A packaging aluminum substrate and manufacturing method thereof

By applying high-impregnant adhesive material to the upper and lower surfaces of the dry film adhesive layer between the aluminum substrate and the BT/line layer, a closed-loop filling belt is formed, which solves the problem of poor airtightness in COB packaging technology and significantly improves the gas of the product Tightness and reliability, and simplify production processes.

CN111106223BActive Publication Date: 2024-11-08APT ELECTRONICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201911382272.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-27
Publication Date
2024-11-08
Estimated Expiration
2039-12-27

AI Technical Summary

Technical Problem

In the existing COB packaging technology, the pure adhesive dry film adhesive layer between the aluminum substrate and the BT/line layer causes poor airtightness of the finished substrate, resulting in water vapor entering and affecting product quality.

Method used

Apply adhesive materials to the upper and lower surfaces of the dry film adhesive layer between the aluminum substrate and the BT/line layer to form a closed-loop filling tape, and use highly wet adhesive materials such as silicone, silicone, etc. to fill the microscopic air gaps and enhance the gas Concentration.

Benefits of technology

It significantly enhances the airtightness and reliability of the finished packaging products, prevents water vapor from entering, and is simple in process and easy to implement, without changing raw materials or complex structures, reducing production costs and processing difficulties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111106223B_ABST
    Figure CN111106223B_ABST
Patent Text Reader

Abstract

The present invention discloses a packaged aluminum substrate, comprising a BT / circuit layer, an aluminum substrate, and a dry film adhesive layer located between the BT / circuit layer and the aluminum substrate, wherein the upper and lower surfaces of the dry film adhesive layer are coated with an adhesive material layer, so that a closed-loop filling belt is formed between the BT / circuit layer, the dry film adhesive layer, and the aluminum substrate. At the same time, the present invention also discloses a method for making a packaged aluminum substrate, wherein adhesive material is applied, the false pasting is performed, and the pressing is performed before the false pasting process. The packaged aluminum substrate of the present invention has the characteristics of high airtightness and strong reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of COB packaging, and in particular relates to a packaging aluminum substrate and a manufacturing method thereof. Background Art

[0002] COB (Chip On Board) chip packaging technology is a new type of LED packaging method, which can also be understood as a light-emitting body in which multiple LED chips are integrated and packaged on the same substrate.

[0003] At present, the market demand is growing day by day, and the production and manufacturing of packaging aluminum substrates generally includes the following steps: BT (resin-based copper clad laminate) circuit layer etching → surface solder mask treatment → aluminum substrate cutting → false pasting → pressing → V-CUT → stamping → finished product washing and inspection.

[0004] The above technologies are relatively mature, but in the process of "pressing", Figure 1 As shown in the figure, the BT / circuit layer is combined with the aluminum substrate. The current traditional process is to add a layer of pure glue (epoxy resin adhesive) with the same shape as the BT / circuit layer between the aluminum substrate and the BT / circuit layer. Then the aluminum substrate and the BT / circuit layer are bonded by a hot pressing process. In this process, the dry film adhesive layer formed by the pure glue has low wettability after being melted by heat, resulting in many microscopic air gaps between the multilayer materials of the finished substrate, such as Figure 2 and Figure 3 In actual use, it provides a path for water vapor to enter, which eventually leads to unstable product quality. Summary of the invention

[0005] In order to solve the problem of poor airtightness of the existing packaging substrate, the first purpose of the present invention is to provide a packaging aluminum substrate with the characteristics of high airtightness and strong reliability.

[0006] To achieve the above object, the present invention is implemented according to the following technical solutions:

[0007] The encapsulated aluminum substrate described in the present invention includes a BT / circuit layer, an aluminum substrate and a dry film adhesive layer located between the BT / circuit layer and the aluminum substrate. The upper surface and the lower surface of the dry film adhesive layer are coated with an adhesive material layer, so that a closed-loop filling belt is formed between the BT / circuit layer, the dry film adhesive layer and the aluminum substrate.

[0008] Furthermore, the two adhesive material layers do not completely overlap in the vertical direction.

[0009] Furthermore, the two adhesive material layers do not overlap in the vertical direction.

[0010] Furthermore, the two adhesive material layers are in the shape of circular rings or polygonal rings.

[0011] Furthermore, the width of the adhesive material layer is 1%-50% of the width of the dry film adhesive layer at its narrowest point.

[0012] Furthermore, the adhesive material used in the adhesive material layer is silica gel, silicone resin, epoxy resin, amino resin, polyurethane resin, unsaturated polyester or acrylic resin.

[0013] In order to solve the problem of poor airtightness of the existing packaging substrate, the second purpose of the present invention is to provide a method for manufacturing a packaging aluminum substrate, which has the characteristics of simple production process and easy implementation.

[0014] To achieve the above object, the present invention is implemented according to the following technical solutions:

[0015] In the method for manufacturing the packaged aluminum substrate of the present invention, before the false pasting process, an adhesive material is applied to the upper surface and the lower surface of the dry film adhesive layer;

[0016] False pasting: Align the BT / circuit layer, dry film adhesive layer and aluminum substrate, and initially paste them together through a laminating machine;

[0017] Lamination: The BT / circuit layer, dry film adhesive layer and aluminum substrate are pressed together by a hot pressing process, so that a closed-loop filling belt is formed between the BT / circuit layer, dry film adhesive layer and aluminum substrate.

[0018] Further, the positions where the adhesive material is applied on the upper surface and the lower surface of the dry film adhesive layer are different in the vertical direction.

[0019] Furthermore, the adhesive material is silica gel, silicone resin, epoxy resin, amino resin, polyurethane resin, unsaturated polyester or acrylic resin.

[0020] Furthermore, the temperature adopted by the laminating machine is 120+ / -10°C; the temperature adopted by the hot pressing process is 172+ / -20°C, and the pressure is 10-50Kg.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The packaged aluminum substrate described in the present invention fills the microscopic air gaps on the water vapor entry path by constructing a closed-loop filling belt between the BT / circuit layer, the dry film adhesive layer, and the aluminum base layer, thereby preventing water vapor from entering, thereby significantly enhancing the airtightness and reliability of the packaged finished light source.

[0023] 2. The manufacturing method of the packaged aluminum substrate of the present invention has a simple production process, which is basically the same as the existing production process. It only adds a simple and mature process step, does not require changing the raw materials, and does not require making more complex structural changes to the aluminum base or BT / circuit layer. It is easy to implement. Whether from the perspective of production cost or processing difficulty, it has achieved very good results. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The specific embodiments of the present invention are further described in detail below in conjunction with the accompanying drawings, wherein:

[0025] Figure 1 It is a schematic diagram of the process of combining the BT / circuit layer with the aluminum substrate using the traditional process in the background art;

[0026] Figure 2 It is a schematic diagram of the state of combining the BT / circuit layer and the aluminum substrate together using the traditional process in the background technology;

[0027] Figure 3 yes Figure 2 The enlarged view of point A in the middle;

[0028] Figure 4 is a cross-sectional view of the packaged aluminum substrate of the present invention;

[0029] Figure 5 It is a schematic diagram showing the addition of adhesive material to the packaged aluminum substrate of the present invention;

[0030] Figure 6 It is a cross-sectional view of the packaged aluminum substrate of the present invention after adding adhesive material;

[0031] Figure 7 It is a cross-sectional view of the packaged aluminum substrate described in Example 1 of the present invention.

[0032] 1: BT / circuit layer 2: dry film adhesive layer 3, aluminum substrate 4, adhesive material layer DETAILED DESCRIPTION

[0033] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0034] like Figure 4-7As shown, the packaging aluminum substrate described in the present invention has made improvements in the process in order to solve the problem of microscopic air gaps existing in the prior art. The improvement is not to add adhesive materials between layers, but to combine the existing substrate and cleverly apply adhesive materials with better wettability. It uses very little material but can solve the problem of microscopic air gaps. That is, it is only necessary to apply adhesive materials on the upper and lower surfaces of the dry film adhesive layer to form a closed-loop filling belt between the BT / circuit layer, the dry film adhesive layer and the aluminum substrate.

[0035] Specifically, the encapsulated aluminum substrate includes a BT / circuit layer 1, an aluminum substrate 3, and a dry film adhesive layer 2 located between the BT / circuit layer and the aluminum substrate. The upper and lower surfaces of the dry film adhesive layer 2 are coated with an adhesive material layer 4, so that a closed-loop filling belt is formed between the BT / circuit layer 1, the dry film adhesive layer 2 and the aluminum substrate 3.

[0036] The adhesive material is silicone, silicone resin, epoxy resin, amino resin, polyurethane resin, unsaturated polyester or acrylic resin, which has higher wettability than pure glue, but is more expensive. Therefore, without affecting the overall product price, the width of the adhesive layer formed is 1%-50% of the narrowest width of the dry film adhesive layer, which can be 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc., preferably 20%. Of course, if the price cost is not considered, the dry film adhesive layer is directly replaced by the adhesive material layer, which is simpler in processing procedures.

[0037] The adhesive material layer is specifically in the shape of a ring, which may be a circular ring, a polygonal ring, or other irregular rings. The main purpose is to form a closed loop to achieve the purpose of eliminating microscopic air gaps.

[0038] Furthermore, the adhesive material layers are not completely overlapped in the vertical direction, or even not overlapped at all. Figure 4 As shown in the figure, it will not cause the problem of significantly increasing the overall thickness of the package aluminum substrate. Figure 7 As shown, Figure 7 The product thickness shown is more uniform across the board.

[0039] Correspondingly, the method for manufacturing the packaged aluminum substrate of the present invention is based on the existing processing, and only the process before lamination is adjusted. The specific process is as follows:

[0040] S1: Etching of BT (resin-based copper clad laminate) circuit layer 1

[0041] Use acidic copper chloride etching solution to etch away the copper layer not covered by the wet film, leaving the required circuit copper foil. Then use alkaline sodium hydroxide aqueous solution to clean the wet film on the etched surface.

[0042] S2: Surface solder mask treatment

[0043] Use a brush grinder or sandblaster to remove the oxide layer on the surface of the BT / circuit layer. Then use the screen printing method to evenly apply photosensitive white oil on the surface of the BT / circuit layer, and then put it in an oven for baking; then perform solder mask exposure, that is, cover the pre-drawn solder mask film on the circuit substrate after the second pre-baking; then perform solder mask development, and develop the BT / circuit layer after the second exposure through a developer; bake again, and then plate a layer of alloy coating on the surface of the gold wire pad; then drill the reference hole and rivet hole.

[0044] S3: Aluminum substrate 3 cutting

[0045] Cut the single-sided copper clad laminate into the size specifications required for production.

[0046] S4: Apply adhesive material

[0047] The release paper of the cut dry film adhesive layer 2 and the mirror film on the surface of the aluminum substrate 3 are peeled off, and adhesive material is applied to the upper surface and the lower surface of the dry film adhesive layer 2.

[0048] S5: Fake Post

[0049] The BT / circuit layer 1, the dry film adhesive layer 2 and the aluminum substrate 3 are aligned and initially bonded by a laminating machine, wherein the temperature of the laminating machine is controlled at 110-130°C.

[0050] S6: Pressing

[0051] On a vacuum hot press machine, the BT / circuit layer 1, the dry film adhesive layer 2 and the aluminum substrate 3 are pressed together by a hot pressing process, so that a closed-loop filling belt is formed between the BT / circuit layer 1, the dry film adhesive layer 2 and the aluminum substrate 3. The hot pressing process uses a traditional hot press machine with a temperature of 170+ / -15℃ and a pressure of 10-50Kg, or a fast press machine with a temperature controlled at 180+ / -10℃ and a pressure of 10-30KG.

[0052] S7: V-CUT

[0053] The V-CUT machine pre-cuts the pressed materials according to the required single shape, making it easier to separate the boards into single light sources during packaging production.

[0054] S8: Stamping

[0055] According to the shape requirements, choose to use CNC drilling and milling or die punching.

[0056] S9: Finished product washing inspection

[0057] The packaged aluminum substrate processed by the above process constructs a closed-loop filling belt between the BT / circuit layer 1, the dry film adhesive layer 2, and the aluminum base layer 3, thereby filling the microscopic air gaps on the water vapor entry path, thereby preventing the entry of water vapor, and ultimately significantly enhancing the airtightness and reliability of the packaged finished light source.

[0058] In terms of processing technology, it is basically the same as the existing production process. It only adds a simple and mature step. There is no need to change the raw materials or make more complex structural changes to the aluminum base or BT / circuit layer. It is easy to implement.

[0059] In order to further demonstrate the remarkable effects of the packaged aluminum substrate and the manufacturing method thereof described in the present invention, the following specific embodiments are described:

[0060] Embodiment 1:

[0061] The encapsulated aluminum substrate described in the present invention includes a BT / circuit layer 1, an aluminum substrate 3 and a dry film adhesive layer 2 located between the BT / circuit layer 1 and the aluminum substrate 3, and the upper surface and lower surface of the dry film adhesive layer 2 are coated with an adhesive material layer 4, so that a closed-loop filling belt is formed between the BT / circuit layer 1, the dry film adhesive layer 2 and the aluminum substrate 3.

[0062] The adhesive material layer 4 does not overlap in the vertical direction, is in the shape of a ring, is made of silica gel, and occupies 20% of the area of ​​the dry film adhesive layer.

[0063] Correspondingly, the method for manufacturing the package aluminum substrate is to apply adhesive material on the upper surface and the lower surface of the dry film adhesive layer 2 before the lamination process;

[0064] The BT / circuit layer 1, the dry film adhesive layer 2 and the aluminum substrate 3 are pressed together by a hot pressing process, so that a closed-loop filling belt is formed between the BT / circuit layer 1, the dry film adhesive layer 2 and the aluminum substrate 3. The hot pressing process uses a traditional hot press machine with a temperature of 170°C and a pressure of 25Kg.

[0065] Embodiment 2:

[0066] The difference between this embodiment and the first embodiment is that the adhesive material layer 4 does not completely overlap in the vertical direction. Compared with the package aluminum substrate described in the first embodiment, the product thickness is slightly inferior.

[0067] Embodiment 3:

[0068] The difference between this embodiment and embodiment 1 is that the shape of the adhesive material layer 4 is a square ring. Compared with the package aluminum substrate described in embodiment 1, the product quality is the same, but the amount of adhesive material used is slightly more, and the cost is slightly higher.

[0069] Embodiment 4:

[0070] The difference between this embodiment and embodiment 1 is that the shape of the adhesive material layer 4 is a hexagonal ring. Compared with the packaged aluminum substrate described in embodiment 1, the product quality is the same, but the amount of adhesive material used is slightly more, and the cost is slightly higher.

[0071] However, compared with the encapsulated aluminum substrate described in Example 3, the product quality is the same, except that the amount of adhesive material used is slightly less and the cost is slightly lower.

[0072] Embodiment 5:

[0073] The difference between this embodiment and embodiment 1 is that the area occupied by the adhesive material layer 4 is 1% of the area of ​​the dry film adhesive layer 2. Compared with the package aluminum substrate described in embodiment 1, the amount of adhesive material used is much less, saving costs, but the microscopic air gaps on the water vapor entry path may not be filled completely. Therefore, the airtightness and reliability of the product are slightly weaker.

[0074] Embodiment 6:

[0075] The difference between this embodiment and embodiment 1 is that the area occupied by the adhesive material layer 4 is 50% of the area of ​​the dry film adhesive layer 2. Compared with the package aluminum substrate described in embodiment 1, the amount of adhesive material used is much larger, which increases the cost, but the microscopic air gaps on the water vapor entry path are filled very fully. Therefore, the product has stronger airtightness and reliability.

[0076] Embodiment 7:

[0077] The difference between this embodiment and embodiment 1 is that the area occupied by the adhesive material layer 4 is 30% of the area of ​​the dry film adhesive layer 2. Compared with the encapsulated aluminum substrate described in embodiment 1, the amount of adhesive material used is slightly more, which increases the cost a little, but the microscopic air gaps on the water vapor entry path are filled more fully. Therefore, the airtightness and reliability of the product are slightly stronger.

[0078] Embodiment 8:

[0079] The only difference between this embodiment and embodiment 1 is that the raw material used for the adhesive material layer is polyurethane resin. Compared with the package aluminum substrate described in embodiment 1, the product quality, cost and thickness are basically the same.

[0080] Embodiment 9:

[0081] The only difference between this embodiment and embodiment 1 is that the raw material used for the adhesive material layer is acrylic resin. Compared with the package aluminum substrate described in embodiment 1, the product quality, cost and thickness are basically the same.

[0082] Embodiment 10:

[0083] The difference between this embodiment and embodiment 1 is that the raw material used for the adhesive material layer is a mixed material of silicone resin and epoxy resin. Compared with the package aluminum substrate described in embodiment 1, the product quality, cost and thickness are basically the same.

[0084] Embodiment 11:

[0085] The difference between this embodiment and embodiment 1 is that the raw material used for the adhesive material layer is a mixed material of amino resin and unsaturated polyester. Compared with the package aluminum substrate described in embodiment 1, the product quality, cost and thickness are basically the same.

[0086] Embodiment 12:

[0087] The difference between this embodiment and embodiment 1 is that the raw material used for the adhesive material layer is a mixed material of silica gel, amino resin and acrylic resin. Compared with the package aluminum substrate described in embodiment 1, the product quality, cost and thickness are basically the same.

[0088] Embodiment 13:

[0089] The only difference between this embodiment and embodiment 1 is that the temperature of the laminating machine during the false application process is controlled at 120° C., and when the hot pressing process uses a traditional hot pressing machine, the temperature is 185° C. and the pressure is 50 Kg.

[0090] Embodiment 14:

[0091] The only difference between this embodiment and embodiment 1 is that the temperature of the laminating machine during the false application process is controlled at 110° C., and when the hot pressing process uses a traditional hot pressing machine, the temperature is 155° C. and the pressure is 10 Kg.

[0092] Embodiment 15:

[0093] The only difference between this embodiment and embodiment 1 is that the temperature of the laminating machine is controlled at 130° C. during the false lamination process, and the hot pressing process uses a fast pressing machine with a temperature of 180° C. and a pressure of 20 Kg.

[0094] Embodiment 16:

[0095] The difference between this embodiment and embodiment 1 is that the temperature of the laminating machine is controlled at 115° C. during the false lamination process, and the hot pressing process adopts a fast pressing machine with a temperature of 190° C. and a pressure of 30 kg.

[0096] Embodiment 17:

[0097] The only difference between this embodiment and embodiment 1 is that the temperature of the laminating machine is controlled at 125° C. during the false lamination process, and the hot pressing process uses a fast pressing machine with a temperature of 170° C. and a pressure of 10 Kg.

[0098] Comparative Example:

[0099] The package aluminum substrate produced by traditional technology is not introduced in detail here because it is existing technology.

[0100] The encapsulated aluminum substrates of Examples 1-17 and the comparative example are compared, and the specific details are shown in Table 1:

[0101] category Microscopic air gap Airtightness reliability thickness(%) cost(%) Example 1 none excellent excellent 0.1 0.10 Example 2 none excellent excellent 0.2 0.10 Example 3 none excellent excellent 0.1 0.12 Example 4 none excellent excellent 0.1 0.11 Example 5 Very rare good good 0.1 0.02 Example 6 none excellent excellent 0.1 0.50 Example 7 none excellent excellent 0.1 0.30 Example 8 none excellent excellent 0.1 0.10 Example 9 none excellent excellent 0.1 0.10 Example 10 none excellent excellent 0.1 0.10 Embodiment 11 none excellent excellent 0.1 0.10 Example 12 none excellent excellent 0.1 0.11 Example 13 none excellent excellent 0.1 0.10 Embodiment 14 none excellent excellent 0.1 0.10 Embodiment 15 none excellent excellent 0.1 0.10 Example 16 none excellent excellent 0.1 0.10 Embodiment 17 none excellent excellent 0.1 0.10 Comparative Example More Difference Difference / /

[0102] According to Table 1 above, the encapsulated aluminum substrate of the present invention has been greatly improved in terms of airtightness and reliability compared to the traditional technology, although the cost has increased, that is, it has increased by 0.5% at most, and the best embodiment usually adopted has only increased by 0.1%, and the thickness of the product has basically not changed. Therefore, from the perspective of the overall market demand and long-term development of the product, it is very worthy of promotion.

[0103] In addition, it should be noted that: although the packaging aluminum substrate and its production method described in the present invention have very small technical improvements, in the actual process, reference was made to the prior art, no one has adopted this method, and it is not easily obtained by technical personnel in this field. It was obtained after hundreds of experiments by the inventor, and the effect of achieving a multiplier effect was achieved.

[0104] Other technologies involved in the packaged aluminum substrate and the manufacturing method thereof described in the present invention can be found in the prior art and will not be described in detail here.

[0105] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Therefore, any modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention shall still fall within the scope of the technical solution of the present invention.

Claims

1. A package aluminum substrate, comprising a BT / circuit layer, an aluminum substrate, and a dry film adhesive layer located between the BT / circuit layer and the aluminum substrate, characterized in that: The upper and lower surfaces of the dry film adhesive layer are coated with adhesive material layers, so that a closed-loop filling belt is formed between the BT / circuit layer, the dry film adhesive layer and the aluminum substrate; The adhesive material layer is annular; the adhesive material used in the adhesive material layer is silica gel, silicone resin, epoxy resin, amino resin, polyurethane resin, unsaturated polyester or acrylic resin.

2. The package aluminum substrate according to claim 1, characterized in that: The two adhesive material layers do not completely overlap in the vertical direction.

3. The package aluminum substrate according to claim 1, characterized in that: The two adhesive material layers do not overlap in the vertical direction.

4. The package aluminum substrate according to claim 1, characterized in that: The two adhesive material layers are in the shape of circular rings or polygonal rings.

5. The package aluminum substrate according to claim 1, characterized in that: The width of the adhesive material layer is 1% to 50% of the width of the dry film adhesive layer at its narrowest point.

6. A method for manufacturing the package aluminum substrate according to any one of claims 1 to 5, characterized in that: Apply adhesive material before the fake pasting process: peel off the release paper of the cut dry film adhesive layer and the mirror film on the surface of the aluminum substrate, and apply adhesive material on the upper and lower surfaces of the dry film adhesive layer; False pasting: Align the BT / circuit layer, dry film adhesive layer and aluminum substrate, and initially paste them together through a laminating machine; Lamination: The BT / circuit layer, the dry film adhesive layer and the aluminum substrate are pressed together by a hot pressing process, so that a closed-loop filling belt is formed between the BT / circuit layer, the dry film adhesive layer and the aluminum substrate.

7. The method for manufacturing a packaged aluminum substrate according to claim 6, characterized in that: The positions where the adhesive material is applied on the upper surface and the lower surface of the dry film adhesive layer are different in the vertical direction.

8. The method for manufacturing a packaged aluminum substrate according to claim 6, characterized in that: The adhesive material is silica gel, silicone resin, epoxy resin, amino resin, polyurethane resin, unsaturated polyester or acrylic resin.

9. The method for manufacturing a packaged aluminum substrate according to claim 6, characterized in that: The temperature adopted by the laminating machine is 120+ / -10°C; the temperature adopted by the hot pressing process is 172+ / -20°C, and the pressure is 10-50Kg.