In-mold label film and preparation method thereof

By employing a five-layer structure of paper-like coating, base layer, and adhesive layer in the in-mold label film, along with a specific raw material formula, the shortcomings of existing in-mold label films in terms of mechanical properties, printing effect, and adhesive performance are solved, achieving excellent comprehensive performance.

CN110619810BActive Publication Date: 2024-11-22江苏福泰涂布科技股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201911011652.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-10-23
Publication Date
2024-11-22
Estimated Expiration
2039-10-23

AI Technical Summary

Technical Problem

Existing in-mold label films struggle to combine excellent mechanical properties, rich printing effects, and superior adhesive performance.

Method used

It adopts a three-layer main structure of paper-like coating, base layer and adhesive layer. The base layer has a five-layer structure of outer surface layer, outer sub-surface layer, core layer, inner sub-surface layer and inner surface layer. The combination of specific thickness and raw material formula, combined with venting structure and transfer film layer, improves mechanical properties and adhesive properties.

Benefits of technology

It achieves excellent mechanical properties, rich printing effects and excellent adhesion of in-mold label film, thus improving the overall performance of label film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110619810B_ABST
    Figure CN110619810B_ABST
Patent Text Reader

Abstract

The present invention relates to an in-mold label film and a preparation method thereof, wherein the in-mold label film comprises a paper-like coating layer, a base layer and an adhesive layer stacked in sequence, wherein the base layer comprises an outer layer, an outer sub-surface layer, a core layer, an inner sub-surface layer and an inner surface layer stacked in sequence, wherein the outer layer is connected to the paper-like coating layer, and the inner surface layer is connected to the adhesive layer. The in-mold label film has excellent mechanical properties, adhesive properties and printing effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of label materials, and in particular relates to an in-mold label film and a preparation method thereof. Background Art

[0002] In-mold label film refers to pre-printed paper, synthetic or thin labels with special hot melt adhesive on the back, which are placed in the mold before plastic blowing, injection molding or thermoforming to produce plastic bottles or pots. The label and the container form a whole, and the label and the bottle body are basically on the same plane. The edge of the label is not visible, just like the image is printed directly on the surface of the bottle body. In-mold labeling no longer requires a labeling machine. Therefore, in-mold labeling is a new technology with great potential.

[0003] CN201725492U discloses an in-mold label, comprising a substrate layer having an upper surface and a lower surface, a printing layer attached to the upper surface of the substrate layer, and further comprising: an adhesive layer connected to the lower surface of the substrate layer; and a light layer connected to the other side of the printing layer. The in-mold label is not easy to peel off from the plastic container, and the light layer can be anti-static, anti-oil, and anti-oxidation, and the in-mold label is not easy to fade; in addition, the multi-layer structure of the in-mold label can make the ink of the printing layer adhere to the substrate layer smoothly, and better protect the pattern or text formed by the ink on the printing layer, and improve the scratch resistance and light resistance of the in-mold label.

[0004] CN108877486A discloses an in-mold label film and a preparation method thereof, comprising a polymer substrate film, a silver-plated printing film and an ethylene-vinyl acetate copolymer in-mold thermoplastic film, wherein the silver-plated printing film comprises a first adhesive layer, a silver-plated laser film, a second adhesive layer and a transparent protective layer, wherein the silver-plated laser film comprises a polymer substrate layer and a laser silver layer, wherein the silver-plated laser film enables the in-mold label film to have excellent glossiness, and in addition, the transparent protective layer not only ensures that the information on the in-mold label film is displayed to consumers in a complete and clear manner, but also protects the in-mold label film from external damage.

[0005] CN108922375A discloses a heat-crosslinked in-mold label film and a preparation method thereof. The heat-crosslinked in-mold label film is prepared by adhering a silver-plated printed film to the outer surface of a polymer substrate film, then coating a melted polyurethane adhesive on the inner surface of the polymer substrate film, then coating a melted high-density ethylene-vinyl acetate copolymer on the polyurethane adhesive, and curing to obtain a transition adhesive layer and a high-density ethylene-vinyl acetate copolymer in-mold thermoplastic layer, then coating a melted low-density ethylene-vinyl acetate copolymer on the high-density ethylene-vinyl acetate copolymer in-mold thermoplastic layer, and performing a cold-pressing operation using a cold-pressing anilox roller, forming a mesh exhaust grid on one side of the formed low-density ethylene-vinyl acetate copolymer in-mold thermoplastic layer, and obtaining an in-mold label with good exhaust performance.

[0006] At present, with the improvement of people's living standards and the advancement of science and technology, people have higher and higher requirements for product appearance, and high requirements for in-mold label films have emerged. However, it is difficult for in-mold labels in the existing technology to have excellent mechanical properties, rich printing effects, and excellent bonding properties. Therefore, it is necessary to develop a new in-mold label film that has excellent mechanical properties, rich printing effects and paper-like effects, and excellent bonding properties. Summary of the invention

[0007] In view of the deficiencies in the prior art, an object of the present invention is to provide an in-mold label film and a preparation method thereof.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] On the one hand, the present invention provides an in-mold label film, which includes a paper-like coating layer, a base layer and an adhesive layer stacked in sequence, wherein the base layer includes an outer layer, an outer sub-surface layer, a core layer, an inner sub-surface layer and an inner surface layer stacked in sequence, wherein the outer layer is connected to the paper-like coating layer, and the inner surface layer is connected to the adhesive layer.

[0010] The in-mold label film of the present invention has a three-layer main structure of a paper-like coating, a base layer and an adhesive layer, wherein the base layer further has a five-layer structure of an outer layer, an outer sub-surface layer, a core layer, an inner sub-surface layer and an inner surface layer. This unique structure enables the in-mold label film to have excellent mechanical properties.

[0011] Preferably, the thickness of the base layer is 50-110 μm, for example, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm or 110 μm.

[0012] Preferably, the thickness of the core layer is 35-85 μm, for example, 35 μm, 40 μm, 45 μm, 55 μm, 65 μm, 75 μm, 80 μm or 85 μm, etc. The core layer thickness is specifically selected within this range, so that the in-mold label film has a sufficient support effect. If the thickness is further increased, the overall thickness of the in-mold label will increase, and the integrity of the edge of the in-mold label and the container and the volume strength of the edge of the in-mold label will deteriorate. If the thickness is further reduced, the support effect will be limited, the mechanical properties will decrease, and the die-cutting performance will deteriorate.

[0013] Preferably, the raw materials for preparing the core layer include resin, antistatic agent and inorganic powder.

[0014] Preferably, the resin includes any one of copolymer polypropylene resin, homopolypropylene resin, low-density polyethylene resin or high-density polyethylene resin, or a combination of at least two of them. The combination of at least two is for example a combination of copolymer polypropylene resin and homopolypropylene resin, a combination of low-density polyethylene resin and high-density polyethylene resin, a combination of homopolypropylene resin and low-density polyethylene resin, etc. Other arbitrary combinations will not be described here one by one.

[0015] Preferably, the antistatic agent comprises any one of ethoxylated aliphatic alkylamine, ethoxylated alkyl acid amine, ethoxylated lauryl amide, glycerol-stearate, alkali metal alkyl sulfonate, alkali metal phosphate or alkali metal dithiocarbamate, or a combination of at least two thereof, such as a combination of ethoxylated aliphatic alkylamine and ethoxylated alkyl acid amine, a combination of ethoxylated lauryl amide and glycerol-stearate, a combination of alkali metal alkyl sulfonate and alkali metal phosphate, etc. Ethoxylated aliphatic alkylamine and / or ethoxylated alkyl acid amine are preferred.

[0016] Preferably, the inorganic substance includes any one of calcium carbonate, titanium dioxide, talc, barium sulfate or kaolin, or a combination of at least two thereof, such as a combination of calcium carbonate and titanium dioxide, a combination of talc and barium sulfate, a combination of titanium dioxide and barium sulfate, etc. Calcium carbonate and / or titanium dioxide are preferred.

[0017] Preferably, the mesh size of the inorganic powder is 100-3000 mesh, for example, 100 mesh, 200 mesh, 500 mesh, 800 mesh, 1000 mesh, 1500 mesh, 2000 mesh, 2500 mesh or 3000 mesh.

[0018] Preferably, the raw materials for preparing the core layer include, by weight, 50-90 parts of homopolymer or copolymer polypropylene resin, 5-40 parts of calcium carbonate powder, 1-5 parts of antistatic agent, and 0-10 parts of titanium dioxide powder.

[0019] The weight ratio of each prepared raw material in the core layer is a key factor affecting the product performance. Polypropylene resin is the material of the core layer and plays the role of muscle in the core layer. As the amount of acrylic resin added increases, the chemical resistance and mechanical properties improve; the inorganic powder plays the role of skeleton in the core layer. As the amount of inorganic powder added increases, the dimensional stability, hardness, rigidity and heat resistance gradually improve.

[0020] The weight proportion of the homopolymer or copolymer polypropylene resin may be 50 parts, 60 parts, 70 parts, 80 parts or 90 parts.

[0021] The weight proportions of the calcium carbonate powder may be 5 parts, 10 parts, 20 parts, 30 parts or 40 parts, etc.

[0022] The weight proportion of the antistatic agent can be 1 part, 2 parts, 3 parts, 4 parts or 5 parts.

[0023] The weight proportions of the titanium dioxide powder may be 0 parts, 1 parts, 2 parts, 4 parts, 6 parts, 8 parts or 10 parts, etc.

[0024] Preferably, the thickness of the outer sub-layer and the inner sub-layer is independently 5-10 μm, such as 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, etc. The thickness of the outer sub-layer and the inner sub-layer may be different.

[0025] Preferably, the raw materials for preparing the outer sub-surface layer and the inner sub-surface layer include resin, and the resin includes any one of copolymer polypropylene resin, homopolypropylene resin, low-density polyethylene resin or high-density polyethylene resin, or a combination of at least two of them. The combination of at least two of them can be, for example, a combination of copolymer polypropylene resin and homopolypropylene resin, a combination of low-density polyethylene resin and high-density polyethylene resin, a combination of homopolypropylene resin and low-density polyethylene resin, etc. Other arbitrary combinations will not be described here one by one.

[0026] The outer sub-surface layer and the inner sub-surface layer having the above characteristics can be closely combined with the core layer and can provide a matching transition layer for the surface layer.

[0027] Preferably, the raw materials for preparing the outer sub-surface layer and the inner sub-surface layer include 80-100 parts by weight of homopolymer or copolymer polypropylene resin and 0-20 parts by weight of high-density or low-density polyethylene resin.

[0028] The addition of polyethylene in the sub-surface layer and the inner sub-surface layer serves as a transition between the core layer and the outer layer. The content of copolymerized polypropylene resin or low-density polyethylene resin with higher bonding performance is gradually increased toward the outer layer.

[0029] The weight proportion of the homopolymer or copolymer polypropylene resin may be 80 parts, 85 parts, 90 parts, 95 parts or 100 parts, etc.

[0030] The weight proportions of the high-density or low-density polyethylene resin may be 0 parts, 1 parts, 2 parts, 4 parts, 8 parts, 10 parts, 15 parts, 18 parts or 20 parts, etc.

[0031] Preferably, the thickness of the outer layer and the inner layer is independently 5-10 μm, such as 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, etc. The thickness of the outer layer and the inner layer may be different.

[0032] Preferably, the raw materials for preparing the outer layer and the inner layer include resin, and the resin includes any one of copolymer polypropylene resin, homopolypropylene resin, low-density polyethylene resin or high-density polyethylene resin, or a combination of at least two of them. The combination of at least two is for example a combination of copolymer polypropylene resin and homopolypropylene resin, a combination of low-density polyethylene resin and high-density polyethylene resin, a combination of homopolypropylene resin and low-density polyethylene resin, etc. Other arbitrary combinations will not be described here one by one.

[0033] Specifically, the outer surface layer and the inner surface layer with the above characteristics can be closely combined with the sub-surface layer and can provide a suitable bonding surface for the paper-like coating layer and the bonding layer.

[0034] Preferably, the raw materials for preparing the outer surface layer and the inner surface layer include 50-100 parts by weight of homopolymer or copolymer polypropylene resin and 0-50 parts by weight of high-density or low-density polyethylene resin.

[0035] The weight ratio of the raw materials for preparing the outer layer and the inner layer is a key factor affecting the product performance. Compared with the sub-layer, the outer layer or the inner layer increases the content of the copolymerized polypropylene resin or the low-density polyethylene resin with higher bonding performance to provide a suitable bonding surface for the paper-like coating and the adhesive layer. If the content is too low, it may lead to poor fastness of the paper-like coating or poor bonding strength between the adhesive layer and the inner layer.

[0036] The weight proportion of the homopolymer or copolymer polypropylene resin may be 50 parts, 60 parts, 70 parts, 80 parts, 90 parts or 100 parts, etc.

[0037] The weight proportions of the high-density or low-density polyethylene resin may be 0 parts, 1 parts, 5 parts, 10 parts, 20 parts, 30 parts, 40 parts or 50 parts, etc.

[0038] The raw materials for the preparation of the surface layer and the sub-surface layer are similar, but the proportions of homopolymer or copolymer polypropylene resin and high-density or low-density polyethylene resin are different. The reason for this is: the core layer requires better mechanical properties, and the outer layer mainly requires better bonding properties. Gradually adding resins with good bonding properties from the core layer to the outside can ensure the bonding strength between layers.

[0039] Preferably, the thickness of the paper-like coating is 5-10 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm.

[0040] Preferably, the raw materials for preparing the paper-like coating include resin and inorganic powder.

[0041] Preferably, the resin includes any one of homopolymer acrylic resin, copolymer acrylic resin, polyisocyanate resin or amino resin, or a combination of at least two of them. The combination of at least two of them is, for example, a combination of homopolymer acrylic resin and copolymer acrylic resin, a combination of copolymer acrylic resin and polyisocyanate resin, a combination of polyisocyanate resin and amino resin, etc. Other arbitrary combinations will not be described here one by one.

[0042] Preferably, the inorganic substance includes any one of calcium carbonate, titanium dioxide, talc, barium sulfate or kaolin, or a combination of at least two thereof, such as a combination of calcium carbonate and titanium dioxide, a combination of talc and barium sulfate, a combination of titanium dioxide and barium sulfate, etc.

[0043] Preferably, the mesh size of the inorganic powder is 100-3000 mesh, for example, 100 mesh, 200 mesh, 500 mesh, 800 mesh, 1000 mesh, 1500 mesh, 2000 mesh, 2500 mesh or 3000 mesh.

[0044] The addition of inorganic powder of specific type and specific particle size makes the paper-like coating have good printing adaptability.

[0045] Preferably, the raw materials for preparing the paper-like coating include, by weight, 50-90 parts of homopolymer or copolymer acrylic resin, 0-20 parts of polyisocyanate resin, 0-20 parts of amino resin, and 5-30 parts of inorganic powder.

[0046] The weight proportion of the homopolymer or copolymer acrylic resin may be 50 parts, 60 parts, 70 parts, 80 parts or 90 parts.

[0047] The weight proportion of the polyisocyanate resin may be 0 parts, 1 parts, 2 parts, 5 parts, 8 parts, 10 parts, 15 parts or 20 parts.

[0048] The weight proportions of the amino resin may be 0 parts, 1 parts, 2 parts, 5 parts, 8 parts, 10 parts, 15 parts or 20 parts, etc.

[0049] The weight proportions of the inorganic powder may be 5 parts, 10 parts, 15 parts, 18 parts, 20 parts, 22 parts, 25 parts, 28 parts or 30 parts, etc.

[0050] Preferably, the raw materials for preparing the paper-like coating further include 0-5 parts of auxiliary agents by weight, such as 0 part, 1 part, 2 parts, 3 parts, 4 parts or 5 parts.

[0051] Preferably, the auxiliary agent includes any one of a dispersant, a leveling agent or an anti-settling agent, or a combination of at least two of them. The combination of at least two of them is, for example, a combination of a dispersant and a leveling agent, a combination of a leveling agent and an anti-settling agent, a combination of a dispersant and an anti-settling agent, etc. Other arbitrary combinations are not described here one by one.

[0052] Preferably, the thickness of the adhesive layer is 15-25 μm, for example, 15 μm, 17 μm, 18 μm, 20 μm, 22 μm, 24 μm or 25 μm.

[0053] Preferably, the raw materials for preparing the adhesive layer include 98-100 parts of resin and 0-2 parts of antistatic agent.

[0054] Preferably, the resin includes any one of low-density polyethylene resin, high-density polyethylene resin, copolymerized polypropylene resin, homopolypropylene resin, ethylene acrylic acid copolymer resin, ethylene methyl acrylate copolymer resin, ethylene ethyl acrylate copolymer resin, and ethylene butyl acrylate copolymer resin, or a combination of at least two of them. The combination of at least two of them can be, for example, a combination of low-density polyethylene resin and high-density polyethylene resin, a combination of copolymerized polypropylene resin and homopolypropylene resin, a combination of ethylene acrylic acid copolymer resin and ethylene methyl acrylate copolymer resin, and the like. Any other combinations will not be described here one by one.

[0055] The addition of the ethylene acrylic acid copolymer resin and the ethylene acrylate copolymer resin can significantly improve the bonding performance of the bonding layer, that is, the composite strength of the bonding layer is significantly improved.

[0056] Preferably, the antistatic agent comprises any one or a combination of at least two of ethoxylated fatty alkyl amines, ethoxylated alkyl acid amines, ethoxylated lauryl amide, glycerol stearate, alkali metal alkyl sulfonates, alkali metal phosphates or alkali metal dithiocarbamates; preferably ethoxylated fatty alkyl amines and / or ethoxylated alkyl acid amines.

[0057] Preferably, the raw materials for preparing the adhesive layer include, by weight, 50-100 parts of high-density or low-density polyethylene resin, 0-50 parts of homopolymer or copolymer polypropylene resin, 0-50 parts of ethylene acrylic acid copolymer resin, and 0-50 parts of ethylene acrylate copolymer resin.

[0058] The combination of the above-mentioned specific types and specific weight proportions of resins enables the in-mold label film of the present invention to have excellent adhesive properties.

[0059] The weight proportion of the high-density or low-density polyethylene resin may be 50 parts, 60 parts, 70 parts, 80 parts, 90 parts or 100 parts, etc.

[0060] The weight proportions of the homopolymer or copolymer polypropylene resin may be 0, 5, 10, 20, 30, 35, 40 or 50 parts, etc.

[0061] The weight proportions of the ethylene acrylic acid copolymer resin may be 0 parts, 5 parts, 10 parts, 20 parts, 30 parts, 35 parts, 40 parts or 50 parts, etc.

[0062] The weight proportions of the ethylene acrylate copolymer resin (including ethylene methyl acrylate copolymer resin, ethylene ethyl acrylate copolymer resin, ethylene butyl acrylate copolymer resin) can be 0 parts, 5 parts, 10 parts, 20 parts, 30 parts, 35 parts, 40 parts or 50 parts, etc.

[0063] Preferably, the adhesive layer has an exhaust structure, and the exhaust structure is a diamond-shaped, rectangular or hexagonal air guide groove, and the cross-section of the air guide groove is a "V" shape or a "︺" shape.

[0064] Preferably, the depth of the air guide groove is 5-15 μm, for example, 5 μm, 7 μm, 8 μm, 10 μm, 12 μm, 13 μm, 14 μm or 15 μm.

[0065] The above-mentioned venting structure can further improve the adhesive performance of the in-mold label film involved in the present invention.

[0066] In the present invention, the in-mold label film further comprises an adhesive layer and an aluminum-plated or silver-plated transfer layer stacked in sequence, and the adhesive layer is connected to the paper-like coating layer.

[0067] Preferably, the aluminum-plated transfer layer includes a transfer layer of an aluminum-plated transfer film or an aluminum-plated laser transfer film.

[0068] Preferably, the silver-plated transfer layer comprises a transfer layer of a silver-plated transfer film or a silver-plated laser transfer film.

[0069] Preferably, the transfer film layer has a thickness of 30-300 nm, for example, 30 nm, 40 nm, 50 nm, 80 nm, 100 nm, 150 nm, 200 nm or 300 nm.

[0070] Preferably, the thickness of the adhesive layer is 1-3 μm, such as 1 μm, 2 μm or 3 μm.

[0071] Preferably, the adhesive comprises acrylic adhesive, polyurethane adhesive or epoxy adhesive.

[0072] On the other hand, the present invention provides a method for preparing the in-mold label film as described above, the preparation method comprising: preparing a paper-like coating paint and an adhesive layer paint by mixing the raw material formula, applying the paper-like coating paint and the adhesive layer paint on the outer surface and the inner surface of the base layer respectively, and curing them to obtain the in-mold label film.

[0073] Preferably, the preparation method of the base layer is: the outer layer, outer sub-surface layer, core layer, inner sub-surface layer and inner surface layer are mixed according to the raw material formula respectively and extruded by co-extrusion, cooled, longitudinally stretched, tempered, transversely stretched, tempered and cooled, and corona treated to obtain the base layer.

[0074] Preferably, the co-extrusion temperature is 180-330°C, for example, 180°C, 200°C, 220°C, 250°C, 280°C, 300°C, 320°C or 330°C.

[0075] Preferably, the temperature of the longitudinal stretching is 110-160°C, such as 110°C, 120°C, 130°C, 140°C, 150°C or 160°C.

[0076] Preferably, the temperature of the transverse stretching is 140-190°C, for example, 140°C, 150°C, 160°C, 170°C, 180°C or 190°C.

[0077] Preferably, the paper-like coating material is applied by roller coating.

[0078] Preferably, the adhesive layer coating is applied in a casting manner.

[0079] Preferably, after the adhesive layer coating is applied, the air guide grooves are cold pressed out using an anilox roller.

[0080] Preferably, the curing temperature is 90-150°C, for example, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C.

[0081] Preferably, the preparation method further comprises: after applying the adhesive layer on the transfer film layer and drying it, laminating it with the imitation paper coating in the in-mold label film, peeling off the polyester film, and aging. This step is to obtain an in-mold label film with a bright silver effect or a laser effect. The aluminum (silver) transfer film or aluminum (silver) laser transfer film is formed by vacuum evaporation of aluminum (silver) on a polyester film or a polyester film with a molded laser pattern, and the thickness of the aluminum (silver) layer is 30-300nm. The aluminum / silver transfer film or aluminum / silver laser transfer film is formed by vacuum aluminum or silver plating on a polyester film.

[0082] As a preferred technical solution of the present invention, the method for preparing the in-mold label film specifically comprises the following steps:

[0083] (1) Five different formulations are extruded into five-layer extrudates through an extruder; the extrudates are extruded through the same die head in a five-layer co-extrusion mode at 180-330° C., and a sheet is obtained after cooling; the sheet is longitudinally stretched by a stretching device at 110-160° C., tempered and cooled, transversely stretched by a stretching device at 140-190° C., tempered and cooled, and corona treated to obtain a five-layer base layer with a thickness of 50-110 μm.

[0084] (2) Paper-like coating The coating is evenly applied to the outer surface of the base layer by roller coating and cured at 90-150° C. to obtain a paper-like coating with paper-like effect.

[0085] (3) The inner surface of the base layer is corona treated with a corona treatment amount of 4000-6000 J / m 2 The resin is coated on the inner surface of the base layer through the same die head at 180-330°C by casting, and the air-conducting grooves with diamond, rectangle and hexagon shapes are cold pressed by an anilox roller to obtain an adhesive layer with an air-conducting structure with a thickness of 15-25μm.

[0086] (4) The adhesive layer is coated on the aluminum (silver) layer of the aluminum (silver) transfer film or the aluminum (silver) laser transfer film by a knife scraping method. After drying, the transfer film coated with the adhesive is pressed with the imitation paper coating, and the polyester film is peeled off. After aging in an aging room at 30-80° C., an aluminum (silver) layer with a bright silver effect and a laser effect is obtained.

[0087] Compared with the prior art, the present invention has the following beneficial effects:

[0088] The in-mold label film involved in the present invention has a three-layer main structure of a paper-like coating, a base layer and an adhesive layer, wherein the base layer further has a five-layer structure of an outer surface layer, an outer sub-surface layer, a core layer, an inner sub-surface layer and an inner surface layer. This unique structure enables the in-mold label film to have excellent mechanical properties. Compared with the prior art, the total thickness of the label film is not much different. The thickness of the core layer is increased to 35-85 μm, which can provide sufficient support effect for the label film, that is, better mechanical properties, while the thickness of the adhesive layer is reduced to 15-25 μm, but the special raw material formula and exhaust structure of the adhesive layer make it still have adhesive properties. At the same time, the paper-like coating and transfer film layer in the in-mold label film of the present invention provide the label film with rich printing effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0089] Figure 1 1 is a schematic structural diagram of the in-mold label film involved in the present invention, wherein 11 is a core layer, 12 is an outer sub-surface layer, 13 is an inner sub-surface layer, 14 is an outer surface layer, 15 is an inner surface layer, 20 is a paper-like coating layer, 30 is a bonding layer, 41 is an adhesive layer, and 42 is an aluminum-plated layer or a silver-plated layer;

[0090] Figure 2 It is a schematic diagram of an adhesive layer with a venting structure in the in-mold label film of the present invention. DETAILED DESCRIPTION

[0091] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0092] Example 1

[0093] The present embodiment provides an in-mold label film, which includes an 8μm paper-like coating layer, a 67μm base layer and a 20μm adhesive layer stacked in sequence, and the base layer includes an outer layer of 5μm, an outer sub-surface layer of 5μm, a core layer of 47μm, an inner sub-surface layer of 5μm and an inner surface layer of 5μm stacked in sequence, wherein the outer layer is connected to the paper-like coating layer, and the inner surface layer is connected to the adhesive layer.

[0094] The raw materials for the core layer are: 77% homopolypropylene resin (MI: 2.2), 3% ethoxylated lauryl amide, 15% calcium carbonate powder and 5% titanium dioxide powder. The raw materials for the outer layer are: 100% copolymerized polypropylene resin (MI: 15.0). The raw materials for the outer sub-surface layer are: 50% homopolypropylene resin (MI: 3.2) and 50% copolymerized polypropylene resin (MI: 15.0). The raw materials for the inner sub-surface layer are: 100% homopolypropylene resin (MI: 3.2). The raw materials for the inner surface layer are: 100% homopolypropylene resin (MI: 3.2). The raw materials for the paper-like layer are: 80% copolymerized acrylic resin (MI: 60), 5% additives (dispersant: BYK110, leveling agent: BYK300, mixed in equal proportions), 10% calcium carbonate powder and 5% titanium dioxide powder. The raw materials for preparing the adhesive layer are: 98% low-density polyethylene resin (MI: 7.0) and 2% antistatic agent (ethoxylated lauryl amide).

[0095] The preparation method thereof comprises the following steps:

[0096] (1) The five different raw materials of the outer surface layer, outer sub-surface layer, core layer, inner sub-surface layer and inner surface layer are mixed respectively and extruded into five-layer extrudates through an extruder; the extrudates are extruded through the same die head in a five-layer co-extrusion manner at 200° C., and a plate is obtained after cooling; the plate is longitudinally stretched by a stretching device at 150° C., tempered and cooled, transversely stretched by a stretching device at 180° C., tempered and cooled, and corona treated to obtain a five-layer base layer with a thickness of 67 μm;

[0097] (2) mixing the raw materials of the paper-like coating and coating them on the outer surface of the base layer obtained in step (1) by means of an anilox roller, curing at 120° C., and cooling to obtain a paper-like coating with a thickness of 8 μm and having a paper-like effect;

[0098] (3) Mix the raw materials of the adhesive layer and apply them on the inner surface of the base layer after corona treatment through the same die head by casting at 250° C., and use an anilox roller to cold-press a diamond-shaped air-conducting groove with a depth of 10 μm, and cool it to obtain an adhesive layer with a thickness of 20 μm and an air-conducting structure. Finally, the in-mold label film is obtained.

[0099] Example 2

[0100] The present embodiment provides an in-mold label film, which includes a 5μm paper-like coating layer, a 55μm base layer and a 15μm adhesive layer stacked in sequence, and the base layer includes an outer layer of 5μm, an outer sub-surface layer of 5μm, a core layer of 35μm, an inner sub-surface layer of 5μm and an inner surface layer of 5μm stacked in sequence, wherein the outer layer is connected to the paper-like coating layer, and the inner surface layer is connected to the adhesive layer.

[0101] The raw materials for the core layer are: 75% copolymerized polypropylene resin (MI: 2.2), 5% ethoxylated lauryl amide, 15% calcium carbonate powder and 5% titanium dioxide powder. The raw materials for the outer layer are: 100% copolymerized polypropylene resin (MI: 15.0). The raw materials for the outer sub-surface layer are: 50% homopolymerized polypropylene resin (MI: 3.2) and 50% copolymerized polypropylene resin (MI: 15.0). The raw materials for the inner sub-surface layer are: 50% homopolymerized polypropylene resin (MI: 3.2) and 50% copolymerized polypropylene resin (MI: 15.0). The raw materials for the inner surface layer are: 70% copolymerized polypropylene resin (MI: 15.0) and 30% low-density polyethylene resin (MI: 7.0). The raw materials for the paper-like layer are: 80% copolymerized acrylic resin (MI: 60), 5% additives (dispersant: BYK110, leveling agent: BYK300, mixed in equal proportions), 10% calcium carbonate powder and 5% titanium dioxide powder. The raw materials for preparing the adhesive layer are: 50% low-density polyethylene resin (MI: 7.0) and 50% ethylene butyl acrylate copolymer resin (MI: 8.0).

[0102] The preparation method thereof comprises the following steps:

[0103] (1) The five different raw materials of the outer surface layer, outer sub-surface layer, core layer, inner sub-surface layer and inner surface layer are mixed separately and extruded into five-layer extrudates through an extruder; the extrudates are extruded through the same die head in a five-layer co-extrusion manner at 180° C., and a sheet is obtained after cooling; the sheet is longitudinally stretched by a stretching device at 110° C., tempered and cooled, transversely stretched by a stretching device at 140° C., tempered and cooled, and corona treated to obtain a five-layer base layer with a thickness of 55 μm;

[0104] (2) mixing the raw materials of the paper-like coating and coating them on the outer surface of the base layer obtained in step (1) by means of an anilox roller, curing at 90° C., and cooling to obtain a paper-like coating with a thickness of 5 μm and having a paper-like effect;

[0105] (3) Mix the raw materials of the adhesive layer and apply them on the inner surface of the base layer after corona treatment through the same die head by casting at 180° C., and use an anilox roller to cold-press a diamond-shaped air-conducting groove with a depth of 10 μm, and cool it to obtain an adhesive layer with a thickness of 15 μm and an air-conducting structure. Finally, the in-mold label film is obtained.

[0106] Example 3

[0107] The present embodiment provides an in-mold label film, which includes a 10 μm paper-like coating layer, an 80 μm base layer and a 25 μm adhesive layer stacked in sequence, the base layer includes an outer layer of 10 μm, an outer sub-surface layer of 5 μm, a core layer of 50 μm, an inner sub-surface layer of 5 μm and an inner surface layer of 10 μm stacked in sequence, wherein the outer layer is connected to the paper-like coating layer, and the inner surface layer is connected to the adhesive layer.

[0108] The raw materials for the core layer are: 75% homopolypropylene resin (MI: 2.2), 5% ethoxylated lauryl amide, 15% calcium carbonate powder and 5% titanium dioxide powder. The raw materials for the outer layer are: 70% copolymerized polypropylene resin (MI: 15.0) and 30% low-density polyethylene resin (MI: 7.0). The raw materials for the outer sub-layer are: 90% homopolypropylene resin (MI: 3.2) and 10% low-density polyethylene resin (MI: 7.0). The raw materials for the inner sub-layer are: 90% homopolypropylene resin (MI: 3.2) and 10% low-density polyethylene resin (MI: 7.0). The raw materials for the inner layer are: 70% copolymerized polypropylene resin (MI: 15.0) and 30% low-density polyethylene resin (MI: 7.0). The raw materials for preparing the paper-like layer are: 60% copolymerized acrylic resin (MI: 80), 20% polyisocyanate resin (HDI), 5% additives (dispersant: BYK110, leveling agent: BYK300, mixed in equal proportions), 10% calcium carbonate powder and 5% titanium dioxide powder. The raw materials for preparing the adhesive layer are: 30% copolymerized polypropylene resin (MI: 15.0), 20% ethylene butyl acrylate copolymerized resin (MI: 8.0), 20% ethylene ethyl acrylate copolymerized resin (MI: 6.0) and 30% ethylene acrylic acid copolymerized resin (MI: 60.0).

[0109] The preparation method thereof comprises the following steps:

[0110] (1) The five different raw materials of the outer surface layer, outer sub-surface layer, core layer, inner sub-surface layer and inner surface layer are mixed separately and extruded into five-layer extrudates through an extruder; the extrudates are extruded through the same die head in a five-layer co-extrusion manner at 300° C., and a sheet is obtained after cooling; the sheet is longitudinally stretched by a stretching device at 160° C., tempered and cooled, transversely stretched by a stretching device at 190° C., tempered and cooled, and corona treated to obtain a base layer with a five-layer structure having a thickness of 100 μm;

[0111] (2) mixing the raw materials of the paper-like coating and applying them to the outer surface of the base layer obtained in step (1) by roller coating with an anilox roller, curing at 130° C., and cooling to obtain a paper-like coating with a thickness of 10 μm and having a paper-like effect;

[0112] (3) Mix the raw materials of the adhesive layer and apply them on the inner surface of the base layer after corona treatment through the same die head by casting at 300° C., and use an anilox roller to cold-press a diamond-shaped air-conducting groove with a depth of 10 μm, and cool it to obtain an adhesive layer with a thickness of 25 μm and an air-conducting structure. Finally, the in-mold label film is obtained.

[0113] Example 4

[0114] This embodiment provides a bright silver in-mold label film, and the structure of the bright silver in-mold label film is different from that of the embodiment 3 only in that the outer surface is also covered with an aluminum-plated transfer polyester film.

[0115] The preparation method thereof comprises the following steps:

[0116] (1)-(3) are consistent with Example 3;

[0117] (4) The surface of the aluminum-plated transfer polyester film is evenly coated with an acrylic adhesive by knife scraping. After drying, the transfer film coated with the adhesive is pressed with the paper-like coating of the product obtained in step (3), the polyester film is peeled off, and the aluminum-plated layer is obtained after aging in an aging chamber at 60° C. The thickness of the acrylic adhesive is 2 μm, and the thickness of the aluminum layer is 30 nm.

[0118] Example 5

[0119] This embodiment provides a laser in-mold label film, the structure of which is different from that of the embodiment 3 only in that the outer surface is also covered with an aluminum-plated laser transfer polyester film.

[0120] The preparation method thereof comprises the following steps:

[0121] (1)-(3) are consistent with Example 3;

[0122] (4) The surface of the aluminum-plated laser transfer polyester film is evenly coated with an acrylic adhesive by knife scraping. After drying, the transfer film coated with the adhesive is pressed with the paper-like coating of the product obtained in step (3), the polyester film is peeled off, and the aluminum-plated laser layer is obtained after curing in a curing chamber at 60° C. The thickness of the acrylic adhesive is 2 μm, and the thickness of the aluminum layer is 30 nm.

[0123] Example 6

[0124] The present embodiment provides an in-mold label film, which includes a 10 μm paper-like coating layer, a 110 μm base layer and a 25 μm adhesive layer stacked in sequence, and the base layer includes an outer layer of 10 μm, an outer sub-surface layer of 5 μm, a core layer of 80 μm, an inner sub-surface layer of 5 μm and an inner surface layer of 10 μm stacked in sequence, wherein the outer layer is connected to the paper-like coating layer, and the inner surface layer is connected to the adhesive layer.

[0125] The raw materials for preparing each layer are consistent with those in Example 3.

[0126] The preparation method thereof is similar to that in Example 3.

[0127] Example 7

[0128] The present embodiment provides an in-mold label film, which includes a 10 μm paper-like coating layer, a 50 μm base layer and a 25 μm adhesive layer stacked in sequence, and the base layer includes an outer layer of 10 μm, an outer sub-surface layer of 5 μm, a core layer of 20 μm, an inner sub-surface layer of 5 μm and an inner surface layer of 10 μm stacked in sequence, wherein the outer layer is connected to the paper-like coating layer, and the inner surface layer is connected to the adhesive layer.

[0129] The raw materials for preparing each layer are consistent with those in Example 3.

[0130] The preparation method thereof is similar to that in Example 3.

[0131] Example 8

[0132] The present embodiment provides an in-mold label film, which includes a 10 μm paper-like coating layer, an 80 μm base layer and a 25 μm adhesive layer stacked in sequence, the base layer includes an outer layer of 10 μm, an outer sub-surface layer of 5 μm, a core layer of 50 μm, an inner sub-surface layer of 5 μm and an inner surface layer of 10 μm stacked in sequence, wherein the outer layer is connected to the paper-like coating layer, and the inner surface layer is connected to the adhesive layer.

[0133] The raw materials for preparing each layer are different from those in Example 3 only in that the raw material for preparing the adhesive layer is 100% homopolypropylene resin, and the rest are the same.

[0134] The preparation method thereof is similar to that in Example 3.

[0135] Comparative Example 1

[0136] This comparative example provides an in-mold label film, which includes a 10 μm paper-like coating layer, an 80 μm core layer and a 25 μm adhesive layer stacked in sequence. The base layer of this comparative example does not have a 5-layer structure, but only has one layer, namely, the core layer. Others are the same.

[0137] The raw materials for preparing each layer are consistent with those in Example 3.

[0138] The preparation method thereof is similar to that in Example 3.

[0139] Comparative Example 2

[0140] This comparative example provides an in-mold label film, which includes a 10 μm paper-like coating layer, an 80 μm base layer, and a 25 μm adhesive layer stacked in sequence. The base layer includes an outer layer of 10 μm, a core layer of 60 μm, and an inner layer of 10 μm stacked in sequence, wherein the outer layer is connected to the paper-like coating layer, and the inner layer is connected to the adhesive layer. The base layer of this comparative example does not have a 5-layer structure, but only has 3 layers, namely, an outer layer, a core layer, and an inner layer. The others are the same.

[0141] The raw materials for preparing each layer are consistent with those in Example 3.

[0142] The preparation method thereof is similar to that in Example 3.

[0143] Comparative Example 3

[0144] This comparative example provides an in-mold label film, which includes an 8μm paper-like coating layer, a 67μm core layer and a 20μm adhesive layer stacked in sequence. The base layer of this comparative example does not have a 5-layer structure, but only has one layer, namely the core layer. The others are the same.

[0145] The raw materials for preparing each layer are consistent with those in Example 1.

[0146] The preparation method thereof is similar to that in Example 1.

[0147] Comparative Example 4

[0148] This comparative example provides an in-mold label film, which includes an 8μm paper-like coating, a 67μm base layer and a 20μm adhesive layer stacked in sequence. The base layer includes an outer layer of 5μm, a core layer of 57μm and an inner layer of 5μm stacked in sequence, wherein the outer layer is connected to the paper-like coating, and the inner layer is connected to the adhesive layer. The base layer of this comparative example does not have a 5-layer structure, but only has 3 layers, namely, an outer layer, a core layer and an inner layer. The others are the same.

[0149] The raw materials for preparing each layer are consistent with those in Example 1.

[0150] The preparation method thereof is similar to that in Example 1.

[0151] Example 9

[0152] Evaluation test:

[0153] In this example, the label film products prepared in Examples 1-8 and Comparative Examples 1-4 were evaluated on the following indicators:

[0154] 1. Mechanical properties evaluation

[0155] (1) Determination of thermal shrinkage rate: method: GB / T 26192-2010.

[0156] (2) Warpage value determination, evaluation standard: GB / T 25257-2010.

[0157] (3) Thickness measurement: method: GB / T 451.3-2002.

[0158] 2. Evaluation of bonding effect

[0159] (1) Composite strength measurement: The composite strength of the sample is measured using a tensile and compression testing machine with a width of 15 mm, a 90° peeling angle, and a peeling speed of 150 mm / min.

[0160] 3. Evaluation of printing effect

[0161] (1) Whiteness determination method: GB / T 7974-2013.

[0162] (2) Opacity determination method: GB / T 1543-2005.

[0163] (3) Roughness determination method: GB / T 1031-2009.

[0164] The results are shown in Table 1:

[0165] Table 1

[0166]

[0167] It can be seen from the data in Table 1 that the in-mold label film involved in the present invention has excellent mechanical properties, adhesive properties and printing effects; comparing Example 3 with Comparative Examples 1 and 2 or comparing Example 1 with Comparative Examples 3 and 4, the unique 5-layer base structure can significantly increase the composite strength of the label film; comparing Example 3 with Examples 6 and 7, the thickness of the core layer is one of the key factors affecting the product performance; comparing Example 3 with Example 8, the resin composition of the adhesive layer is also one of the key factors affecting the product performance.

[0168] The applicant declares that the present invention illustrates an in-mold label film and a preparation method thereof through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0169] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0170] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

Claims

1. An in-mold label film, It is characterized in that The in-mold label film comprises a paper-like coating layer, a base layer and an adhesive layer stacked in sequence, wherein the base layer comprises an outer layer, an outer sub-surface layer, a core layer, an inner sub-surface layer and an inner surface layer stacked in sequence, wherein the outer layer is connected to the paper-like coating layer, and the inner surface layer is connected to the adhesive layer; The raw materials for preparing the core layer include 50-90 parts of homopolymer or copolymer polypropylene resin, 5-40 parts of calcium carbonate powder, 1-5 parts of antistatic agent, and 0-10 parts of titanium dioxide powder by weight; The raw materials for preparing the outer surface layer and the inner surface layer include 50-100 parts of homopolymer or copolymer polypropylene resin and 0-50 parts of high-density or low-density polyethylene resin in parts by weight.

2. The in-mold label film according to claim 1, It is characterized in that The thickness of the base layer is 50-110 μm.

3. The in-mold label film according to claim 1, It is characterized in that The thickness of the core layer is 35-85 μm.

4. The in-mold label film according to claim 1, It is characterized in that The antistatic agent includes any one of ethoxylated fatty alkyl amines, ethoxylated alkyl acid amines, ethoxylated lauryl amide, glycerol stearate, alkali metal alkyl sulfonates, alkali metal phosphates, or alkali metal dithiocarbamates, or a combination of at least two thereof.

5. The in-mold label film according to claim 4, It is characterized in that The antistatic agent is ethoxylated aliphatic alkylamine and / or ethoxylated alkyl acid amine.

6. The in-mold label film according to claim 1, It is characterized in that The mesh size of the titanium dioxide powder is 100-3000 meshes.

7. The in-mold label film according to claim 1, It is characterized in that The thickness of the outer sub-layer and the inner sub-layer are independently 5-10 μm.

8. The in-mold label film according to claim 1, It is characterized in that The raw materials for preparing the outer sub-surface layer and the inner sub-surface layer include resin, and the resin includes any one of copolymer polypropylene resin, homopolypropylene resin, low-density polyethylene resin or high-density polyethylene resin, or a combination of at least two thereof.

9. The in-mold label film according to claim 8, It is characterized in that The raw materials for preparing the outer sub-surface layer and the inner sub-surface layer include 80-100 parts of homopolymer or copolymer polypropylene resin and 0-20 parts of high-density or low-density polyethylene resin by weight.

10. The in-mold label film according to claim 1, It is characterized in that The thickness of the outer layer and the inner layer is independently 5-10 μm.

11. The in-mold label film according to claim 1, It is characterized in that The thickness of the paper-like coating is 5-10 μm.

12. The in-mold label film according to claim 1, It is characterized in that The raw materials for preparing the paper-like coating include resin and inorganic powder.

13. The in-mold label film according to claim 12, It is characterized in that The resin includes any one of homopolymer acrylic resin, copolymer acrylic resin, polyisocyanate resin or amino resin, or a combination of at least two of them.

14. The in-mold label film according to claim 12, It is characterized in that The inorganic substance includes any one of calcium carbonate, titanium dioxide, talc, barium sulfate or kaolin, or a combination of at least two of them.

15. The in-mold label film according to claim 12, It is characterized in that The mesh size of the inorganic powder is 100-3000 meshes.

16. The in-mold label film according to claim 12, It is characterized in that The raw materials for preparing the paper-like coating include, by weight, 50-90 parts of homopolymer or copolymer acrylic resin, 0-20 parts of polyisocyanate resin, 0-20 parts of amino resin, and 5-30 parts of inorganic powder.

17. The in-mold label film according to claim 16, It is characterized in that The raw materials for preparing the paper-like coating further include 0-5 parts of auxiliary agents by weight.

18. The in-mold label film according to claim 17, It is characterized in that The auxiliary agent includes any one of a dispersant, a leveling agent or an anti-settling agent, or a combination of at least two of them.

19. The in-mold label film according to claim 1, It is characterized in that The thickness of the adhesive layer is 15-25 μm.

20. The in-mold label film according to claim 1, It is characterized in that The raw materials for preparing the bonding layer include 98-100 parts of resin and 0-2 parts of antistatic agent.

21. The in-mold label film according to claim 20, It is characterized in that The resin includes any one of low-density polyethylene resin, high-density polyethylene resin, copolymerized polypropylene resin, homopolypropylene resin, ethylene acrylic acid copolymerized resin, ethylene methyl acrylate copolymerized resin, ethylene ethyl acrylate copolymerized resin, and ethylene butyl acrylate copolymerized resin, or a combination of at least two thereof.

22. The in-mold label film according to claim 21, It is characterized in that The raw materials for preparing the adhesive layer include 50-100 parts of high-density or low-density polyethylene resin, 0-50 parts of homopolymer or copolymer polypropylene resin, 0-50 parts of ethylene acrylic acid copolymer resin, and 0-50 parts of ethylene acrylate copolymer resin in parts by weight.

23. The in-mold label film according to claim 20, It is characterized in that The antistatic agent includes any one of ethoxylated fatty alkyl amines, ethoxylated alkyl acid amines, ethoxylated lauryl amide, glycerol stearate, alkali metal alkyl sulfonates, alkali metal phosphates, or alkali metal dithiocarbamates, or a combination of at least two thereof.

24. The in-mold label film according to claim 23, It is characterized in that The antistatic agent is ethoxylated aliphatic alkylamine and / or ethoxylated alkyl acid amine.

25. The in-mold label film according to claim 1, It is characterized in that The adhesive layer has an exhaust structure, and the exhaust structure is a diamond-shaped, rectangular or hexagonal air guide groove.

26. The in-mold label film according to claim 25, It is characterized in that The depth of the air guide groove is 5-15 μm.

27. The in-mold label film according to claim 1, It is characterized in that The in-mold label film further comprises an adhesive layer and an aluminum-plated or silver-plated transfer layer stacked in sequence, and the adhesive layer is connected to the paper-like coating layer.

28. The in-mold label film according to claim 27, It is characterized in that The aluminum-plated transfer layer includes a transfer layer of an aluminum-plated transfer film or an aluminum-plated laser transfer film.

29. The in-mold label film according to claim 27, It is characterized in that The silver-plated transfer layer includes a transfer layer of a silver-plated transfer film or a silver-plated laser transfer film.

30. The in-mold label film according to claim 29, It is characterized in that The thickness of the aluminum-plated or silver-plated transfer layer is 30-300 nm.

31. The in-mold label film according to claim 27, It is characterized in that The thickness of the adhesive layer is 1-3 μm.

32. The in-mold label film according to claim 27, It is characterized in that The adhesive includes acrylic adhesive, polyurethane adhesive or epoxy adhesive.

33. A method for preparing an in-mold label film according to any one of claims 1 to 32, It is characterized in that The preparation method comprises: preparing a paper-like coating paint and an adhesive layer paint by mixing raw material formulas, coating the paper-like coating paint and the adhesive layer paint on the outer surface and the inner surface of the base layer respectively, and curing them to obtain the in-mold label film.

34. The method for preparing the in-mold label film according to claim 33, It is characterized in that The preparation method of the base layer is: the outer layer, the outer sub-surface layer, the core layer, the inner sub-surface layer and the inner surface layer are mixed according to the raw material formula respectively, and then extruded by co-extrusion, cooled, longitudinally stretched, tempered, transversely stretched, tempered, and corona treated to obtain the base layer.

35. The method for preparing the in-mold label film according to claim 34, It is characterized in that The co-extrusion temperature is 180-330°C.

36. The method for preparing the in-mold label film according to claim 34, It is characterized in that The temperature of the longitudinal stretching is 110-160°C.

37. The method for preparing the in-mold label film according to claim 34, It is characterized in that The temperature of the transverse stretching is 140-190°C.

38. The method for preparing the in-mold label film according to claim 33, It is characterized in that The paper-like coating paint is applied by roller coating.

39. The method for preparing the in-mold label film according to claim 33, It is characterized in that The adhesive layer coating is applied in a casting manner.

40. The method for preparing the in-mold label film according to claim 33, It is characterized in that After the adhesive layer coating is applied, the air guide grooves are cold pressed out using an anilox roller.

41. The method for preparing the in-mold label film according to claim 33, It is characterized in that The curing temperature is 90-150°C.

42. The method for preparing the in-mold label film according to claim 33, It is characterized in that The preparation method further comprises: coating the adhesive layer on the transfer film layer and drying it, laminating it with the imitation paper coating in the in-mold label film, peeling off the polyester film, and aging.