Nylon 612 abrasive wire with low end group content and preparation method thereof
By using nylon 612 prepolymer with molecular weight of 10000-40000 and specific additives, the filling rate and thermal performance of abrasive wire are improved, and the problem of low service life and effect of abrasive wire under high speed and high pressure is solved, and higher wear resistance is achieved and mechanical properties.
Patent Information
- Application Number
- CN202411092158.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
AI Technical Summary
During dry operation under high speed and high pressure, the existing abrasive wires generate heat due to friction, which leads to softening, wear and breaking of the contact surface, and the service life decreases, and the adhesion of the filler powder to the resin, resulting in surface defects and workpiece yields decrease.
The high-flow nylon 612 prepolymer with a molecular weight of 10,000-40,000 is used as the matrix resin. The filling rate is increased by spinning and rolling, and the molecular weight of the matrix resin is increased by subsequent reaction treatment, combining amine groups, antioxidants, catalysts and molecular weight adjustment. nylon 612 abrasive wire with high filling rate and high thermal performance was prepared.
It improves the filling rate and thermal performance of abrasive wires, extends the service life, reduces wear and fracture phenomena, enhances the wear resistance and mechanical properties of the product, and maintains excellent performance and effect under high speed and high pressure.
Smart Images

Figure BDA0004986883030000091 
Figure BDA0004986883030000151 
Figure BDA0004986883030000171
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of nylon, and in particular to a nylon 612 abrasive wire with a low end group content and a preparation method thereof. Background Art
[0002] Abrasive wires are widely used in industrial production, mainly for polishing, cleaning or grinding of metal, stone, glass and other workpiece surfaces. Generally, abrasive wires are made of thermoplastic resin and wear-resistant powder as raw materials, and are made into monofilaments by melt spinning, and then fixed on a certain form of workpiece to make an abrasive brush or roller. Through high-speed rotation, it is used to remove surface unevenness on the workpiece, improve mirror gloss, remove burrs or chamfers, grind powders, etc.
[0003] The raw materials of abrasive wire mainly include thermoplastic resin and wear-resistant filler. The resin is currently mainly nylon 6 and nylon 612, and the filler is mainly diamond, silicon carbide, and alumina powder. The mesh size of the powder will vary according to the application requirements.
[0004] When the abrasive wire of the prior art is used in dry operation (such as dry grinding or polishing) at high speed and high pressure, the wear rate is sometimes significantly accelerated or the wire breakage phenomenon is significantly increased. Therefore, the replacement frequency of the brush has to be increased, which leads to a significant increase in the cost of use. At the same time, when the dry operation is carried out at high speed and high pressure, the tendency of long strip scratches on the surface of the processed workpiece gradually increases over time, resulting in a decrease in the yield rate of the workpiece.
[0005] The main reason for the above problems is that when dry operation is performed under high speed and high pressure, the abrasive wire will generate heat due to friction, causing the contact surface to generate a high temperature. High temperature will cause the contact part of the abrasive wire to melt and soften. The melting and softening of the abrasive wire will cause the product head to deform, wear, and break, resulting in a decrease in the service life of the product. At the same time, high-temperature melting will also reduce the adhesion between the filler powder and the resin, and the powder will fall off and shift, resulting in defects on the product surface.
[0006] Therefore, a new technology is needed to improve the performance of existing abrasive wire products so that they can maintain excellent performance and effects when performing dry operations under high speed and high pressure. Summary of the invention
[0007] In view of the deficiencies in the prior art, the present application provides a nylon 612 abrasive wire with a low end group content and a preparation method thereof. Specifically, by studying the resin and the preparation process, a specific resin is used to manufacture the abrasive wire. Under the premise of not affecting the product processing, the filling degree of the product is improved, thereby improving the thermal performance and grinding performance of the product.
[0008] In a first aspect, the present application provides a nylon 612 abrasive wire with a low end group content, characterized in that it comprises the following raw materials, measured by weight: 10-90 parts of nylon 612 prepolymer and 10-90 parts of wear-resistant filler; the nylon 612 prepolymer has a molecular weight of 10,000-40,000.
[0009] Preferably, the molecular weight of the nylon 612 prepolymer is 15000-20000.
[0010] The technical principle of this application is as follows: The applicant has found that the main reason why the service life and use effect of traditional abrasive wire products at high temperatures are low is that the existing products have low filling degree, and the resin and filler are not stable enough at high temperatures, resulting in a reduced service life and poor effect. If a higher fluidity resin is used to increase the filling rate, although the effect will increase, it will lead to a further reduction in the stability of the resin and filler, and a further reduction in service life.
[0011] Based on this, the present invention adopts nylon 612 prepolymer with a molecular weight of 10000-40000. The prepolymer is of high fluidity and has a low end group content. It is used as a matrix resin to increase the filling rate of the abrasive wire during spinning and twisting. The molecular weight of the matrix resin is increased to a normal level through subsequent reaction treatment, so that the prepared abrasive wire has a higher filling rate and thermal performance, and can also ensure that the product service life will not decrease due to higher fluidity, thereby obtaining a higher performance nylon 612 abrasive wire.
[0012] Among them, if the molecular weight of the nylon 612 prepolymer is too high, its fluidity will be relatively small, which will increase the difficulty of dispersion with the wear-resistant filler; if the molecular weight of the nylon 612 prepolymer is too small, its fluidity will be relatively large, although it helps the wear-resistant filler to be quickly dispersed therein, but because the density of the wear-resistant filler is relatively large, it will settle in the prepolymer under the action of gravity, and it is difficult to ensure that the wear-resistant filler always maintains a uniform dispersion effect. Therefore, the molecular weight of the nylon 612 prepolymer in this application should not be too large or too small, and 10000-40000 is appropriate, and a molecular weight of 15000-20000 is further preferred.
[0013] Preferably, the terminal group of the nylon 612 prepolymer molecule is an amine group.
[0014] By adopting the above technical solution, the present invention can increase the hydrophilicity of the prepolymer by introducing an amine group, which helps to improve the efficiency of the subsequent polymerization reaction. In addition, the amine group can also serve as a reactive group to participate in further chemical reactions and increase the functionality of the product.
[0015] Preferably, the nylon 612 prepolymer is obtained by condensation polymerization of a prepolymer raw material and water accounting for 5-30% of the mass of the prepolymer raw material. The prepolymer raw material includes 97-100 parts of nylon 612 salt, 0-1 part of antioxidant, 0-1 part of catalyst and 0-1 part of molecular weight regulator in parts by weight.
[0016] By adopting the above technical scheme, in the process of preparing nylon 612, adding an appropriate amount of antioxidant can reduce the oxidation of the prepolymer and ensure the quality and performance of the product; adding an appropriate amount of catalyst can promote the reaction and improve production efficiency; and adding an appropriate amount of molecular weight regulator to control the reaction process, thereby obtaining the prepolymer with the molecular weight distribution required by the present application.
[0017] Preferably, the nylon 612 abrasive wire further comprises maleic anhydride or maleic anhydride olefin copolymer, and the molar ratio of the maleic anhydride or maleic anhydride olefin copolymer to the molecular weight regulator is 1:1.
[0018] By adopting the above technical scheme, maleic anhydride or maleic anhydride olefin copolymer can be used as a reactant to carry out ring-opening polymerization of double bonds in nylon 612 prepolymer. In addition, the excess end groups of nylon 612 prepolymer can be combined, which not only reduces the end group content but also increases the molecular weight, thereby further improving the thermal performance and polishing performance of the product.
[0019] Preferably, the antioxidant in the nylon 612 prepolymer is selected from one or more of antioxidant 1098, antioxidant 1010, antioxidant 168, and antioxidant H10.
[0020] Preferably, the antioxidant in the nylon 612 prepolymer is a compound of antioxidant 1098 and antioxidant 168 in a mass ratio of 1:1.
[0021] By adopting the above technical scheme, it was found through research that the prepolymers obtained by using antioxidant 1098, antioxidant 1010, antioxidant 168, and antioxidant H10 in this application have better performance. Among them, the antioxidant 1098 and antioxidant 168 are compounded in a mass ratio of 1:1 to form an antioxidant, and the corresponding prepolymer effect is better, so it is further preferred.
[0022] Preferably, the catalyst in the nylon 612 prepolymer is selected from one of phosphoric acid, hypophosphorous acid, sodium hypophosphite, potassium hypophosphite and calcium hypophosphite.
[0023] By adopting the above technical solution, the above catalysts all contain phosphate or hypophosphite, which can significantly accelerate the polymerization reaction rate and shorten the polymerization time compared with other catalysts, thereby improving production efficiency; on this basis, it can also reduce the activation energy required for the polymerization reaction, making the reaction easier to carry out, further improving the efficiency and feasibility of the reaction; in addition, the use of the above catalysts is environmentally friendly, and can also increase the toughness and light transmittance of the polymer to a certain extent, and improve its mechanical properties. Phosphoric acid and sodium hypophosphite are more preferred.
[0024] Preferably, the molecular weight regulator in the nylon 612 prepolymer is an amine molecular weight regulator.
[0025] Preferably, the molecular weight regulator in the nylon 612 prepolymer is selected from one of pentamethylenediamine, hexamethylenediamine, nonanediamine and decanediamine.
[0026] By adopting the above technical scheme, the amine molecular weight regulator can effectively control the molecular weight of the prepolymer so that it falls within a specific target range (molecular weight of 10000-40000), which has an important impact on the subsequent polymerization process and the performance of the final product. Secondly, the use of amine molecular weight regulators can also improve the efficiency and selectivity of the polymerization reaction, and it can avoid excessive or insufficient reactions by accurately controlling the molecular weight, thereby optimizing the production process, reducing waste and improving economic benefits. In addition, compared with traditional molecular weight regulators, amine regulators may have better chemical stability and can maintain effective regulation in a wider temperature and pressure range, which makes the preparation process more flexible and easier to control, thereby helping to improve the physical and mechanical properties of the product, and obtaining nylon 612 materials with better performance, meeting the needs of different application scenarios. After research, it was found that the prepolymer performance obtained by the amine molecular weight regulators of pentamethylenediamine, hexamethylenediamine, nonamethylenediamine and decanediamine is more excellent, so it is preferred, and hexamethylenediamine is further preferred.
[0027] In a second aspect, the present application provides a method for preparing nylon 612 abrasive wire, comprising the following steps:
[0028] Mixing: Weigh a set amount of nylon 612 prepolymer, wear-resistant filler and maleic anhydride or maleic anhydride olefin copolymer, and mix them thoroughly to obtain abrasive wire raw materials;
[0029] Forming: The abrasive wire raw materials are sequentially subjected to the processes of melting, spinning, drawing, shaping and viscosity increasing to obtain nylon 612 abrasive wire products.
[0030] By adopting the above technical solution, the nylon 612 prepolymer of the present application is an important intermediate for synthesizing nylon 612. Maleic anhydride or maleic anhydride olefin copolymer as a reactant can undergo addition reaction with the double bonds in the nylon 612 prepolymer by ring-opening polymerization, thereby forming new covalent bonds, increasing the cross-linking density between molecules, and thus improving the heat resistance and other physical properties of the material. Wear-resistant fillers can enhance the mechanical properties of nylon 612 and improve its durability. During the polymerization process, these fillers are usually evenly dispersed between the prepolymers and correspondingly integrated into the molecular structure of nylon 612. The present application first mixes the above three evenly, which is convenient for the operation of subsequent processes. The resulting nylon 612 abrasive wire product has good component uniformity and can effectively exert the performance of the material.
[0031] Preferably, in the mixing step, the abrasive filament raw materials are fully mixed in a high-speed mixer at a stirring speed of 1000 r / min and a mixing time of 5-60 min.
[0032] By adopting the above technical solution, the length of time for mixing nylon 612 prepolymer and wear-resistant filler in a high-speed mixer will affect the performance of the final product. If the mixing time is too long, it may lead to over-mixing, which will reduce the compatibility between the prepolymer and the filler, thereby affecting the final performance of the material and reducing production efficiency. On the other hand, if the mixing time is too short, the filler may not be fully dispersed, which may lead to uneven product quality, which will also lead to performance degradation. After research, it was found that the mixing time can be appropriately adjusted within the range of 5-60 minutes according to the feed amount.
[0033] Preferably, in the mixing step, the wear-resistant filler is one or more of silicon carbide powder, diamond powder, and alumina powder activated by a coupling agent, and the particle size of the powder is 18-3000 mesh.
[0034] By adopting the above technical solution, the powder activated by the coupling agent has good compatibility with the prepolymer, and its particle size can be appropriately adjusted within the range of 18-3000 mesh as needed.
[0035] Preferably, in the forming step, the abrasive filament raw material is placed in an abrasive filament spinning device for processing, and the abrasive filament spinning device includes a twin-screw extruder, a drawing device, a winder and a hot oven connected in sequence, and the twin-screw extruder is provided with a spinneret. The abrasive filament raw material is put into the twin-screw extruder to be heated and melted, and then sequentially passes through the spinneret, the drawing device, the winder and the oven to perform the corresponding processes of spinning, drawing, winding, drying and shaping.
[0036] By adopting the above technical solution, melting, spinning, drawing, winding and drying are integrated into one, reducing the multiple transfers of intermediate materials, which not only helps to improve the production efficiency of the product, but also reduces the possibility of oxidation of the product during the production process.
[0037] Preferably, in the molding step, the twin-screw extruder has an aspect ratio of 44, a rotation speed of 60-200 rpm, and a setting range of different temperature zones of 230-280°C.
[0038] By adopting the above technical solution, the larger the aspect ratio and the slower the rotation speed, the longer the reaction time of the abrasive filament raw material in the twin-screw extruder, the higher the temperature, and the more intense the reaction. In the present application, suitable extrusion parameters can reduce the situation of incomplete reaction or excessive reaction, thereby obtaining a nylon 612 abrasive filament product with excellent performance.
[0039] Preferably, in the forming step, the drawing device is preheated in a boiling water bath, and the drawing ratio is 2-4 times.
[0040] By adopting the above technical solution, the water temperature of the boiling water bath is easy to control, and the drafting ratio is preferably 2-4 times. If the ratio is too small, the obtained nylon 612 abrasive wire product is relatively coarse, and it is difficult to effectively play a role in polishing, cleaning or grinding the surfaces of workpieces such as metals, stones, and glass. If the obtained nylon 612 abrasive wire product is relatively fine, the corresponding polishing, cleaning or grinding force is insufficient.
[0041] Preferably, in the forming step, the temperature of the hot oven is 160-220° C., and the hot baking time is 0.1-100 h.
[0042] By adopting the above technical solution, if the drying temperature is too low and the time is too short, it is difficult to effectively remove the moisture from the product. If the drying temperature is too high and the time is too long, the product will curl and deform, affecting the yield of the product. This application is preferably heated at 160-220°C for 0.1-100h, and its specific parameters can be adjusted within the above range according to the actual drying conditions of the product.
[0043] In summary, this application has the following beneficial effects:
[0044] 1. The present application adopts a high-flowable nylon 612 prepolymer with a molecular weight of 10,000-40,000 as a matrix resin, which can increase the filling rate of the abrasive filament during spinning and twisting, and then increase the molecular weight of the matrix resin to a normal level through subsequent reaction treatment, so that the prepared abrasive filament has both a high filling rate and thermal performance, and can also ensure that the product service life will not decrease due to higher fluidity, thereby obtaining a higher-performance nylon 612 abrasive filament.
[0045] 2. The present application introduces an amine group into the nylon 612 prepolymer molecule, which not only increases the hydrophilicity of the prepolymer and helps to improve the efficiency of the subsequent polymerization reaction, but the amine group can also serve as a reactive group to participate in further chemical reactions and increase the functionality of the product.
[0046] 3. The present application uses specific nylon 612 salt, antioxidant, catalyst and molecular weight regulator, combined with appropriate addition amounts, to effectively obtain the nylon 612 prepolymer with the molecular weight required by the present application, providing a good basis for the preparation of nylon 612 abrasive wire.
[0047] 4. A proper amount of maleic anhydride or maleic anhydride olefin copolymer is added to the nylon 612 abrasive wire of the present application, which not only reduces the end group content but also increases the molecular weight, thereby further improving the thermal performance and grinding performance of the product.
[0048] 5. In the process of preparing nylon 612 abrasive wire, the present application strictly controls the raw materials and process parameters, thereby ensuring that the prepared nylon 612 abrasive wire has good wear resistance and mechanical properties. DETAILED DESCRIPTION
[0049] The following embodiments further illustrate the technical solutions provided by the present invention, but the present invention is not limited to the listed embodiments, and also includes any other known changes within the scope of the present application.
[0050] The main raw material information is shown in Table 1 below:
[0051] Table 1 Main raw material information
[0052]
[0053]
[0054] Preparation Example
[0055] Preparation Example of Nylon 612 Prepolymer 1
[0056] The preparation was carried out according to the following steps: in the prepolymerization stage, 99100g of nylon 612 salt, 300g of antioxidant (150g of antioxidant 1098+150g of antioxidant 168), 300g of phosphoric acid, 300g of hexamethylenediamine and 15000g of ultrapure water were added into the reactor in sequence, and the nitrogen was replaced three times. The temperature was raised to 280°C and maintained for 5h to complete the polymerization reaction of nylon 612 salt; in the pressure relief and melt polycondensation stage, after the ring opening was completed, the pressure in the reactor was relieved to 10kPa at a pressure relief rate of -2kPa / s, and the temperature was reduced to 230°C while the pressure was relieved. The vacuum valve was opened and the vacuum was evacuated to -95KPa. When the torque increased to 17N.m, the material was discharged and pelletized to obtain nylon 612 prepolymer particles. The number average molecular weight tested by GPC was 14890.
[0057] Preparation Example of Nylon 612 Prepolymer 2
[0058] The preparation was carried out according to the following steps: in the prepolymerization stage, 99100g of nylon 612 salt, 300g of antioxidant (150g of antioxidant 1098+150g of antioxidant 168), 300g of phosphoric acid, 300g of hexamethylenediamine and 15000g of ultrapure water were added into the reactor in sequence, and the nitrogen was replaced three times. The temperature was raised to 280°C and maintained for 5h to complete the polymerization reaction of nylon 612 salt; in the pressure relief and melt polycondensation stage, after the ring opening was completed, the pressure in the reactor was relieved to 10kPa at a pressure relief rate of -2kPa / s, and the temperature was reduced to 230°C while the pressure was relieved. The vacuum valve was opened and the vacuum was evacuated to -95KPa. When the torque increased to 24N.m, the material was discharged and pelletized to obtain nylon 612 prepolymer particles. The number average molecular weight tested by GPC was 20130.
[0059] Preparation Example of Nylon 612 Prepolymer 3
[0060] The preparation was carried out according to the following steps: in the prepolymerization stage, 99100g of nylon 612 salt, 300g of antioxidant (150g of antioxidant 1098+150g of antioxidant 168), 300g of phosphoric acid, 300g of hexamethylenediamine and 15000g of ultrapure water were added into the reactor in sequence, and the nitrogen was replaced three times. The temperature was raised to 280°C and maintained for 5h to complete the polymerization reaction of nylon 612 salt; in the pressure relief and melt polycondensation stage, after the ring opening was completed, the pressure in the reactor was relieved to 10kPa at a pressure relief rate of -2kPa / s, and the temperature was reduced to 230°C while the pressure was relieved. The vacuum valve was opened and the vacuum was evacuated to -95KPa. When the torque increased to 30N.m, the material was discharged and pelletized to obtain nylon 612 prepolymer particles. The number average molecular weight tested by GPC was 24669.
[0061] Preparation Example of Nylon 612 Prepolymer 4
[0062] The preparation was carried out according to the following steps: in the prepolymerization stage, 97000g of nylon 612 salt, 1000g of antioxidant (150g of antioxidant 1098+150g of antioxidant 168), 1000g of phosphoric acid, 1000g of hexamethylenediamine and 5000g of ultrapure water were added into the reactor in sequence, and the nitrogen was replaced three times. The temperature was raised to 280°C and maintained for 5h to complete the polymerization reaction of nylon 612 salt; in the pressure relief and melt polycondensation stage, after the ring opening was completed, the pressure in the reactor was relieved to 10kPa at a pressure relief rate of -2kPa / s, and the temperature was reduced to 230°C while the pressure was relieved. The vacuum valve was opened and the vacuum was evacuated to -95KPa. When the torque increased to 24N.m, the material was discharged and pelletized to obtain nylon 612 prepolymer particles. The number average molecular weight tested by GPC was 20210.
[0063] Preparation Example of Nylon 612 Prepolymer 5
[0064] The preparation was carried out according to the following steps: in the prepolymerization stage, 100,000 g of nylon 612 salt and 30,000 g of ultrapure water were added to the reactor in sequence, and the nitrogen was replaced three times. The temperature was heated to 280°C and maintained for 5 hours to complete the polymerization reaction of nylon 612 salt; in the pressure relief and melt polycondensation stage, after the ring opening was completed, the pressure in the reactor was relieved to 10 kPa at a pressure relief rate of -2 kPa / s, and the temperature was reduced to 230°C while the pressure was relieved. The vacuum valve was opened and the vacuum was evacuated to -95 KPa. When the torque increased to 24 N.m, the material was discharged and pelletized to obtain nylon 612 prepolymer particles. The number average molecular weight tested by GPC was 20443.
[0065] Preparation Example of Nylon 612 Prepolymer 6
[0066] The preparation was carried out according to the following steps: in the prepolymerization stage, 99100g of nylon 612 salt, 300g of antioxidant 1098, 300g of phosphoric acid, 300g of hexamethylenediamine and 15000g of ultrapure water were added into the reactor in sequence, and the nitrogen was replaced for 3 times. The temperature was raised to 280°C and maintained for 5h to complete the polymerization reaction of nylon 612 salt; in the pressure relief and melt polycondensation stage, after the ring opening was completed, the pressure in the reactor was relieved to 10kPa at a pressure relief rate of -2kPa / s, and the temperature was reduced to 230°C while the pressure was relieved. The vacuum valve was opened and the vacuum was evacuated to -95KPa. When the torque increased to 24N.m, the material was discharged and pelletized to obtain nylon 612 prepolymer particles. The number average molecular weight tested by GPC was 19523.
[0067] Preparation Example of Nylon 612 Prepolymer 7
[0068] The preparation was carried out according to the following steps: in the prepolymerization stage, 99100g of nylon 612 salt, 300g of antioxidant (150g of antioxidant 1098+150g of antioxidant 168), 300g of hypophosphorous acid, 300g of hexamethylenediamine and 15000g of ultrapure water were added into the reactor in sequence, and the nitrogen was replaced three times. The temperature was raised to 280°C and maintained for 5h to complete the polymerization reaction of nylon 612 salt; in the pressure relief and melt polycondensation stage, after the ring opening was completed, the pressure in the reactor was relieved to 10kPa at a pressure relief rate of -2kPa / s, and the temperature was reduced to 230°C while the pressure was relieved. The vacuum valve was opened and the vacuum was evacuated to -95KPa. When the torque increased to 24N.m, the material was discharged and pelletized to obtain nylon 612 prepolymer particles. The number average molecular weight tested by GPC was 19041.
[0069] Preparation Example of Nylon 612 Prepolymer 8
[0070] The preparation was carried out according to the following steps: in the prepolymerization stage, 99100g of nylon 612 salt, 300g of antioxidant (150g of antioxidant 1098+150g of antioxidant 168), 300g of sodium hypophosphite, 300g of hexamethylenediamine and 15000g of ultrapure water were added into the reactor in sequence, and the nitrogen was replaced for 3 times. The temperature was raised to 280°C and maintained for 5h to complete the polymerization reaction of nylon 612 salt; in the pressure relief and melt polycondensation stage, after the ring opening was completed, the pressure in the reactor was relieved to 10kPa at a pressure relief rate of -2kPa / s, and the temperature was reduced to 230°C while the pressure was relieved. The vacuum valve was opened and the vacuum was evacuated to -95KPa. When the torque increased to 24N.m, the material was discharged and pelletized to obtain nylon 612 prepolymer particles. The number average molecular weight tested by GPC was 19550.
[0071] Preparation Example of Nylon 612 Prepolymer 9
[0072] The preparation was carried out according to the following steps: in the prepolymerization stage, 99100g of nylon 612 salt, 300g of antioxidant (150g of antioxidant 1098+150g of antioxidant 168), 300g of phosphoric acid, 300g of pentamethylenediamine and 15000g of ultrapure water were added into the reactor in sequence, and the nitrogen was replaced for 3 times. The temperature was raised to 280°C and maintained for 5h to complete the polymerization reaction of nylon 612 salt; in the pressure relief and melt polycondensation stage, after the ring opening was completed, the pressure in the reactor was relieved to 10kPa at a pressure relief rate of -2kPa / s, and the temperature was reduced to 230°C while the pressure was relieved. The vacuum valve was opened and the vacuum was evacuated to -95KPa. When the torque increased to 24N.m, the material was discharged and pelletized to obtain nylon 612 prepolymer particles. The number average molecular weight tested by GPC was 19460.
[0073] Preparation Example of Nylon 612 Prepolymer 10
[0074] The preparation was carried out according to the following steps: in the prepolymerization stage, 99100g of nylon 612 salt, 300g of antioxidant (150g of antioxidant 1098+150g of antioxidant 168), 300g of phosphoric acid, 300g of nonanediamine and 15000g of ultrapure water were added into the reactor in sequence, and the nitrogen was replaced for 3 times. The temperature was raised to 280°C and maintained for 5h to complete the polymerization reaction of nylon 612 salt; in the pressure relief and melt polycondensation stage, after the ring opening was completed, the pressure in the reactor was relieved to 10kPa at a pressure relief rate of -2kPa / s, and the temperature was reduced to 230°C while the pressure was relieved. The vacuum valve was opened and the vacuum was evacuated to -95KPa. When the torque increased to 24N.m, the material was discharged and pelletized to obtain nylon 612 prepolymer particles. The number average molecular weight tested by GPC was 19582.
[0075] The present application is further described in detail below in conjunction with embodiments and comparative examples.
[0076] Example
[0077] Example 1
[0078] Example 1a
[0079] This embodiment discloses a method for preparing nylon 612 abrasive wire, comprising the following steps:
[0080] a) Mixing: 9.0 kg of a mixture of nylon 612 prepolymer 1 and maleic anhydride (the molar ratio of maleic anhydride to ethylenediamine in the nylon 612 prepolymer 1 used in this embodiment is 1:1) and 1.0 kg of coupling agent activated silicon carbide are put into a high-speed mixer, stirred at a speed of 1000 r / min, and mixed at high speed for 20 min (adjustable within the range of 5-60 min according to the amount of raw materials added), to obtain abrasive wire raw materials;
[0081] b) abrasive filament spinning: the abrasive filament raw materials are put into a twin-screw extruder with an aspect ratio of 44, the extrusion temperature is set to 250°C, the rotation speed is 200r / min, the extruder melts and shears the abrasive filament raw materials prepared in step a), and then passes through a spinneret, a boiling water bath, and a differential traction roller, and is cooled and shaped to obtain abrasive filaments. The corresponding maximum draft ratios are: the maximum draft ratio of abrasive filament raw material 1 is 4.5 times;
[0082] c) Post-treatment of abrasive filaments: The abrasive filaments in step b) were placed in an oven, and the temperature of the oven was set to 180° C., and heat-treated for 24 hours. After the heat-treatment, nylon 612 abrasive filaments with a molecular weight of 33154 were obtained.
[0083] Examples 1b-1g
[0084] In Examples 1b-1g, based on the method of Example 1a, the amounts of nylon 612 prepolymer a and silicon carbide activated by coupling agent and the maximum draft ratio are adjusted. For specific parameter adjustments, see Table 2 below.
[0085] Example 2
[0086] Examples 2a-2g are based on the methods of Examples 1a-1g, except that nylon 612 prepolymer 1 is replaced by nylon 612 prepolymer 2, and the maximum draft ratio is adjusted accordingly. For specific parameter adjustments, see Table 2 below.
[0087] Example 3
[0088] Examples 3a-3g are based on the methods of Examples 1a-1g, except that nylon 612 prepolymer 1 is replaced by nylon 612 prepolymer 3, and the maximum draft ratio is adjusted accordingly. For specific parameter adjustments, see Table 2 below.
[0089] Comparative Example 1
[0090] This comparative example discloses a method for preparing nylon 612 abrasive wire, comprising the following steps:
[0091] a) Mixing: 7.0 kg of nylon 612 resin with a molecular weight of 42356 and 3.0 kg of coupling agent activated silicon carbide were put into a high-speed mixer and mixed at high speed for 20 minutes to obtain abrasive wire raw materials.
[0092] b) Abrasive filament spinning: the abrasive filament raw material is put into a twin-screw extruder with an aspect ratio of 44, and the extrusion temperature is set to 250°C and the rotation speed is 200r / min. The extruder melts, shears and mixes the abrasive filament raw material obtained in step a), passes through a spinneret, a boiling water bath, and a differential traction roller, and is cooled and shaped to obtain abrasive filaments. The maximum drawing ratio of the abrasive filament raw material is 1.9 times.
[0093] c) Post-treatment of abrasive filaments: The abrasive filaments in step b) are placed in an oven, and the temperature of the oven is set to 180° C., and heat treated for 24 hours. After the heat treatment, nylon 612 abrasive filaments with a molecular weight of 42112 are obtained.
[0094] Performance measurement
[0095] The nylon 612 abrasive wires prepared in the above Examples 1a-1g, 2a-2g, 3a-3g and Comparative Example 1 were used as samples to measure the molecular weight, wear resistance, thermal properties and mechanical properties. The specific measurement methods are as follows. The measurement results are shown in Table 2 below:
[0096] 1. Molecular weight: Hexafluoroisopropanol was used as solvent and tested by gel chromatography analyzer (GPC). The model of the gel chromatography analyzer was Agilent 1260 Infinity II GPC / SEC gel chromatography analyzer;
[0097] 2. Wear resistance: Use Taber abrasion tester to test and measure the amount of wear (g) of the sample before and after the test;
[0098] 3. Thermal properties: The test was carried out according to the test method of GB / T 3682-2000, with a temperature of 230°C and a load of 2.16 kg to measure the melt flow rate (g / 10min) of the sample.
[0099] 4. Mechanical properties: The tensile strength (MPa) was measured according to the test method of GB / T 1040-2006, and the tensile rate was 50 mm / min; the flexural strength (MPa) was measured according to the test method of GB / T 9341-2008, and the bending speed was 2 mm / min; the simply supported beam notched impact strength (kJ / m 2 ), the gap type is type A.
[0100] Table 2 Parameter adjustment and performance measurement table of Examples 1a-1g, 2a-2g, 3a-3g and Comparative Example 1
[0101]
[0102] It can be seen from Table 2 that the nylon 612 abrasive wire prepared in the embodiment of the present application has excellent wear resistance (6.0-21.7 g), thermal properties (9.8-20.2 g / 10 min) and mechanical properties (tensile strength 57.5-73.7 MPa, flexural strength 67.1-84.5 MPa, simply supported beam notched impact strength 7.1-20.4 kJ / m 2 ). The nylon 612 abrasive wire obtained by using nylon 612 prepolymer 2 in Example 2 has better wear resistance, thermal properties and mechanical properties than those in Examples 1 and 3. This may be because the nylon 612 prepolymer 2 used in Example 2 not only makes the wear-resistant filler uniformly dispersed between the prepolymers when participating in the reaction, but also integrates into the molecular structure of nylon 612, thereby obtaining nylon 612 abrasive wire with better performance.
[0103] In addition, it can be seen from Table 2 that the present application further prefers the raw material ratio of "20-80 parts of nylon 612 prepolymer and 20-80 parts of wear-resistant filler", and further prefers the raw material ratio of "70 parts of nylon 612 prepolymer and 30 parts of wear-resistant filler". The present application continues to conduct experiments with "70 parts of nylon 612 prepolymer and 30 parts of wear-resistant filler" as the preferred ratio.
[0104] Example 4
[0105] In this embodiment, based on the method of embodiment 2d, nylon 612 prepolymer 2 is replaced by nylon 612 prepolymer 4.
[0106] Example 5
[0107] In this embodiment, based on the method of embodiment 2d, nylon 612 prepolymer 2 is replaced by nylon 612 prepolymer 5.
[0108] Example 6
[0109] In this embodiment, based on the method of embodiment 2d, nylon 612 prepolymer 2 is replaced by nylon 612 prepolymer 6.
[0110] Example 7
[0111] In this embodiment, based on the method of embodiment 2d, nylon 612 prepolymer 2 is replaced by nylon 612 prepolymer 7.
[0112] Example 8
[0113] In this embodiment, based on the method of embodiment 2d, nylon 612 prepolymer 2 is replaced by nylon 612 prepolymer 8.
[0114] Example 9
[0115] In this embodiment, based on the method of embodiment 2d, nylon 612 prepolymer 2 is replaced by nylon 612 prepolymer 9.
[0116] Example 10
[0117] In this embodiment, based on the method of embodiment 2d, nylon 612 prepolymer 2 is replaced by nylon 612 prepolymer 10.
[0118] Examples 11-15
[0119] In Examples 11-15, based on the method of Example 2d, the process parameters of the forming step (abrasive filament spinning step and abrasive filament post-treatment step) are adjusted. For specific adjustments, please refer to Table 2 below.
[0120] Table 3 Forming step parameter table of Example 2d and Examples 11-15
[0121]
[0122] Performance measurement
[0123] The nylon 612 abrasive wires prepared in the above Examples 4-17 were used as samples to measure the molecular weight, wear resistance, thermal properties and mechanical properties. The specific measurement methods are as described above. The measurement results are shown in Table 4 below.
[0124] Table 4 Performance measurement table of Example 2d and Examples 4-17
[0125]
[0126] It can be seen from Table 4 that Examples 4-5 are based on the raw materials of nylon 612 prepolymer. When preparing nylon 612 prepolymer, the present application adds a set amount of antioxidant, catalyst and molecular weight regulator, which can promote efficient reaction, reduce oxidation of prepolymer, ensure product quality and performance, improve production efficiency, and thus obtain the prepolymer with the molecular weight distribution required by the present application.
[0127] Combining the test results of Example 2d with Example 6, it can be concluded that the antioxidant prepared by compounding antioxidant 1098 and antioxidant 168 in a mass ratio of 1:1 in the present application has a better effect on the prepolymer obtained, so it is further preferred.
[0128] Combining the test results of Example 2d with those of Examples 7-8, it can be concluded that the catalyst containing phosphate or hypophosphite used in the present application enables the reaction to proceed smoothly, further improving the efficiency and feasibility of the reaction, and phosphoric acid and sodium hypophosphite are more preferred.
[0129] Combining the test results of Example 2d with Examples 7-8, it can be concluded that the use of an amine molecular weight regulator in the present application can effectively control the molecular weight of the prepolymer so that it falls within a specific target range (molecular weight of 10,000-40,000), thereby obtaining a nylon 612 material with better performance to meet the needs of different application scenarios. A further preferred molecular weight regulator is hexamethylenediamine.
[0130] In addition, in combination with Example 1d, Example 2d and Examples 4-10, it can be obtained that when the molecular weight of the nylon 612 prepolymer is 15000-20000, the corresponding nylon 612 abrasive wire has more excellent wear resistance and mechanical properties. This may be because the nylon 612 prepolymer at this time not only promotes the rapid dispersion of the wear-resistant filler, but also maintains a dynamic balance of the dispersed wear-resistant filler, thereby ensuring that the wear-resistant filler always maintains a uniform dispersion effect, providing a good foundation for subsequent reactions.
[0131] Combining Example 2d with Examples 11-17, it can be obtained that when preparing nylon 612 abrasive filaments in the present application, the parameters in the steps of extrusion, drawing, and heat drying will also affect the performance of the product to a certain extent, and specifically define "the aspect ratio of the twin-screw extruder is 44, the rotation speed is 60-200rpm, and the temperature in the temperature zone is 230-280°C; the drawing device is preheated in a boiling water bath, and the drawing ratio is 2-4 times; the hot oven temperature is 160-220°C, and the heat drying is 0.1-100h" as appropriate, and further preferred process parameters are "the aspect ratio of the twin-screw extruder is 44, the rotation speed is 100-200rpm, and the temperature in the temperature zone is 240-260°C; the drawing device is preheated in a boiling water bath, and the drawing ratio is 2.9-3.1 times; the hot oven temperature is 160-220°C, and the heat drying is 24h".
[0132] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A nylon 612 abrasive wire, characterized in that: The raw materials include the following components in parts by weight: 10-90 parts of nylon 612 prepolymer and 10-90 parts of wear-resistant filler; the molecular weight of the nylon 612 prepolymer is 10,000-40,000.
2. The nylon 612 abrasive filament according to claim 1, characterized in that: The molecular weight of the nylon 612 prepolymer is 15,000-20,000.
3. The nylon 612 abrasive filament according to claim 1, characterized in that: The terminal group of the nylon 612 prepolymer molecule is an amino group.
4. The nylon 612 abrasive filament according to claim 1, characterized in that: The nylon 612 prepolymer is obtained by condensation polymerization of a prepolymer raw material and water accounting for 5-30% of the mass of the prepolymer raw material. The prepolymer raw material includes 97-100 parts of nylon 612 salt, 0-1 part of antioxidant, 0-1 part of catalyst and 0-1 part of molecular weight regulator in parts by weight.
5. The nylon 612 abrasive filament according to any one of claims 4, characterized in that: It also includes maleic anhydride or maleic anhydride olefin copolymer, and the molar ratio of the maleic anhydride or maleic anhydride olefin copolymer to the molecular weight regulator is 1:
1.
6. The nylon 612 abrasive filament according to any one of claims 4, characterized in that: The antioxidant in the nylon 612 prepolymer is selected from one or more of antioxidant 1098, antioxidant 1010, antioxidant 168, and antioxidant H10.
7. The nylon 612 abrasive filament according to claim 5, characterized in that: The antioxidant in the nylon 612 prepolymer is a compound of antioxidant 1098 and antioxidant 168 in a mass ratio of 1:
1.
8. The nylon 612 abrasive filament according to claim 4, characterized in that: The catalyst in the nylon 612 prepolymer is selected from one of phosphoric acid, hypophosphorous acid, sodium hypophosphite, potassium hypophosphite and calcium hypophosphite.
9. The nylon 612 abrasive filament according to claim 4, characterized in that: The molecular weight regulator in the nylon 612 prepolymer is an amine molecular weight regulator.
10. The nylon 612 abrasive filament according to claim 8, characterized in that: The molecular weight regulator in the nylon 612 prepolymer is selected from one of pentamethylenediamine, hexamethylenediamine, nonanediamine and decanediamine.
11. The method for preparing nylon 612 abrasive filament according to claim 1, characterized in that: The following steps are involved: Mixing: Weigh a set amount of nylon 612 prepolymer, wear-resistant filler and maleic anhydride or maleic anhydride olefin copolymer, and mix them thoroughly to prepare the abrasive filament raw material. Molding: The abrasive wire raw materials are subjected to the processes of melting, spinning, drawing, shaping and viscosity increasing in sequence to produce nylon 612 abrasive wire products.
12. The preparation method according to claim 11, characterized in that: In the mixing step, the abrasive filament raw materials are fully mixed in a high-speed mixer at a stirring speed of 1000 r / min and a mixing time of 5-60 min.
13. The preparation method according to claim 11, characterized in that: In the mixing step, the wear-resistant filler is one or more of silicon carbide powder, diamond powder, and aluminum oxide powder that have been activated by a coupling agent, and the particle size of the powder is 18-3000 mesh.
14. The preparation method according to claim 11, characterized in that: In the forming step, the abrasive wire raw material is placed in an abrasive wire spinning device for processing. The abrasive wire spinning device includes a twin-screw extruder, a drawing device, a winder and a hot oven connected in sequence. The twin-screw extruder is provided with a spinneret. The abrasive wire raw material is put into the twin-screw extruder for heating and melting, and then passes through the spinneret, drawing device, winder and oven in sequence to carry out the corresponding processes of spinning, drawing, winding, drying and shaping.
15. The preparation method according to claim 14, characterized in that: In the forming step, the twin-screw extruder has an aspect ratio of 44, a rotation speed of 60-200 rpm, and a temperature zone of 230-280°C.
16. The preparation method according to claim 14, characterized in that: In the forming step, the drawing device is preheated in a boiling water bath, and the drawing ratio is 2-4 times.
17. The preparation method according to claim 14, characterized in that: In the forming step, the temperature of the hot oven is 160-220° C., and the hot baking time is 0.1-100 hours.