Magnetic matrix containing metal magnetic particles and electronic component containing the magnetic matrix

By using metallic magnetic particles with different average particle sizes and providing insulating layers of different thicknesses in the magnetic matrix, the problem of uneven magnetic flux distribution is solved, the inductance and allowable current are improved, and the magnetic saturation characteristics of the magnetic matrix are enhanced.

CN110634640BActive Publication Date: 2024-11-12TAIYO YUDEN KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910502192.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-06-21
Filing Date
2019-06-11
Publication Date
2024-11-12
Estimated Expiration
2039-06-11

AI Technical Summary

Technical Problem

The uneven distribution of magnetic flux in existing magnetic substrates leads to problems such as reduced inductance and limited allowable current.

Method used

Metal magnetic particles with different average particle sizes are used, and insulating layers of different thicknesses are provided on their surfaces to form a magnetic matrix, thereby improving the filling rate and uniform magnetic flux distribution of the metal magnetic particles.

Benefits of technology

This achieves a more uniform magnetic flux distribution in the magnetic matrix, improves inductance and allowable current, and enhances the magnetic saturation characteristics of the magnetic matrix.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110634640B_ABST
    Figure CN110634640B_ABST
Patent Text Reader

Abstract

The present invention provides a magnetic molded body having a high filling rate of metal magnetic particles and improved current allowance. A magnetic substrate according to one embodiment of the present invention comprises first metal magnetic particles having a first average particle size and second metal magnetic particles having a second average particle size smaller than the first average particle size. In this embodiment, a first insulating layer having a first thickness is provided on the surface of the first metal magnetic particles, and a second insulating layer having a second thickness thinner than the first thickness is provided on the surface of the second metal magnetic particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a magnetic matrix containing metal magnetic particles and an electronic component containing the magnetic matrix. Background Art

[0002] Various magnetic materials have been used in electronic components such as inductors. For example, an inductor generally includes a magnetic base made of a magnetic material, a coil conductor embedded in the magnetic base, and an external electrode connected to an end of the coil conductor.

[0003] Ferrite is widely used as a magnetic material for coil components. Ferrite is suitable as a magnetic material for inductors because of its high magnetic permeability.

[0004] As magnetic materials for electronic components other than ferrite, metal magnetic particles are known. An insulating film with low magnetic permeability is provided on the surface of the metal magnetic particles. A magnetic matrix containing metal magnetic particles can be produced by press forming. For example, a magnetic matrix containing metal magnetic particles can be produced by injecting a slurry obtained by kneading metal magnetic particles and a binding material into a mold, and applying pressure to the slurry in the mold.

[0005] In order to improve the magnetic permeability of a magnetic matrix containing metal magnetic particles, the filling rate of the metal magnetic particles of the magnetic matrix can be increased. For a long time, there have been proposals to increase the filling rate of magnetic particles in a magnetic matrix in order to improve the magnetic permeability. For example, in Japanese Patent Publication No. 2006-179621, a composite magnetic material containing a first magnetic particle and a second magnetic particle is disclosed, the average particle size of the second magnetic particle is less than 50% of the average particle size of the first magnetic particle, and when the content of the first magnetic particle is X [wt%] and the content of the second magnetic particle is Y [wt%], the relationship of 0.05≤Y / (X+Y)≤0.30 is satisfied, thereby, a molded body filled with magnetic particles at a high density can be obtained. In addition, in Japanese Patent Publication No. 2010-34102, a clay-like magnetic matrix is ​​disclosed in which two or more amorphous metal magnetic particles with different average particle sizes and an insulating binding material are mixed. According to such a magnetic matrix, a high filling rate and low iron loss can be achieved.

[0006] It is disclosed in Japanese Patent Gazette No. 2015-026812 that the first metal magnetic particles and the second metal magnetic particles contained in the magnetic matrix are made of amorphous metal containing iron (Fe), the first magnetic particles are coarse powders with a long axis length of more than 15 μm, and the second magnetic particles are fine powders with a long axis length of less than 5 μm, thereby improving the filling rate of the metal magnetic particles.

[0007] Japanese Patent Application Laid-Open No. 2016-208002 discloses that the filling rate of magnetic particles can be increased by causing a magnetic body to contain magnetic particles having three or more types of particle size distributions.

[0008]

Prior technical literature

[0009] [Patent Literature]

[0010] [Patent Document 1] Japanese Patent Application Publication No. 2006-179621

[0011] [Patent Document 2] Japanese Patent Application Publication No. 2010-034102

[0012] [Patent Document 3] Japanese Patent Application Publication No. 2015-026812

[0013] [Patent Document 4] Japanese Patent Application Publication No. 2016-208002

[0014] In a magnetic matrix containing a plurality of metal magnetic particles with different average particle sizes, since the magnetic permeability of the metal magnetic particles with a larger average particle size is higher than that of the metal particles with a smaller average particle size, the magnetic flux easily passes through the path with a high existence ratio of the metal magnetic particles with a larger average particle size. Therefore, in a coil component provided with a coil conductor in such a magnetic matrix, if the DC current flowing through the coil conductor increases, magnetic saturation occurs in sequence in the numerous magnetic paths of the magnetic flux passing through the magnetic matrix, starting from the magnetic path with a high existence ratio of the metal magnetic particles with a large average particle size. In this way, in the existing magnetic matrix, there are paths where magnetic saturation is easy to occur and paths where it is difficult to occur. Therefore, if the DC current flowing through the coil conductor increases, magnetic saturation occurs in sequence and in stages in the multiple magnetic flux paths, starting from the path where magnetic saturation is easy to occur, so the inductance of the coil component gradually decreases. In this way, in a magnetic matrix containing metal magnetic particles, there is a problem of uneven distribution of magnetic flux. In addition, when a magnetic substrate containing metal magnetic particles is used for a coil component, the inductance decreases slowly due to the unevenness of the magnetic flux distribution. Therefore, it is difficult to increase the allowable current in a coil component having a magnetic substrate containing metal magnetic particles. Summary of the invention

[0015] The purpose of the present invention is to solve or alleviate at least part of the above problems. One of the more specific purposes of the present invention is to provide a magnetic molded body having a high filling rate of metal magnetic particles and allowing improved current flow. Other purposes of the present invention are explained through the description of the entire specification.

[0016] A magnetic substrate according to an embodiment of the present invention comprises: first metal magnetic particles having a first average particle size, and second metal magnetic particles having a second average particle size smaller than the first average particle size. In this embodiment, a first insulating layer having a first thickness is provided on the surface of the first metal magnetic particles, and a second insulating layer having a second thickness thinner than the first thickness is provided on the surface of the second metal magnetic particles.

[0017] In the magnetic substrate according to one embodiment of the present invention, a ratio of an average particle diameter ratio, which is a ratio of the second average particle diameter to the first average particle diameter, and a thickness ratio, which is a ratio of the second thickness to the first thickness, are within a range of 0.5 to 1.5.

[0018] In the magnetic substrate according to one embodiment of the present invention, both the first metal magnetic particles and the second metal magnetic particles contain Fe, and the Fe content of the second metal magnetic particles is higher than the Fe content of the first metal magnetic particles.

[0019] In the magnetic matrix according to one embodiment of the present invention, both the first metal magnetic particles and the second metal magnetic particles contain Si, and the Si content ratio of the first metal magnetic particles is higher than the Si content ratio of the second metal magnetic particles.

[0020] The magnetic substrate according to one embodiment of the present invention further comprises third metal magnetic particles having a third average particle size smaller than the second average particle size. A third insulating layer may be provided on the surface of the third metal magnetic particles.

[0021] In the magnetic substrate according to one embodiment of the present invention, the third metal magnetic particles contain at least one of Ni and Co.

[0022] In the magnetic substrate according to one embodiment of the present invention, at least one of the first insulating layer, the second insulating layer, and the third insulating layer contains Si.

[0023] In the magnetic substrate according to one embodiment of the present invention, the first metal magnetic particles contain Fe, and the first insulating layer contains Fe oxide.

[0024] The magnetic substrate according to one embodiment of the present invention further includes a binder.

[0025] One embodiment of the present invention relates to an electronic component. The electronic component includes the above-mentioned magnetic substrate.

[0026] An electronic component according to one embodiment of the present invention includes the magnetic base described above and a coil provided in the magnetic base.

[0027] According to the disclosure of this specification, it is possible to provide a magnetic molded body having a high filling rate of metal magnetic particles and improved current allowance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a perspective view of a coil component according to one embodiment of the present invention.

[0029] Figure 2 It is a schematic representation of the I-I line cut Figure 1 A cross-sectional view of a coil component.

[0030] Figure 3 Is magnification Figure 2 A diagram schematically showing area A of a magnetic entity.

[0031] Figure 4a It is schematically indicated Figure 2 A cross-sectional view of a first metal magnetic particle included in a magnetic entity.

[0032] Figure 4b It is schematically indicated Figure 2 A cross-sectional view of a second metal magnetic particle included in a magnetic entity.

[0033] Figure 5a Yes means Figure 2 A graph showing the volume-based particle size distribution of metal magnetic particles contained in a magnetic entity.

[0034] Figure 5b Yes means Figure 2 A graph showing the volume-based particle size distribution of metal magnetic particles contained in a magnetic entity.

[0035] Figure 6 This is a diagram schematically showing the current-inductance characteristics of a magnetic body according to one embodiment of the present invention.

[0036] Figure 7 This is a diagram schematically showing an enlarged region A of a magnetic entity according to another embodiment of the present invention.

[0037] Figure 8 It is schematically indicated Figure 7 A cross-sectional view of a third metal magnetic particle included in a magnetic entity.

[0038] Fig. 9 This is a perspective view of a coil component according to another embodiment of the present invention.

[0039] Fig.10 It is a rough representation Fig. 9 A cross-sectional view of a cross section of a coil component.

[0040] Explanation of symbols

[0041] 10,110 Coil parts

[0042] 20,120 Magnetic base

[0043] 25, 125 coil conductor

[0044] 31. The first metal magnetic particle

[0045] 32 Second metal magnetic particle

[0046] 33 Third Metal Magnetic Particles

[0047] 41 First insulation layer

[0048] 42 Second insulation layer

[0049] 43 Third insulation layer DETAILED DESCRIPTION

[0050] Hereinafter, various embodiments of the present invention will be described with reference to the accompanying drawings as appropriate. In addition, in a plurality of drawings, the same reference numerals are attached to common components in the plurality of drawings. It should be noted that the drawings may not be described in exact scale for the sake of convenience.

[0051] Reference Figure 1 and Figure 2 , a coil component 10 according to an embodiment of the present invention will be described. Figure 1 is a perspective view of a coil component 1 according to an embodiment of the present invention. Figure 2 It schematically shows that the I-I line is cut off. Figure 1 FIG. 1 is a cross-sectional view of the coil component 1. Figure 1 , the internal structure of the coil component 10 is shown by partially showing the components of the coil component.

[0052] The present invention can be applied to various coil components. The present invention can be applied to, for example, inductors, filters, reactors, and various other coil components and other electronic components. The present invention is more effective by being applied to coil components and other electronic components to which large currents are applied. An inductor used in a DC-DC converter is an example of a coil component to which large currents can be applied. Figure 1 and Figure 2 , a magnetic coupling type inductor used in a DC-DC converter is shown as an example of a coil component 10 to which the present invention is applicable. The present invention is applicable to various magnetic coupling type coil components other than magnetic coupling type inductors, such as transformers, common mode choke coils, coupled inductors, and others.

[0053] As shown in the figure, the coil component 10 of one embodiment of the present invention includes a magnetic base 20, a coil conductor 25 provided in the magnetic base 20, an insulating substrate 50, and four external electrodes 21 to 24. The coil conductor 25 includes a coil conductor 25a formed on the upper surface of the insulating substrate 50 and a coil conductor 25b formed on the lower surface of the insulating substrate 50.

[0054] The external electrode 21 is electrically connected to one end of the coil conductor 25a, and the external electrode 22 is electrically connected to the other end of the coil conductor 25a. The external electrode 23 is electrically connected to one end of the coil conductor 25b, and the external electrode 24 is electrically connected to the other end of the coil conductor 25b.

[0055] In this specification, unless otherwise explained in the text, the "length" direction, "width" direction and "thickness" direction of the coil component 10 are respectively Figure 1 When referring to the up and down direction of the coil component 10, Figure 1 The up and down direction is used as the reference.

[0056] In one embodiment of the present invention, the coil component 10 is formed to have a length dimension (dimension in the L direction) of 1.0 mm to 2.6 mm, a width dimension (dimension in the W direction) of 0.5 mm to 2.1 mm, and a height dimension (dimension in the H direction) of 0.5 mm to 1.0 mm.

[0057] The insulating substrate 50 is a member formed of a magnetic material in a plate shape. The magnetic material used for the insulating substrate 50 is, for example, a composite magnetic material containing a binder and filler particles. The binder is, for example, a thermosetting resin with excellent insulation properties, such as an epoxy resin, a polyimide resin, a polystyrene (PS) resin, a high-density polyethylene (HDPE) resin, a polyoxymethylene (POM) resin, a polycarbonate (PC) resin, a polyvinylidene fluoride (PVDF) resin, a phenolic resin, a polytetrafluoroethylene (PTFE) resin, or a polyparaphenylene benzobisoxazole (PBO) resin.

[0058] In one embodiment of the present invention, the filler particles contained in the insulating substrate 50 are ferrite particles, metal magnetic particles, SiO 2 and Al 2 O 3 Inorganic material particles such as ferrite particles, glass particles, or any other known filler particles. Ferrite material particles that can be applied to the present invention are, for example, Ni—Zn ferrite particles or Ni—Zn—Cu ferrite particles.

[0059] In one embodiment of the present invention, the insulating substrate 50 is configured to have a greater resistance value than the magnetic base 20. Thus, even if the insulating substrate 50 is thinned, electrical insulation between the coil conductor 25a and the coil conductor 25b can be ensured.

[0060] The coil conductor 25a is formed to have a predetermined pattern on the upper surface of the insulating substrate 50. In the illustrated embodiment, the coil conductor 25a is formed to have a surrounding portion wound a plurality of turns around the coil axis CL.

[0061] Similarly, the coil conductor 25b is formed to have a predetermined pattern on the lower surface of the insulating substrate 50. In the illustrated embodiment, the coil conductor 25b is formed to have a surrounding portion wound around the coil axis CL with multiple turns. In one embodiment of the present invention, the coil conductor 25b is formed so that the upper surface of the surrounding portion is opposite to the lower surface of the surrounding portion of the coil conductor 25a.

[0062] A lead conductor 26a is provided at one end of the coil conductor 25a, and a lead conductor 27a is provided at the other end. The coil conductor 25a is electrically connected to the external electrode 21 via the lead conductor 26a, and is electrically connected to the external electrode 22 via the lead conductor 27a. Similarly, a lead conductor 26b is provided at one end of the coil conductor 25b, and a lead conductor 27b is provided at the other end. The coil conductor 25b is electrically connected to the external electrode 23 via the lead conductor 26b, and is electrically connected to the external electrode 24 via the lead conductor 27b.

[0063] In one embodiment, the coil conductor 25 a and the coil conductor 25 b are formed by forming a patterned resist on the surface of the insulating substrate 50 and filling the openings of the resist with a conductive metal by plating.

[0064] In one embodiment of the present invention, the magnetic substrate 20 has a first main surface 20a, a second main surface 20b, a first end surface 20c, a second end surface 20d, a first side surface 20e, and a second side surface 20f. The outer surface of the magnetic substrate 20 is defined by these six surfaces.

[0065] The external electrodes 21 and 23 are provided on the first end surface 20c of the magnetic base 20. The external electrodes 22 and 24 are provided on the second end surface 20d of the magnetic base 20. As shown in the figure, each external electrode extends to the upper surface 20a and the lower surface 20c of the magnetic base 20.

[0066] In one embodiment of the present invention, the magnetic matrix 20 is formed of a composite resin material obtained by mixing a large amount of metal magnetic particles in a binder. In one embodiment of the present invention, the binder contained in the magnetic matrix 20 is a resin, for example, a thermosetting resin with excellent insulation. As the thermosetting resin for the magnetic matrix 20, benzocyclobutene (BCB), epoxy resin, phenolic resin, unsaturated polyester resin, vinyl ester resin, polyimide resin (PI), polyphenylene ether resin (PPO), bismaleimide triazine cyanate resin (bismaleimide triazine cyanate resin), fumarate resin, polybutadiene resin, or polyvinyl benzyl ether resin (polyvinyl benzyl ether resin) can be used.

[0067] As described above, the magnetic matrix 20 contains a large number of metal magnetic particles. The metal magnetic particles contain two or more metal magnetic particles with different average particle sizes. In one embodiment of the present invention, the magnetic matrix 20 contains two metal magnetic particles with different average particle sizes. An enlarged view of the cross section of the magnetic matrix 20 containing two metal magnetic particles with different average particle sizes is shown in FIG. Figure 3 middle. Figure 3 It is to amplify the magnetic entity 20 Figure 2 The figure schematically shows the region A shown. Region A is an arbitrary region within the magnetic entity 20. Figure 3 In the illustrated embodiment, the magnetic matrix 20 includes a plurality of first metal magnetic particles 31 and a plurality of second metal magnetic particles 32 .

[0068] In other embodiments, the magnetic matrix 20 may also contain three types of metal magnetic particles having different average particle sizes. An enlarged view of a cross section of the magnetic matrix 20 containing three types of metal magnetic particles having different average particle sizes is shown in FIG. Figure 7 In. Figure 7 As shown, the magnetic matrix 20 may further contain a plurality of third metal magnetic particles 33 in addition to the plurality of first metal magnetic particles 31 and the plurality of second metal magnetic particles 32 .

[0069] One thing to note is that Figure 3 and Figure 7 The metal magnetic particles shown are not shown in exact size ratios in order to emphasize the differences in average particle sizes. Figure 3 and Figure 7 In the embodiment, the region other than the first metal magnetic particles 31, the second metal magnetic particles 32, and the third metal magnetic particles 33 is filled with a binder. The first metal magnetic particles 31, the second metal magnetic particles 32, and the third metal magnetic particles 33 are bonded to each other by the binder.

[0070] Among the three types of magnetic particles, the first metal magnetic particles 31 have the largest average particle size. The average particle size of the first metal magnetic particles 31 is, for example, 1 μm to 200 μm. The average particle size of the second metal magnetic particles 32 is smaller than that of the first metal magnetic particles 31 .

[0071] In one embodiment, the average particle size of the second metal magnetic particles 32 is less than 1 / 10 of the average particle size of the first metal magnetic particles 31. The average particle size of the second metal magnetic particles 32 is, for example, 0.1 μm to 20 μm. When the average particle size of the second metal magnetic particles 32 is less than 1 / 10 of the average particle size of the first metal magnetic particles 31, the second metal magnetic particles 32 easily enter between adjacent first metal magnetic particles 31, and as a result, the filling rate (density) of the metal magnetic particles of the magnetic matrix 20 can be increased.

[0072] In one embodiment, the average particle size of the third metal magnetic particles 33 is smaller than the average particle size of the second metal magnetic particles 32. In one embodiment, the average particle size of the third metal magnetic particles 33 is less than 2 μm. The average particle size of the third metal magnetic particles 33 may also be less than 0.5 μm. Thus, even when the coil component is excited at a high frequency, the occurrence of eddy currents in the third metal magnetic particles 33 can be suppressed. Thus, a coil component 10 having excellent high-frequency characteristics can be obtained.

[0073] The average particle size of the first metal magnetic particles 31 is larger than the average particle size of the second metal magnetic particles 32. In addition, the average particle size of the second metal magnetic particles 32 is larger than the average particle size of the third metal magnetic particles 33. Therefore, as needed, the first metal magnetic particles 31 are called large particles, the second metal magnetic particles 32 are called medium particles, and the third metal magnetic particles 33 are called small particles.

[0074] The average particle size of the metal magnetic particles contained in the magnetic matrix 20 is determined by cutting the magnetic matrix along its thickness direction (T direction) to expose the cross section, photographing the cross section at a magnification of 1000 to 2000 times using a scanning electron microscope (SEM), obtaining a particle size distribution based on the photographed photograph, and determining based on the particle size distribution. For example, the 50% value of the particle size distribution obtained based on the SEM photograph can be used as the average particle size of the metal magnetic particles.

[0075] When the magnetic substrate 20 includes two kinds of metal magnetic particles having different average particle sizes, the particle size distribution obtained based on the SEM photograph is as described below. Figure 5a or Figure 5b Shape shown. Figure 5a and Figure 5b: is a diagram showing an example of the particle size distribution of the first metal magnetic particles 31 and the second metal magnetic particles 32 contained in the magnetic matrix 20. As shown in the figure, the particle size distribution diagram includes two peaks, namely, the first peak P1 and the second peak P2. The particle size distribution containing the first peak P1 represents the particle size distribution of the first metal magnetic particles 31, and the particle size distribution containing the second peak P2 represents the particle size distribution of the second metal magnetic particles 32. The magnetic matrix 20 of one embodiment is obtained by mixing the first metal magnetic particles 31 and the second metal magnetic particles 32 at a predetermined ratio. Figure 5a or Figure 5b , represents the particle size distribution of the two mixed magnetic particles. In one embodiment of the present invention, Figure 5a As shown in FIG. 1 , the particle size distribution of the first magnetic particles 31 is completely non-repetitive or almost non-repetitive with the particle size distribution of the second metal magnetic particles 32. In one embodiment of the present invention, Figure 5b As shown, the particle size distribution of the first magnetic particles 31 may overlap with the particle size distribution of the second metal magnetic particles 32. For example, the particle size distributions of the two may overlap in such a way that the 5% value of the particle size distribution of the first metal magnetic particles 31 is equal to or greater than the 95% value of the particle size distribution of the second magnetic particles 32. Based on such a particle size distribution, the average particle size of the two (or more than three) metal magnetic particles contained in the actually manufactured magnetic matrix can be obtained.

[0076] When the magnetic matrix 20 further includes the third metal magnetic particles 33, the third peak of the particle size distribution of the third metal magnetic particles 33 appears. The particle size distribution of the second magnetic particles 32 and the particle size distribution of the third metal magnetic particles 33 may or may not overlap.

[0077] As described above, by mixing two or more metal magnetic particles having different average particle sizes, the filling rate of the metal magnetic particles in the magnetic substrate 20 can be increased. In one embodiment of the present invention, the filling rate of the metal magnetic particles in the magnetic substrate is 87% or more. Thus, a magnetic substrate having excellent magnetic permeability can be obtained.

[0078] In this specification, the average particle diameter of the first metal magnetic particles 31 is referred to as a first average particle diameter, the average particle diameter of the second metal magnetic particles 32 is referred to as a second average particle diameter, and the average particle diameter of the third metal magnetic particles 33 is referred to as a third average particle diameter.

[0079] In one embodiment, the first metal magnetic particles 31, the second metal magnetic particles 32, and the third metal magnetic particles 33 may be spherical or flat. The magnetic substrate 20 may include four or more metal magnetic particles having different average particle sizes.

[0080] like Figure 4a As shown, a first insulating layer 41 is provided on the surface of the first metal magnetic particle 31. The first insulating layer 41 is preferably formed in such a manner as to cover the entire surface of the first metal magnetic particle 31 so that the first metal magnetic particle 31 does not short-circuit with other metal magnetic particles. The first insulating layer 41 may not cover the entire surface of the first metal magnetic particle 31 but only a portion thereof. During the manufacturing process of the coil component 1, a portion of the first insulating layer 41 may fall off from the first metal magnetic particle 31. In this case, the first insulating layer 41 does not cover the entire surface of the first metal magnetic particle 31 but only a portion thereof.

[0081] like Figure 4b As shown, a second insulating layer 42 is provided on the surface of the second metal magnetic particle 32. The second insulating layer 42 covers the entire or a portion of the surface of the second metal magnetic particle 32.

[0082] like Figure 8 As shown, a third insulating layer 43 is provided on the surface of the third metal magnetic particle 33. The third insulating layer 43 covers the entire or a portion of the surface of the third metal magnetic particle 33. The third insulating layer 43 may be omitted depending on the insulating properties required of the magnetic substrate 20.

[0083] In one embodiment of the present invention, the first metal magnetic particles 31, the second metal magnetic particles 32, and the third metal magnetic particles 33 are formed of a crystalline or amorphous metal or alloy containing at least one element of iron (Fe), nickel (Ni), and cobalt (Co). The first metal magnetic particles 31, the second metal magnetic particles 32, and the third metal magnetic particles 33 may also contain at least one element of silicon (Si), chromium (Cr), and aluminum (Al). The first metal magnetic particles 31, the second metal magnetic particles 32, and the third metal magnetic particles 33 may also be particles of pure iron composed of Fe and inevitable impurities. The first metal magnetic particles 31, the second metal magnetic particles 32, and the third metal magnetic particles 33 may also be Fe-based amorphous alloys containing iron (Fe). The Fe-based amorphous alloys include, for example, Fe-Si, Fe-Si-Al, Fe-Si-Cr-B, Fe-Si-B-C, and Fe-Si-P-B-C. The first metal magnetic particles 31 may also contain particles of only a single type of metal or a single type of alloy. For example, the first metal magnetic particle 31 may be a particle entirely composed of pure iron or a specific type of Fe-based amorphous alloy. This also applies to the second metal magnetic particle 32 and the third metal magnetic particle 33. The first metal magnetic particle 31 may also contain particles of multiple different types of metals or alloys. For example, the first metal magnetic particle 31 may also include multiple particles of the first metal magnetic particle 31 composed of pure iron, and multiple particles of the first metal magnetic particle 31 composed of Fe-Si. This also applies to the second metal magnetic particle 32 and the third metal magnetic particle 33.

[0084] In one embodiment, both the first metal magnetic particles 31 and the second metal magnetic particles contain Fe, and the content ratio of Fe in the second metal magnetic particles 32 is higher than the content ratio of Fe in the first metal magnetic particles 31 .

[0085] As described above, in one embodiment, the first metal magnetic particle 31 and the second metal magnetic particle 32 may also be formed of pure iron or an alloy containing Fe. In this case, the first metal magnetic particle 31 and the second metal magnetic particle 32 may also be formed in the following manner, that is, the Fe content ratio of the second metal magnetic particle 32 is higher than the Fe content ratio of the first metal magnetic particle 31. For example, the first metal magnetic particle 31 contains 72wt% to 80wt% of Fe, and the second metal magnetic particle 32 contains 87wt% to 99.8wt% of Fe. The third metal magnetic particle 33 may, for example, also contain 50wt% to 93wt% of Fe. The Fe content ratio of the second metal magnetic particle 32 and the third metal magnetic particle 33 may also be 92wt% or more.

[0086] As described above, the first metal magnetic particles 31, the second metal magnetic particles 32, and the third metal magnetic particles 33 may all contain Si. In one embodiment, the first metal magnetic particles 31 and the second metal magnetic particles 32 are formed so that the Si content ratio of the first metal magnetic particles 31 is higher than the Si content ratio of the second metal magnetic particles 32. In one embodiment, the second metal magnetic particles 32 and the third metal magnetic particles 33 are formed so that the Si content ratio of the second metal magnetic particles 32 is higher than the Si content ratio of the third metal magnetic particles 33.

[0087] As described above, the first metal magnetic particles 31, the second metal magnetic particles 32, and the third metal magnetic particles 33 may all contain at least one of Ni and Co. In one embodiment, the first metal magnetic particles 31 and the second metal magnetic particles 32 are formed so that the Ni content ratio of the second metal magnetic particles 32 is higher than the Ni content ratio of the first metal magnetic particles 31. In one embodiment, the first metal magnetic particles 31 and the second metal magnetic particles 32 are formed so that the Co content ratio of the second metal magnetic particles 32 is higher than the Co content ratio of the first metal magnetic particles 31. In one embodiment, the second metal magnetic particles 32 and the third metal magnetic particles 33 are formed so that the Ni content ratio of the third metal magnetic particles 33 is higher than the Ni content ratio of the second metal magnetic particles 32. In one embodiment, the second metal magnetic particles 32 and the third metal magnetic particles 33 are formed so that the Co content ratio of the third metal magnetic particles 33 is higher than the Co content ratio of the second metal magnetic particles 32.

[0088] Next, the first insulating layer 41, the second insulating layer 42, and the third insulating layer 43 are described. The first insulating layer 41, the second insulating layer 42, and the third insulating layer 43 are formed of an organic material or an inorganic material. As the material of the first insulating layer 41, the second insulating layer 42, and the third insulating layer 43, a non-magnetic material or a magnetic material having a lower magnetic permeability than the first metal magnetic particles 31, the second metal magnetic particles 32, and the third metal magnetic particles 33 can be used.

[0089] As the organic material for the first insulating layer 41, the second insulating layer 42, and the third insulating layer 43, epoxy, phenolic, silicone, polyimide or other thermosetting resins can be used. When silicone is used as the organic material for the first insulating layer 41, the first metal magnetic particle 31 is put into a silicone resin solution in which the silicone resin is dissolved in a petroleum-based organic solvent such as xylene, and then the organic solvent is evaporated from the silicone resin solution to form the first insulating layer 41 composed of silicone on the surface of the first metal magnetic particle 31. In order to improve the uniformity of the film thickness, the silicone resin solution can also be stirred as needed. The second insulating layer 42 and the third insulating layer 43 can also be formed in the same way as the first insulating layer 41.

[0090] As the inorganic material for the first insulating layer 41, the second insulating layer 42, and the third insulating layer 43, phosphate, borate, chromate, glass (for example, SiO 2 ), and metal oxides (e.g., Fe 2 O 3 or Al 2 O 3 ).

[0091] The first insulating layer 41 , the second insulating layer 42 , and the third insulating layer 43 can be formed by a powder mixing method, a dipping method, a sol-gel method, a CVD method, a PVD method, or various well-known methods other than those described above.

[0092] SiO 2 The layer can be formed on the surface of the metal magnetic particles by, for example, a coating process using a sol-gel method. Specifically, first, a mixture containing TEOS (tetraethoxysilane, Si (OC 2 H 5 ) 4 ), ethanol and water to prepare a mixed solution, and then, after stirring the mixed solution, filtering to separate the SiO 2 The insulating layer is made of metal magnetic particles.

[0093] When the first insulating layer 41, the second insulating layer 42, and the third insulating layer 43 are composed of glass or metal oxide, the first metal magnetic particles 31, the second metal magnetic particles 32, and the third metal magnetic particles 33 provided with these insulating layers may be heat treated. The heat treatment may be performed in an air atmosphere, in a vacuum atmosphere, or in an inert gas atmosphere. As an inert gas, a rare gas such as nitrogen, helium, or argon may be used. The heating temperature is, for example, 400°C to 850°C, or 500°C to 750°C. The heat treatment may reduce the stress strain of the first metal magnetic particles 31, the second metal magnetic particles 32, and the third metal magnetic particles 33. For example, when the heating temperature is 650°C or less, the heating is performed for more than 60 minutes. When the heating temperature is higher than 650°C, the heating time is a time shorter than 60 minutes. By heat treating at this heating temperature and heating time, the desired volume resistivity can be achieved in the first insulating layer 41, the second insulating layer 42, and the third insulating layer 43. The volume efficiency of the first insulating layer 41, the second insulating layer 42, and the third insulating layer 43 is, for example, 10 6 Ω·cm or more. In addition, by performing heat treatment at the above-mentioned heating temperature and heating time, the occurrence of excessive oxidation reaction of the first metal magnetic particles 31, the second metal magnetic particles 32, and the third metal magnetic particles 33 can be suppressed. Thus, the reduction in the magnetic permeability of the first metal magnetic particles 31, the second metal magnetic particles 32, and the third metal magnetic particles 33 can be prevented or suppressed by the heat treatment. The above-mentioned heat treatment method and heating temperature are not restrictive.

[0094] The thickness of the first insulating layer 41, the second insulating layer 42, and the third insulating layer 43 formed of an organic material may be 1 μm to 50 μm, or 10 to 30 μm, respectively. The thickness of the first insulating layer 41, the second insulating layer 42, and the third insulating layer 43 formed of an inorganic material may be 1 nm to 500 nm, 1 nm to 100 nm, 1 nm to 50 nm, or 1 nm to 20 nm, respectively. The insulating layer having a film thickness of 1 nm to 50 nm or 1 nm to 20 nm can be realized by a sol-gel method.

[0095] The thickness of the insulating layer provided on the metal magnetic particles contained in the actually produced magnetic matrix can be measured by cutting the magnetic matrix along its thickness direction (T direction) to expose the cross section, photographing the cross section with a scanning electron microscope (SEM) at a magnification of 50,000 to 100,000 times, and measuring based on the photographed photograph. For example, the thickness of the insulating layer provided on a metal magnetic particle contained in the SEM photograph can be as follows: an imaginary straight line connecting the geometric center of gravity of the metal magnetic particle in the SEM photograph and the geometric center of gravity of another metal magnetic particle adjacent to the metal magnetic particle, and the size of the insulating layer along the direction of this imaginary straight line. The thickness of the insulating layer provided on the metal magnetic particle contained in the SEM photograph can also be as follows: an imaginary line extending from the geometric center of gravity of the metal magnetic particle in the SEM photograph toward the up and down direction of the SEM photograph, and the size of the insulating layer along this imaginary line. At this time, since the dimensions at the upper side and the dimensions at the lower side relative to the center of gravity are measured, the average of the dimensions can be used as the thickness of the insulating layer of the metal magnetic particle. When there are multiple first metal magnetic particles in the SEM photograph, the thickness of the insulating layer can be calculated for each of the multiple metal magnetic particles, and the average value can be used as the thickness of the insulating layer provided on the first metal magnetic particle in the magnetic matrix.

[0096] The materials for the first insulating layer 41, the second insulating layer 42, and the third insulating layer 43 are selected according to the insulation required in the magnetic substrate 20. A plurality of materials may be used as the materials for the first insulating layer 41, the second insulating layer 42, and the third insulating layer 43. The first insulating layer 41, the second insulating layer 42, and the third insulating layer 43 may be two or more layers made of different materials.

[0097] The second insulating layer 42 is formed thinner than the first insulating layer 41. The thickness of the second insulating layer 42 is, for example, 1 / 10 or less of the thickness of the first insulating layer 41. The third insulating layer 43 is formed thinner than the first insulating layer 42. The thickness of the third insulating layer 43 is, for example, 1 / 10 or less of the thickness of the second insulating layer 42.

[0098] In this specification, the thickness of the first insulating layer 41 is referred to as a first thickness, the thickness of the second insulating layer 42 is referred to as a second thickness, and the thickness of the third insulating layer 43 is referred to as a third thickness.

[0099] As described later, the magnetic substrate 20 can also be formed by press-molding a composite resin material including the first metal magnetic particles 31, the second metal magnetic particles 32, and the third metal magnetic particles 33 provided with the first insulating layer 41, the second insulating layer 42, and the third insulating layer 43. The insulating layer formed of an inorganic material has a smaller change in film thickness during press molding than the insulating layer formed of an organic material. Therefore, in order to obtain a film thickness within the expected range, it is preferred to use an inorganic material as the material of the first insulating layer 41, the second insulating layer 42, and the third insulating layer 43.

[0100] In one embodiment of the present invention, the ratio of the average particle size ratio to the thickness ratio is in the range of 0.5 to 1.5, wherein the average particle size ratio refers to the ratio of the second average particle size as the average particle size of the second metal magnetic particles 32 to the first average particle size as the average particle size of the first metal magnetic particles 31, and the thickness ratio refers to the ratio of the second thickness as the thickness of the second insulating layer 42 provided on the second metal magnetic particles 32 to the first thickness as the thickness of the first insulating layer 41 provided on the first metal magnetic particles 31. For the convenience of explanation, if Figure 4a Where r1 represents the average particle size of the first metal magnetic particles 31, and t1 represents the first thickness of the first insulating layer 41, Figure 4b In which r2 represents the average particle size of the second metal magnetic particles 32, and t2 represents the second thickness of the second insulating layer 42, the average particle size ratio is represented by r2 / r1, and the thickness ratio is represented by t2 / t1. At this time, the ratio of the average particle size ratio r2 / r1 to the thickness ratio t2 / t1 is r2·t1 / r1·t2. As described above, in one embodiment, because r2 is less than 1 / 10 of r1 and t2 is less than 1 / 10 of t1, if r2 is 1 / 20 of r1 and t2 is 1 / 15 of t1, then at this time, the ratio of the average particle size ratio r2 / r1 to the thickness ratio t2 / t1, that is, r2·t1 / r1·t2 is 0.75.

[0101] Next, an example of a method for manufacturing the coil component 10 is described. First, an insulating substrate formed into a plate shape by a magnetic material is prepared. The insulating substrate is, for example, constructed in the same manner as the above-mentioned insulating substrate 50. Next, a photoresist is applied to the upper surface and the lower surface of the insulating substrate, and then, a conductor pattern is exposed and transferred to the upper surface and the lower surface of the insulating substrate, respectively, and a development process is performed. Thus, a resist having an opening pattern for forming a coil conductor is formed on the upper surface and the lower surface of the insulating substrate, respectively. The conductor pattern formed on the upper surface of the insulating substrate is, for example, a conductor pattern corresponding to the above-mentioned coil conductor 25a, and the conductor pattern formed on the lower surface of the insulating substrate is, for example, a conductor pattern corresponding to the above-mentioned coil conductor 25b.

[0102] Next, the opening patterns are filled with conductive metal by plating. Next, the resist is removed from the insulating substrate by etching, thereby forming coil conductors on the upper surface and the lower surface of the insulating substrate.

[0103] Next, a magnetic matrix is ​​formed on both sides of the insulating substrate on which the coil conductor is formed. The magnetic matrix, for example, corresponds to the aforementioned magnetic matrix 20. The magnetic matrix, for example, is made by sheet molding. Specifically, an insulating substrate on which the coil conductor is formed is arranged in a molding die, and a resin composition (slurry) obtained by mixing three kinds of metal magnetic particles and a thermosetting resin (for example, epoxy resin) is injected into the molding die, and pressure is applied, so that a molded product having a magnetic matrix formed on the insulating substrate can be obtained. Instead of pressurizing the resin composition, or in addition to pressurizing the resin composition, the resin composition can also be heated. These three magnetic particles, for example, are the aforementioned first metal magnetic particles 31, second metal magnetic particles 32, and third metal magnetic particles 33.

[0104] Next, a predetermined number of external electrodes are formed on the molded product having the magnetic base formed on the insulating substrate. The external electrodes correspond to the external electrodes 21 to 24 described above, for example. Each external electrode is formed by applying a conductive paste on the surface of the magnetic base to form a base electrode, and forming a plating layer on the surface of the base electrode. The plating layer is, for example, a double-layer structure of a nickel plating layer containing nickel and a tin plating layer containing tin.

[0105] Through the above steps, the coil component 10 according to one embodiment of the present invention can be obtained. The above-described method for manufacturing the coil component 10 is merely an example, and the method for manufacturing the coil component 10 is not limited to the above-described method.

[0106] Next, refer to Fig. 9 and Fig.10 , a coil component 110 according to another embodiment of the present invention is described. The coil component 110 is an inductor. As shown in the figure, the coil component 110 includes a magnetic substrate 120, a coil conductor 125 embedded in the magnetic substrate 120, an external electrode 121, and an external electrode 122. The coil conductor 125 is configured such that one end thereof is electrically connected to the external electrode 121, and the other end thereof is electrically connected to the external electrode 122.

[0107] The magnetic substrate 120 contains two or more types of metal magnetic particles having different average particle sizes, similar to the magnetic substrate 20. The description of the magnetic substrate 20 in this specification is also applicable to the magnetic substrate 120 unless it contradicts the content of the text.

[0108] Next, the effects of the above-mentioned embodiment are described. In one of the above-mentioned embodiments, the magnetic substrate 20 contains two or more metal magnetic particles (e.g., the first metal magnetic particles 31 and the second metal magnetic particles 32) having different average particle sizes. As a result, the filling rate of the metal magnetic particles in the magnetic substrate 20 can be increased compared to a magnetic substrate containing only one type of metal magnetic particles.

[0109] In the above-mentioned embodiment, the magnetic substrate 20 includes first metal magnetic particles 31 having a first average particle size, and second metal magnetic particles 32 having a second average particle size smaller than the first average particle size. In this embodiment, a first insulating layer 41 having a first thickness is provided on the surface of the first metal magnetic particles, and a second insulating layer 42 having a second thickness thinner than the first thickness is provided on the surface of the second metal magnetic particles. Generally speaking, in a magnetic substrate containing a plurality of metal magnetic particles having different average particle sizes, magnetic flux is more likely to pass through particles having a larger average particle size than particles having a smaller average particle size. Therefore, if an insulating layer having a uniform thickness is formed on the metal magnetic particles regardless of the size of their average particle size, the magnetic flux distribution in the magnetic substrate is non-uniform. Such non-uniform magnetic flux distribution in the magnetic substrate occurs because the metal magnetic particles having a larger average particle size and the metal magnetic particles having a smaller average particle size have an insulating layer having the same thickness, and as a result, the interparticle spacing between the metal magnetic particles having a larger average particle size and the interparticle spacing between the metal magnetic particles having a smaller average particle size are equal in degree. Here, the interparticle spacing between metal magnetic particles can also mean the distance between the outer surfaces of adjacent metal magnetic particles. Therefore, in the magnetic matrix, if the metal magnetic particles form an insulating layer of uniform thickness regardless of the size of their average particle size, magnetic saturation will first occur in the magnetic path passing through the metal magnetic particles with a large average particle size, and magnetic saturation will occur in the magnetic path passing through the metal magnetic particles with a small average particle size in turn. In contrast, in the above-mentioned embodiment, because the first insulating layer 41 formed on the first metal magnetic particle 31 is formed thicker than the second insulating layer 42 formed on the second metal magnetic particle 32, it is possible to suppress the magnetic flux from concentrating on the magnetic path containing the first metal magnetic particle 31. As a result, the magnetic flux distribution in the magnetic matrix can be made more uniform. Therefore, the magnetic saturation characteristics of the magnetic matrix can be improved. When the magnetic matrix is ​​used in a coil component, the allowable current of the coil component can be increased.

[0110] In the above-mentioned embodiment, the ratio of the average particle diameter ratio and the thickness ratio is in the range of 0.5 to 1.5, wherein the average particle diameter ratio refers to the ratio of the second average particle diameter of the second metal magnetic particles 32 to the first average particle diameter of the first metal magnetic particles 31, and the thickness ratio refers to the ratio of the second thickness of the second insulating layer 42 to the first thickness of the first insulating layer 41. According to the above-mentioned embodiment, in the plurality of magnetic paths of the magnetic substrate 20, the ratio of the magnetic path length occupied by the metal magnetic particles with high magnetic permeability (the first metal magnetic particles 31 and the second metal magnetic particles 32) to the magnetic path length occupied by the insulating layers with low magnetic permeability (the first insulating layer 41 and the second insulating layer 32) is in the range of 0.5 to 1.5. Thus, the difference in effective magnetic permeability of each of the plurality of magnetic paths in the magnetic substrate 20 can be reduced. Thus, the magnetic flux distribution of the magnetic substrate 20 can be made more uniform.

[0111] If the filling rate of the metal magnetic particles of the magnetic matrix 20 is low, the proportion of the adhesive material in the magnetic circuit in the magnetic matrix 20 becomes higher. If the area where the adhesive material exists in the magnetic circuit is large relative to the total length of the magnetic circuit, the effective magnetic permeability of each magnetic circuit changes according to the proportion of the adhesive material. Therefore, by increasing the filling rate of the metal magnetic particles of the magnetic matrix 20, the influence of the adhesive material on the effective magnetic permeability of each magnetic circuit can be reduced. As a result, the effect of uniformizing the magnetic flux distribution brought about by adjusting the average particle size of the metal magnetic particles and the film thickness of the insulating layer formed on the metal magnetic particles can be more significantly obtained.

[0112] In one embodiment described above, both the first metal magnetic particle 31 and the second metal magnetic particle 32 contain Fe, and the content ratio of Fe in the second metal magnetic particle 32 is higher than the content ratio of Fe in the first metal magnetic particle 31. The second insulating layer 42 formed on the second metal magnetic particle 32 is thinner than the first insulating layer 41, and is therefore easily destroyed during press molding. If the second insulating layer 42 is destroyed, the second metal magnetic particle 32 covered by the second insulating layer 42 is easily electrically connected to other adjacent metal magnetic particles (the first metal magnetic particle, the second metal magnetic particle, or metal magnetic particles other than the first metal magnetic particle). Because the magnetic flux is more easily concentrated on the two electrically connected metal magnetic particles than before the connection, the destruction of the second insulating layer 42 becomes a factor that makes the magnetic flux distribution uneven. Therefore, by increasing the content ratio of Fe with a high saturation magnetic flux density in the second metal magnetic particle 41, even when the second insulating layer 42 is destroyed, the concentration of the magnetic flux to the second metal particle 42 covered by the second insulating layer 42 can be alleviated.

[0113] In one embodiment described above, both the first metal magnetic particle 31 and the second metal magnetic particle 32 contain Si, and the Si content ratio of the first metal magnetic particle 31 is higher than the Si content ratio of the second metal magnetic particle 32. Since the Si content ratio of the first metal magnetic particle 31 is higher than the Si content ratio of the second metal magnetic particle 32, the first metal magnetic particle 31 is more difficult to deform during press forming, whereas the second metal magnetic particle 32 is more likely to deform during press forming. Accordingly, by pressurizing during the forming of the magnetic body, the second metal magnetic particle can be arranged in a manner to fill the gaps between the first metal magnetic particles. As a result, the filling rate of the metal magnetic particles of the magnetic body can be increased. In addition, since the deformation of the first metal magnetic particle can be suppressed during pressurization, the stress strain inside the first metal magnetic particle can be reduced. By reducing the stress strain of the first metal magnetic particle, the deterioration of the magnetic permeability caused by stress strain can be suppressed in the first metal magnetic particle.

[0114] In one embodiment described above, a third metal magnetic particle having a third average particle size smaller than the second average particle size and having a third insulating layer formed on the surface thereof is further provided. The third metal magnetic particle 33 can further improve the filling rate of the metal magnetic particles of the magnetic matrix 20. In addition, the third metal magnetic particle 33 enters between the first metal magnetic particles 31, between the second metal magnetic particles 32, and between the first metal magnetic particles 31 and the second metal magnetic particles 32, thereby improving the mechanical strength of the magnetic matrix 20. In this way, the third metal magnetic particle 33, because it has a third average particle size smaller than the first metal magnetic particles 31 and the second metal magnetic particles 32, although the influence on the magnetic saturation characteristics of the magnetic matrix 20 is small, it contributes to the improvement of the filling rate of the magnetic matrix 20 and the improvement of the mechanical strength of the magnetic matrix 20.

[0115] In the above-mentioned one embodiment, the magnetic substrate 20 has the third metal magnetic particle 33, and the third metal magnetic particle 33 contains at least one of Ni and Co. In one embodiment, when the third metal magnetic particle 33 contains Fe, the content ratio of Fe in the third metal magnetic particle 33 is lower than the content ratio of Fe in the first magnetic metal particle 31 and the content ratio of Fe in the second metal magnetic particle 32. In another embodiment, the third metal magnetic particle 33 may not contain Fe. In such an embodiment in which the content ratio of Fe in the third metal magnetic particle 33 is low, the third metal magnetic particle 33 is less likely to be oxidized than when the content ratio of Fe in the third metal magnetic particle 33 is high. Thus, the decrease in magnetic permeability due to oxidation can be suppressed in the third metal magnetic particle 33. The smaller the diameter of the metal magnetic particle, the greater the influence of the change in magnetic permeability or other magnetic properties due to oxidation. According to the above-mentioned embodiment, by reducing the content ratio of Fe in the third metal magnetic particle 33 with the smallest diameter among the three metal magnetic particles with different average particle diameters (or making it not contain Fe), the change in magnetic properties caused by oxidation of the third metal magnetic particle 33 with a small diameter can be suppressed.

[0116] In the above-mentioned embodiment, at least one of the first insulating layer 41, the second insulating layer 42, and the third insulating layer 43 contains Si. When the first insulating layer 41, the second insulating layer 42, and the third insulating layer 43 contain Si, the insulating properties of the insulating layer can be improved.

[0117] In the above-mentioned embodiment, the first metal magnetic particle 31 contains Fe, and the first insulating layer 41 contains Fe oxide. This can improve the adhesion between the first metal magnetic particle 31 and the first insulating layer 41, thereby suppressing the occurrence of insulation breakdown caused by the first insulating layer 41 peeling off from the first metal magnetic particle 31.

[0118] The coil component 10 of the above embodiment includes the magnetic base 20 and the coil 25 provided in the magnetic base 20. As a result, the magnetic flux distribution in the magnetic base 20 when the coil 25 is excited is uniform, so that the allowable current of the coil component 10 can be improved.

[0119] The above-mentioned effects described with respect to the magnetic base 20 are also applicable to the magnetic base 120 . In addition, the above-mentioned effects described with respect to the coil component 10 are also applicable to the coil component 110 .

[0120] The size, material and configuration of each component described in this specification are not limited to the contents clearly described in the embodiment, and each component can be deformed in a manner having any size, material and configuration that can be included in the scope of the present invention. In addition, the components not explicitly described in this specification can be added to the embodiment described, and part of the components described in each embodiment can also be omitted.

Claims

1. A magnetic substrate comprising metal magnetic particles, wherein the metal magnetic particles include: first metal magnetic particles containing Fe and having a first average particle size; second metal magnetic particles containing Fe and having a second average particle size smaller than the first average particle size; third metal magnetic particles having a third average particle size smaller than the second average particle size, A first insulating layer having a first thickness is provided on the surface of the first metal magnetic particle. A second insulating layer having a second thickness thinner than the first thickness is provided on the surface of the second metal magnetic particle, The first insulating layer and the second insulating layer contain Fe oxide, The Fe content ratio in the second metal magnetic particles is higher than the Fe content ratio in the first metal magnetic particles, The first metal magnetic particles contain 72 wt% to 80 wt% of Fe, The second metal magnetic particles contain 87 wt% to 99.8 wt% of Fe, The content ratio of Fe in the third metal magnetic particle is lower than the content ratio of Fe in the first metal magnetic particle and the content ratio of Fe in the second metal magnetic particle. The filling rate of the metal magnetic particles in the magnetic matrix is ​​87% or more.

2. The magnetic substrate according to claim 1, in, The ratio of the second average particle size to the first average particle size, i.e., the average particle size ratio, and the ratio of the second thickness to the first thickness, i.e., the thickness ratio, are in the range of 0.5 to 1.

5. The filling rate of the first metal magnetic particles and the second metal magnetic particles is 87% or more.

3. The magnetic substrate according to claim 1 or claim 2, in, The first metal magnetic particle and the second metal magnetic particle both contain Si, The content ratio of Si in the first metal magnetic particles is higher than the content ratio of Si in the second metal magnetic particles.

4. The magnetic substrate according to claim 1, in, The third metal magnetic particles contain at least one of Ni and Co.

5. The magnetic substrate according to claim 1 or claim 2, in, The first insulating layer contains Si.

6. The magnetic substrate according to claim 1 or claim 2, in, The second insulating layer contains Si.

7. The magnetic substrate according to claim 1 or claim 2, in, The third metal magnetic particle further has a third insulating layer on its surface. The third insulating layer contains Si.

8. The magnetic substrate according to claim 1 or claim 2, in, The first insulating layer and the second insulating layer contain Fe oxide, The Fe oxide comprises Fe 2 O 3 .

9. The magnetic substrate according to claim 1 or claim 2, in, Adhesive material is also provided.

10. An electronic component, in, A magnetic substrate comprising the magnetic substrate according to any one of claims 1 to 9.

11. An electronic component, in, have: The magnetic substrate according to any one of claims 1 to 9; A coil is arranged in the magnetic substrate.