] Step (5.2): preparing copper sheets, and processing the required copper sheets according to the workpieces to be welded;
[0095] Step (5.3): Use a fixture to fit one side of the copper sheet tightly against the antenna contact, then apply the electrode cap of the welding gun directly to the copper sheet, and conduct heat to the surface of the antenna contact to be welded through the copper sheet to complete spot welding.
[0096] In this embodiment, the components of the initial alloy raw material and the weight percentage of each component are: 3.0% manganese, 6.0% zinc, 1.0% magnesium, 2.0% titanium, 1.0% tin, 0.8-1.2% silicon, 0.3% copper, and the balance is aluminum.
[0097] In this embodiment, the injection mold in the plastic part injection molding step of step (2) includes a front injection mold and a rear injection mold.
[0098] In the plastic part heating step, the mold temperature before injection molding is set to 90°C.
[0099] The mold temperature after injection molding is set to 90°C.
[0100] The holding time of the plastic part is set to 0.5 to 10 seconds.
[0101] Keep the pressure set at 50~200Mpa,
[0102] The cooling time in the plastic part cooling step is set to 1 to 50 seconds.
[0103] In this embodiment, the primer layer in step (4.2) is prepared according to the ratio of primer crude oil: diluent = 1:1.
[0104] In this embodiment, the topcoat layer in step (4.3) is an ultraviolet-curable UV topcoat, which is prepared in a ratio of full-gloss UV topcoat: matte UV topcoat: diluent = 2:6:9.
[0105] In this embodiment, the thickness of the topcoat layer in step (4.2) is 5 to 10 μm.
[0106] In this embodiment, the size of the copper sheet is 1mm*2mm.
[0107] In this embodiment, spot welding points are arranged on the copper sheet.
[0108] Example 3
[0109] The present invention provides a method for spot welding of mobile phone antenna contacts, comprising the following steps: (1) die-casting a mobile phone shell;
[0110] An initial alloy raw material of the mobile phone shell is prepared according to the composition ratio of the mobile phone shell, and the initial alloy raw material is fed into a die-casting mold through a feeding device after high-temperature treatment for die-casting to obtain a mobile phone shell body;
[0111] (2) Plastic injection molding
[0112] The mobile phone housing obtained in step (1) is subjected to plastic part injection molding operation through an injection mold and an injection molding device, wherein the plastic part injection molding includes a plastic part heating step and a plastic part cooling step, to form an initial mobile phone housing;
[0113] (3) CNC processing
[0114] The initial mobile phone shell obtained in step (2) is subjected to surface treatment so that the shell surface has gloss, which comprises the following steps:
[0115] Step (3.1) Line grinding and polishing: polishing the initial mobile phone housing surface;
[0116] Step (3.2) sandblasting the polished surface to give the polished surface a grainy feel;
[0117] Step (3.3) Remove grease from the surface of the phone case and remove residual liquid:
[0118] Step (3.4) is further polishing and cleaning to make the product surface clean.
[0119] (4) Spraying
[0120] The steps include:
[0121] Step (4.1) Surface dust removal: electrostatically remove dust from the product surface, and then spray the surface;
[0122] Step (4.2) applying primer, spraying the primer onto the mobile phone plastic part in a quantitative, uniform and continuous manner, and forming a uniform and continuous primer layer on the surface of the mobile phone plastic part after the primer is cured, so that the mobile phone plastic part presents the desired color effect;
[0123] Step (4.3) applying topcoat so that the topcoat evenly covers the primer layer to form a uniform and continuous topcoat layer;
[0124] Step (4.4) leveling treatment, leveling the mobile phone shell sprayed with topcoat;
[0125] (5) Spot welding
[0126] Step (5.1): Clean the antenna contacts in the phone case to prevent dust from entering;
[0127] Step (5.2): preparing copper sheets, and processing the required copper sheets according to the workpieces to be welded;
[0128] Step (5.3): Use a fixture to fit one side of the copper sheet tightly against the antenna contact, then apply the electrode cap of the welding gun directly to the copper sheet, and conduct heat to the surface of the antenna contact to be welded through the copper sheet to complete spot welding.
[0129] In this embodiment, the components of the initial alloy raw material and the weight percentage of each component are: 3.0% manganese, 2% zinc, 1.0% magnesium, 0.01% titanium, 1.0% tin, 0.8% silicon, 0.3% copper, and the balance is aluminum.
[0130] In this embodiment, the injection mold in the plastic part injection molding step of step (2) includes a front injection mold and a rear injection mold.
[0131] In the plastic part heating step, the mold temperature before injection molding is set to 80°C.
[0132] The mold temperature after injection molding is set to 80°C.
[0133] The holding time of the plastic part is set to 0.5s.
[0134] Keep the pressure set at 50~200Mpa,
[0135] The cooling time in the plastic part cooling step is set to 1 to 50 seconds.
[0136] In this embodiment, the primer layer in step (4.2) is prepared according to the ratio of primer crude oil: diluent = 1:0.2.
[0137] In this embodiment, the topcoat layer in step (4.3) is an ultraviolet-curable UV topcoat, which is prepared in a ratio of full-gloss UV topcoat: matte UV topcoat: diluent = 2:6:8.5.
[0138] In this embodiment, the thickness of the topcoat layer in step (4.2) is 7 μm.
[0139] In this embodiment, the size of the copper sheet is 3mm*4mm.
[0140] In this embodiment, spot welding points are arranged on the copper sheet.
[0141] The welding method for spot welding of mobile phone antenna contacts provided by the present invention has the advantages of convenient operation, high yield rate, and meeting the requirements of 5G technology. At the same time, the alloy of the mobile phone case prepared in this application can simultaneously achieve the comprehensive properties of high strength, anodization, and die-casting. The welding method for spot welding of mobile phone antenna contacts provided by this application effectively guarantees the quality of the product, while also improving production efficiency and reducing environmental pollution, and has great economic and social value.
[0142] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A welding method for spot welding of mobile phone antenna contacts, characterized in that: The following steps are involved: (1) Die-casting of mobile phone case An initial alloy raw material of the mobile phone shell is prepared according to the composition ratio of the mobile phone shell, and the initial alloy raw material is fed into a die-casting mold through a feeding device after high-temperature treatment for die-casting to obtain a mobile phone shell body; (2) Plastic injection molding The mobile phone housing obtained in step (1) is subjected to plastic part injection molding operation through an injection mold and an injection molding device, wherein the plastic part injection molding includes a plastic part heating step and a plastic part cooling step, to form an initial mobile phone housing; (3) CNC processing The initial mobile phone shell obtained in step (2) is subjected to surface treatment so that the shell surface has gloss, which comprises the following steps: Step (3.1) Line grinding and polishing: polishing the initial mobile phone housing surface; Step (3.2) sandblasting the polished surface to give the polished surface a grainy feel; Step (3.3) Remove grease from the surface of the phone case and remove residual liquid: Step (3.4) further polishing and cleaning to make the product surface clean; (4) Spraying The steps include: Step (4.1) Surface dust removal: electrostatically remove dust from the product surface, and then spray the surface; Step (4.2) applying primer, spraying the primer onto the mobile phone plastic part in a quantitative, uniform and continuous manner, and forming a uniform and continuous primer layer on the surface of the mobile phone plastic part after the primer is cured, so that the mobile phone plastic part presents the desired color effect; Step (4.3) applying topcoat so that the topcoat evenly covers the primer layer to form a uniform and continuous topcoat layer; Step (4.4) leveling treatment, leveling the mobile phone shell sprayed with topcoat; (5) Spot welding Step (5.1): Clean the antenna contacts in the phone case to prevent dust from entering; Step (5.2): preparing copper sheets, and processing the required copper sheets according to the workpieces to be welded; Step (5.3): Use a clamp to fit one side of the copper sheet tightly to the antenna contact, then directly apply the electrode cap of the welding gun to the copper sheet, and conduct heat to the surface of the antenna contact to be welded through the copper sheet to complete spot welding. The components of the initial alloy raw material and the weight percentage of each component are: 1.0-3.0% manganese, 2.0-6.0% zinc, 0.1-1.0% magnesium, 0.01-2.0% titanium, 0.01%-1.0% tin, 0.8-1.2% silicon, 0.2-0.3% copper, and the balance is aluminum.
2. A welding method for spot welding of mobile phone antenna contacts according to claim 1, characterized in that: The injection mold in the plastic part injection molding step of step (2) includes a front injection mold and a rear injection mold. In the plastic part heating step, the mold temperature before injection molding is set to 80-120°C. The mold temperature after injection molding is set at 80-120°C. The holding time of the plastic part is set to 0.5 to 10 seconds. Keep the pressure set at 50~200Mpa, The cooling time in the plastic part cooling step is set to 1 to 50 seconds.
3. A welding method for spot welding of mobile phone antenna contacts according to claim 1, characterized in that: The primer layer in step (4.2) is prepared according to the ratio of primer crude oil: diluent = 1: (0.1-1).
4. A welding method for spot welding of mobile phone antenna contacts according to claim 1, characterized in that: The topcoat layer in step (4.3) is an ultraviolet-curable UV topcoat, which is prepared according to the ratio of full-gloss UV topcoat: matte UV topcoat: diluent = 2:6: (8-9).
5. A welding method for spot welding of mobile phone antenna contacts according to claim 1, characterized in that: The thickness of the topcoat layer in step (4.2) is 5 to 10 μm.
6. A welding method for spot welding of mobile phone antenna contacts according to claim 1, characterized in that: The copper sheet has a size of (1-3) mm*(2-5) mm.
7. A welding method for spot welding of mobile phone antenna contacts according to claim 1, characterized in that: The copper sheet is provided with spot welding points.