A novel turbulence controller for tundish of profiled blank and its preparation method
By adopting the composite structure design of shell and core in the tundish turbulence controller, combined with the isostatic pressing method and special inner cavity shape, the problems of poor fluidity and high cost of molten steel in the existing technology are solved, and efficient steel Liquid residence time is extended and costs are reduced.
Patent Information
- Application Number
- CN202010065250.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-01-20
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-01-20
AI Technical Summary
The existing tundish turbulence controller cannot meet the performance requirements of metallurgical functionalization, longevity and low cost at the same time. The shape design of the inner cavity is not conducive to improving the flow characteristics of molten steel, and the production cost is high.
It is designed with a composite structure of the shell and the core. The core adopts a special truncated cone-shaped inner cavity, which is prepared by isostatic pressing. The joints are designed to adapt to the erosion and erosion rates of different parts, improving the overall performance and extending the service life.
It improves the average residence time and flow quality of the molten steel in the tundish, extends the service life, reduces the production cost, and solves the problems of turbulent kinetic energy of the molten steel and steel penetration in the brick joints.
Smart Images

Figure CN111113633B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of continuous casting refractory material technology, in particular to a novel turbulence controller for a tundish of a profiled blank and a preparation method thereof. Background Art
[0002] Setting a turbulence controller in the tundish of a continuous casting machine can change the route of molten steel in the tundish, prolong the residence time, and promote the floating and removal of inclusions, which plays an important role in improving the quality of the ingot. At the same time, it can slow down the scouring of the impact zone of the tundish working lining by the ladle injection and increase the continuous casting time of the tundish. In recent years, the production technology of turbulence controllers has developed towards metallurgical functionalization, longevity, and low cost, but the tundish turbulence controllers produced by existing technologies cannot meet the performance requirements of metallurgical functionalization, longevity, and low cost at the same time.
[0003] CN103658577B discloses a method for preparing a composite turbulence controller for a continuous casting tundish, wherein the composite turbulence controller comprises an outer shell, a bottom plate, a sleeve core, an expansion joint, and an anti-oxidation coating. The outer shell is cast and formed by magnesium casting material, the bottom plate is built by machine-pressed magnesium carbon bricks, the sleeve core is built by machine-pressed "fan-shaped" magnesium carbon bricks, expansion joints are set between the outer shell and the bottom plate, and between the outer shell and the sleeve core, and an anti-oxidation coating is applied on the outer surface of the sleeve core. However, the inner cavity shape of the invention is "cylindrical", which has a poor effect on suppressing the turbulent kinetic energy of the ladle injection turbulence, and is not conducive to improving the flow characteristics of the molten steel in the tundish. At the same time, the sleeve core is built by "fan-shaped" magnesium carbon bricks, which has poor overall performance, is prone to brick removal, and lacks quality stability.
[0004] CN109591158A discloses a tundish flow stabilizer, which is composed of an outer shell and a hollow inner cavity integrally inlaid, wherein the shape and size of the outer shell are designed to be adapted to the impact zone of the tundish, the center of the outer shell is concave, so that the outer shell is in the shape of a "concave", and the outer shell is formed by a steel fiber aluminum-magnesium castable preform, wherein the steel fiber aluminum-magnesium castable preform is integrally cast; and the hollow inner cavity is cylindrical and suitable for being embedded in the center of the outer shell, the hollow inner cavity is flush with the top of the outer shell, and the hollow inner cavity is masonry-made of a magnesium-carbon preform, wherein the carbon preform is isostatically pressed integrally; and a method for manufacturing a tundish flow stabilizer is also disclosed, by improving the inner cavity of the flow stabilizer from the traditional masonry molding method of multiple magnesium-carbon bricks to an integrally pressed molding method, thereby eliminating the easily corroded inner cavity brick seams in the traditional flow stabilizer, and completely solving the problem of steel seepage and steel penetration in the brick seams of the inner cavity of the traditional flow stabilizer, and greatly extending the life of the tundish flow stabilizer. However, the preparation cost is high and the promotion and application are limited.
[0005] Isostatic pressing is a molding method that subjects the clay to equal liquid static pressure in all directions. Liquid is used as the pressure transmission medium. The clay is loaded into an elastic mold and pressed into shape in a high-pressure cylinder. The isostatic press consists of a high-pressure container and a high-pressure oil pump. The high-pressure container is made of high-grade alloy steel and has a certain thickness to withstand huge pressure. The size of the container is selected according to the size of the molded product. The liquid medium in the high-pressure container can be oil, water or glycerin, etc. Brake oil or anhydrous glycerin is generally used. The compressibility of these two liquids is very small, and almost all the pressure can be transmitted to the elastic mold. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a new type of turbulence controller for a continuous casting tundish of special-shaped billets. The composite structure of the main body shell and the sleeve core is designed. The sleeve core is a truncated cone preform with a special inner cavity shape designed based on water model experimental research. It is prepared by using magnesium carbon material and isostatic pressing, and at the same time meets the technical performance requirements of metallurgical functionalization and longevity.
[0007] To achieve the above-mentioned purpose, the present invention provides the following technical solutions: a novel turbulence controller for a tundish of a profiled blank, comprising a shell and a core, wherein the core is arranged in the inner cavity of the shell, and the longitudinal center line of the core coincides with the longitudinal center line of the inner cavity of the shell, and a joint seam is arranged between the shell and the core, and the outer portion of the core is a truncated cone-shaped magnesium preform, so that the thickness of the side wall of the upper portion of the core is greater than that of the lower portion, so that the scouring and erosion rate of the side wall of the upper portion of the core is greater than that of the lower portion, so that the service life of each part of the side wall of the core is synchronized, and the inner and outer walls of the core are integrally formed. The rotating surface design eliminates the crack problem caused by thermal stress concentration on the side wall of the core sleeve. The interior of the core sleeve is a parabolic cavity, which is divided into an upper core cavity, a lower core cavity and a bottom core cavity. The upper core cavity is a cylindrical surface, the lower core cavity is a concave rotating parabola, and the bottom core cavity is a circular plane. The bottom surface of the core cavity is in contact with the upper surface of the shell cavity. The core sleeve is directly isostatically pressed to form a tundish turbulence controller with the shell. The overall performance is good, which is conducive to ensuring the shape of the cavity and has a long service life.
[0008] Preferably, the core sleeve is made of magnesium carbon material and is a truncated cone-shaped magnesium preform prepared by isostatic pressing, so that the turbulence controller group has a compressive strength of ≥40Mpa, high molding quality, good overall performance, and is resistant to corrosion and erosion.
[0009] Preferably, the outer portion of the sleeve core is in the shape of a truncated cone with a large upper bottom surface and a small lower bottom surface, the diameter D1 of the upper bottom surface of the truncated cone is 650-700 mm, and the diameter D2 of the lower bottom surface of the truncated cone is 570-620 mm;
[0010] Preferably, the upper inner cavity of the sleeve core is cylindrical, and the cylinder height a is 70-90 mm, which is beneficial to maintaining the shape of the upper inner cavity of the sleeve core, and is beneficial to improving the service life, meeting the requirement of 36-40 hours for the service life of the special-shaped blank tundish.
[0011] Preferably, the lower part of the inner cavity of the core sleeve has a small upper opening and a large lower opening, the upper opening diameter d1 is 380-400 mm, the lower opening diameter d2 is 420-450 mm, the height h of the lower part of the inner cavity of the core sleeve is 280-320 mm, and the thickness b of the bottom of the inner cavity of the core sleeve is 70-90 mm. The design of the special shape of the lower part of the inner cavity of the core sleeve changes the running trajectory of the steel flow, extends the flow route, and extends the average residence time of the molten steel in the tundish.
[0012] Preferably, the width of the joint is larger at the top and smaller at the bottom, with the upper width m being 10-15 mm and the lower width n being 5-10 mm. The joint also serves as an expansion joint, thus avoiding quality problems caused by thermal expansion of the magnesium-carbon sleeve.
[0013] A method for preparing a novel turbulence controller for a tundish of a profiled blank comprises the following steps:
[0014] 1. The shell is casted by using a magnesium spinel castable, the shape and size of the shell are designed according to the shape and size of the impact zone of the working lining of the continuous casting tundish, and the shell is casted by using a magnesium spinel castable produced by the prior art, and is prepared after natural curing and baking in a heating furnace; the magnesium spinel castable is produced by the prior art, and has a MgO content of ≥71wt%, a volume density of ≥3.03g / cm3, and a flexural strength (1500°C) of ≥9Mpa;
[0015] 2. The core sleeve is prepared by isostatic pressing and is made of the following raw materials in percentage by weight:
[0016] Main material: 76-84wt% sintered magnesia mixed with 1mm≦particle size≤3mm, 0.074mm<particle size<1mm, and particle size≦0.074mm
[0017] Auxiliary materials: flake graphite 11.5~16wt%
[0018] Antioxidant: 2-5wt% of one or a mixture of aluminum powder, silicon powder, aluminum-magnesium alloy powder, silicon carbide powder
[0019] Binder: 3.5-4.0wt% phenolic resin.
[0020] The sintered magnesia is produced by using light-burned magnesia with a MgO content of 95wt% as raw material through processes such as ball pressing and high-temperature vertical kiln calcination, and the MgO content percentage is 94-95wt%.
[0021] The flake graphite has a purity C content of ≥98wt% and a particle size of 100 meshes.
[0022] The aluminum powder has a purity AI content of ≥99wt% and a particle size of 100 meshes.
[0023] The silicon powder has a purity Si content of ≥97wt% and a particle size of 100 meshes.
[0024] The aluminum-magnesium alloy powder has an AI content of 50±3wt%, an AI+Mg content of ≥97wt%, and a particle size of 100 meshes.
[0025] The silicon carbide has a purity SiC content of ≥94wt% and a particle size of 100 meshes.
[0026] The phenolic resin has a solid content of ≥72wt%, a residual carbon content of ≥42wt%, and a moisture content of ≤5wt%;
[0027] The core sleeve is prepared by isostatic pressing, which includes the following steps:
[0028] 1) Ingredients: weigh the above raw materials according to the above ratio;
[0029] 2) Mixing: preheat the mixer to 40-50°C, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm at low speed → add phenolic resin after dry mixing for 1-2 minutes → add flake graphite after wet mixing for 2-3 minutes → add sintered magnesia with a particle size of ≦0.074mm and antioxidant after wet mixing for 2-3 minutes → wet mixing for 2-3 minutes → high-speed mixing for 10-15 minutes → discharge, the mud temperature during mixing is less than 70°C;
[0030] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 200-250MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;
[0031] 4) Natural drying and baking: After the green body is naturally dried for 8 to 16 hours, it is put into the kiln for baking: ① heating from room temperature to 140 to 160°C at a heating rate of 10°C / h, and keeping warm for 4 to 8 hours; ② heating from room temperature to 200 to 220°C at a heating rate of 10°C / h, and keeping warm for 16 to 24 hours; ③ stopping the fire, cooling naturally to room temperature and then taking out of the kiln, the preparation of the lower part of the core sleeve (3) is completed, and its compressive strength is ≥40MPa.
[0032] 3. Apply a layer of magnesium coating material with a thickness of 25 to 35 mm on the outer surface of the sintered magnesia. The magnesium carbon coating material refers to the coating material prepared by the existing technology using the recycled granular material of waste magnesia carbon bricks with a particle size of 1mm≦<3mm, 0.074mm<particle size<1mm and sintered magnesia fine powder, soft clay, silicon powder, sodium tripolyphosphate, etc. according to a certain ratio, wherein the weight percentage of the recycled magnesium carbon granular material is 60 to 70%;
[0033] 4. Put the core sleeve into the shell of the turbulence controller to ensure that the longitudinal center line of the core sleeve coincides with the longitudinal center line of the inner cavity of the shell. Fill the joint between the shell and the core sleeve with sintered magnesia sand with a particle size of ≤1mm. Naturally cure for 1 to 2 days, and the preparation of the new special-shaped billet continuous casting ladle turbulence controller is completed.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] (1) The core sleeve is directly isostatically pressed and assembled with the shell to form a tundish turbulence controller, which has good overall performance, is conducive to ensuring the shape of the inner cavity, and has a long service life.
[0036] (2) The core sleeve of the novel turbulence controller for the continuous casting tundish of the profiled blank of the present invention is a truncated cone-shaped container with a special inner cavity shape designed based on water model experimental research and application test verification. It effectively reduces the turbulent kinetic energy of the ladle injection and improves the flow field of the molten steel in the tundish. The results of the water model experimental research show that the tundish turbulence controller designed by the present invention is better than the turbulence controller for the continuous casting tundish of the profiled blank described in CN104707956B: the average residence time of the molten steel in the tundish is increased by more than 8.9% year-on-year, and the dead zone ratio is reduced by more than 7.4% year-on-year. By using the present invention, the total oxygen content in the molten steel in the crystallizer is reduced by more than 13% year-on-year.
[0037] (3) A joint seam is provided between the shell and the core of the turbulence controller of the new type of special-shaped billet continuous casting tundish of the present invention, which also serves as an expansion seam, thereby avoiding quality problems caused by thermal expansion of the magnesium-carbon core. The width of the joint seam is larger at the top and smaller at the bottom, thereby effectively preventing the problem of steel infiltration from top to bottom through the joint seam. At the same time, after the joint seam is filled with sintered magnesia sand with a particle size of ≤1mm, a layer of magnesium coating material with a thickness of 25-35mm is applied on its outer surface, thereby preventing the problem of filling material falling off and improving quality reliability.
[0038] (4) The core sleeve of the new turbulence controller of the special-shaped blank continuous casting tundish of the present invention is made of magnesium carbon material and isostatic pressing method, and has achieved beneficial effects: compressive strength ≥40Mpa, high molding quality, good overall performance, corrosion resistance and erosion resistance, and effectively solves the problem that the core sleeve of the flow stabilizer of the special-shaped blank continuous casting tundish described in CN104707956B is made of arc-shaped magnesium carbon bricks in annular masonry, has poor overall performance, lacks quality stability, and the service life is not synchronized with the service life of the tundish working lining. The service life is increased from 31-35 hours to 36-40 hours year-on-year. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0040] Figure 1 This is a front view of the structure of the new type of turbulence controller for the continuous casting tundish of the profiled blank of the present invention;
[0041] Figure 2 It is a top view of the sleeve core structure of the novel turbulence controller of the special-shaped blank continuous casting tundish of the present invention.
[0042] In the figure, 1. outer shell; 2. core sleeve; 3. joint seam; 4. upper part of the inner cavity of the core sleeve; 5. lower part of the inner cavity of the core sleeve, 6. bottom of the inner cavity of the core sleeve. DETAILED DESCRIPTION
[0043] The following examples are provided to further illustrate the invention, but the invention is not limited thereto. The magnesium castables and magnesium coating materials used in the examples are all produced by existing technologies. Other raw materials are commercially available products:
[0044] Sintered magnesia is made of light-burned magnesia with a MgO content of 95wt% as raw material, produced by processes such as ball pressing and high-temperature vertical kiln calcination. The MgO content is 94-95wt%, and it is a mixture of 1mm≦particle size≤3mm, 0.074mm<particle size<1mm, and particle size≦0.074mm.
[0045] Flake graphite, with a purity C content of ≥98wt% and a particle size of 100 mesh.
[0046] Aluminum powder, with a purity of AI content ≥99wt% and a particle size of 100 mesh.
[0047] Silicon powder, with a purity Si content of ≥97wt% and a particle size of 100 mesh.
[0048] Aluminum-magnesium alloy powder, with an AI content of 50±3wt%, an AI+Mg content of ≥97wt%, and a particle size of 100 mesh.
[0049] Silicon carbide, with a purity SiC content of ≥94wt% and a particle size of 100 mesh.
[0050] The solid content of the phenolic resin is ≥72wt%, the residual carbon content is ≥42wt%, and the moisture content is ≤5wt%.
[0051] The technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The magnesium castables and magnesium coatings used in the embodiments are all produced using existing technologies.
[0052] See also Figure 1-2 ,
[0053] Embodiment 1:
[0054] like Figure 1 , Figure 2 As shown, a novel turbulence controller for a tundish of a special-shaped blank comprises an outer shell 1 and a core 2. The core 2 is arranged in the inner cavity of the outer shell 1, and the longitudinal center line of the core 2 coincides with the longitudinal center line of the inner cavity of the outer shell 1. A joint seam 3 is provided between the outer shell 1 and the core 2. The outer portion of the core 2 is a truncated cone-shaped magnesium preform, and the inner portion of the core 2 is a parabolic inner cavity, which is divided into an upper portion 4 of the core inner cavity, a lower portion 5 of the core inner cavity and a bottom portion 6 of the core inner cavity. The upper portion 4 of the core inner cavity is a cylindrical surface, the lower portion 5 of the core inner cavity is a concave rotating parabola, and the bottom portion 6 of the core inner cavity is a circular plane.
[0055] Preferably, the sleeve core 2 is made of magnesium carbon material and is a truncated cone-shaped magnesium preform prepared by isostatic pressing.
[0056] The core 2 of the turbulence controller is in the shape of a truncated cone with a large upper bottom and a small lower bottom, the diameter D1 of the upper bottom of the truncated cone is 700 mm, and the diameter D2 of the lower bottom of the truncated cone is 620 mm; the upper part 4 of the inner cavity of the core is a cylindrical surface, and the cylinder height a is 80 mm, the lower part 5 of the inner cavity of the core is in the shape of a "drum" with a small upper opening and a large lower opening, the upper opening diameter d1 is 400 mm, the lower opening diameter d2 is 450 mm, the height h of the lower part 5 of the inner cavity of the core is 300 mm, and the thickness b of the inner cavity bottom 6 of the core is 80 mm.
[0057] The width of the joint seam 3 is larger at the top and smaller at the bottom, with the upper width m being 15 mm and the lower width n being 10 mm.
[0058] The shape and size of the shell 1 are designed according to the shape and size of the impact zone of the continuous casting tundish working lining, and are cast by using magnesium castables produced by existing technology, and are prepared by natural curing and baking in a heating furnace.
[0059] The core sleeve 2 is prepared by isostatic pressing and is made of the following raw materials in percentage by weight:
[0060] Main material: 84wt% sintered magnesia mixed with 1mm≦particle size≤3mm, 0.074mm<particle size<1mm, and particle size≦0.074mm
[0061] Auxiliary materials: flake graphite 10.5wt%
[0062] Antioxidant: Aluminum powder 2.0wt%
[0063] Binder: 3.5wt% phenolic resin.
[0064] The core sleeve 2 is prepared by isostatic pressing, which includes the following steps:
[0065] 1) Ingredients: weigh the above raw materials according to the above ratio;
[0066] 2) Mixing: preheat the mixer to 40°C, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.075mm<particle size<1mm at low speed → add phenolic resin after dry mixing for 1 minute → add flake graphite after wet mixing for 3 minutes → add sintered magnesia with a particle size of ≦0.075mm and antioxidant after wet mixing for 2 minutes → wet mixing for 3 minutes → high-speed mixing for 10 minutes → discharge, and the temperature of the mud during mixing is less than 70°C;
[0067] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 200MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;
[0068] 4) Natural drying and baking: After the green body is naturally dried for 8 hours, it is put into the kiln for baking: ① uniformly and continuously heated from room temperature to 140°C, and kept warm for 8 hours; ② uniformly and continuously heated from 140°C to 200°C, and kept warm for 16 hours. After natural cooling, it is taken out of the kiln. The preparation of the sleeve core 2 is completed, and its compressive strength is ≥40MPa.
[0069] The preparation method of the novel turbulence controller for the continuous casting ladle of special-shaped billets is as follows: the core sleeve 2 is installed in the shell 1 of the turbulence controller, and the longitudinal center line of the core sleeve 2 is ensured to coincide with the longitudinal center line of the inner cavity of the shell 1, and the joint seam 3 between the shell 1 and the core sleeve 2 is filled with sintered magnesia sand with a particle size of ≤1mm, and a layer of magnesium coating material with a thickness of 25mm is applied on the outer surface thereof, and naturally cured for 1 day, and the preparation of the novel turbulence controller for the continuous casting ladle of special-shaped billets is completed.
[0070] Example 2
[0071] As described in Example 1, except that:
[0072] The core sleeve 2 of the turbulence controller has a diameter D1 of the upper bottom surface of the truncated cone of 650 mm and a diameter D2 of the lower bottom surface of the truncated cone of 570 mm; the cylindrical height a of the upper part 4 of the inner cavity of the core sleeve is 65 mm, the upper opening diameter d1 of the lower part of the inner cavity of the core sleeve is 380 mm, the lower opening diameter d2 is 420 mm, the height h of the lower part 5 of the inner cavity of the core sleeve is 280 mm, and the thickness b of the inner cavity bottom 6 of the core sleeve is 70 mm.
[0073] The width of the joint seam 3 is larger at the top and smaller at the bottom, with the upper width m being 10 mm and the lower width n being 5 mm.
[0074] The core sleeve 2 is prepared by isostatic pressing and is made of the following raw materials in percentage by weight:
[0075] Main material: 76wt% sintered magnesia mixed with 1mm≦particle size≤3mm, 0.074mm<particle size<1mm, and particle size≦0.074mm
[0076] Auxiliary materials: flake graphite 16wt%
[0077] Antioxidant: Silicon powder 2wt%, Silicon carbide powder 2wt%
[0078] Binder: 4.0wt% phenolic resin.
[0079] The core sleeve 2 is prepared by isostatic pressing, which includes the following steps:
[0080] 1) Ingredients: weigh the above raw materials according to the above ratio;
[0081] 2) Mixing: preheat the mixer to 50°C, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm at low speed → add phenolic resin after dry mixing for 2 minutes → add flake graphite after wet mixing for 2 minutes → add sintered magnesia with a particle size of ≦0.074mm and antioxidant after wet mixing for 3 minutes → wet mixing for 2 minutes → high-speed mixing for 15 minutes → discharge, and the temperature of the mud during mixing is less than 70°C;
[0082] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 250MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;
[0083] 4) Natural drying and baking: After the green body is naturally dried for 16 hours, it is put into the kiln for baking: ① uniformly and continuously heated from room temperature to 160°C, and kept warm for 8 hours; ② uniformly and continuously heated from 160°C to 220°C, and kept warm for 24 hours. After natural cooling, it is taken out of the kiln. The preparation of the sleeve core 2 is completed, and its compressive strength is ≥40MPa.
[0084] The preparation method of the novel turbulence controller for the continuous casting ladle of special-shaped blanks is as follows: the core sleeve 2 is installed in the shell 1 of the turbulence controller, and the longitudinal center line of the core sleeve 2 is ensured to coincide with the longitudinal center line of the inner cavity of the shell 1, and the joint seam 3 between the shell 1 and the core sleeve 2 is filled with sintered magnesia sand with a particle size of ≤1mm, and a layer of magnesium coating material with a thickness of 35mm is applied on the outer surface thereof, and naturally cured for 1 day, and the preparation of the novel turbulence controller for the continuous casting ladle of special-shaped blanks is completed.
[0085] Example 3
[0086] As described in Example 1, except that:
[0087] The core sleeve 2 of the turbulence controller has a diameter D1 of the upper bottom surface of the truncated cone of 670 mm and a diameter D2 of the lower bottom surface of the truncated cone of 600 mm; the cylindrical height a of the upper part 4 of the inner cavity of the core sleeve is 95 mm, the upper opening diameter d1 of the lower part of the inner cavity of the core sleeve is 390 mm, the lower opening diameter d2 is 440 mm, the height h of the lower part 5 of the inner cavity of the core sleeve is 290 mm, and the thickness b of the inner cavity bottom 6 of the core sleeve is 90 mm.
[0088] The width of the joint seam 3 is larger at the top and smaller at the bottom, with the upper width m being 12 mm and the lower width n being 7 mm.
[0089] The core sleeve 2 is prepared by isostatic pressing and is made of the following raw materials in percentage by weight:
[0090] Main material: 79wt% sintered magnesia mixed with 1mm≦particle size≤3mm, 0.074mm<particle size<1mm, and particle size≦0.074mm
[0091] Auxiliary materials: flake graphite 14wt%
[0092] Antioxidant: Aluminum-magnesium alloy powder 3.3wt%
[0093] Binder: 3.7wt% phenolic resin.
[0094] The core sleeve 2 is prepared by isostatic pressing, which includes the following steps:
[0095] 1) Ingredients: weigh the above raw materials according to the above ratio;
[0096] 2) Mixing: preheat the mixer to 45°C, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm at low speed → add phenolic resin after dry mixing for 1 minute → add flake graphite after wet mixing for 3 minutes → add sintered magnesia with a particle size of ≦0.074mm and antioxidant after wet mixing for 3 minutes → wet mixing for 2 minutes → high-speed mixing for 10 minutes → discharge, and the temperature of the mud during mixing is less than 70°C;
[0097] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 220MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;
[0098] 4) Natural drying and baking: After the green body is naturally dried for 12 hours, it is put into the kiln for baking: ① uniformly and continuously heated from room temperature to 150°C, and kept warm for 6 hours; ② uniformly and continuously heated from 150°C to 210°C, and kept warm for 20 hours. After natural cooling, it is taken out of the kiln. The preparation of the sleeve core 2 is completed, and its compressive strength is ≥40MPa.
[0099] The preparation method of the novel turbulence controller for the continuous casting ladle of special-shaped billets is as follows: the core sleeve 2 is installed in the shell 1 of the turbulence controller, and the longitudinal center line of the core sleeve 2 is ensured to coincide with the longitudinal center line of the inner cavity of the shell 1, and the joint seam 3 between the shell 1 and the core sleeve 2 is filled with sintered magnesia sand with a particle size of ≤1mm, and a layer of magnesium coating material with a thickness of 30mm is applied on the outer surface thereof, and naturally cured for 1 day, and the preparation of the novel long-life continuous casting ladle turbulence controller is completed.
[0100] Comparative example: CN104707956B discloses a turbulence controller for a continuous casting tundish of a special-shaped billet and an installation method thereof, comprising an outer shell, a bottom plate, a sleeve core and a pressure ring. The outer shell is a cavity structure with an upper end opening, the bottom plate is located on the bottom of the outer shell cavity, the bottom end of the sleeve core is located above the bottom plate, the pressure ring is arranged at the upper end of the sleeve core and is located in the outer shell cavity, and expansion joints are arranged between the bottom of the inner cavity of the outer shell and the bottom plate, and between the inner wall of the outer shell and the sleeve core. The invention solves the problem of falling off of the upper layer of magnesium-carbon bricks on the side wall of the sleeve core by arranging a pressure ring above the sleeve core; when installing the turbulence controller, a plurality of pressure bricks are arranged on the same circumference in the same plane above the pressure ring to solve the problem of overall floating of the turbulence controller.
[0101] The water models of the turbulence controller for the tundish of the continuous casting of the profiled blank disclosed in Examples 1-3 of the present invention and the comparative document CN104707956B are established according to the similarity ratio of 1:2. The results of the water model experiments are compared and analyzed as shown in Table 1 below:
[0102] Table 1
[0103]
[0104]
[0105] By comparing the data in Table 1 above, the tundish turbulence controller designed by the present invention is compared with the profiled billet continuous casting tundish flow stabilizer described in comparison example CN104707956B: the average residence time of the molten steel in the tundish is increased by more than 8.9% year-on-year, and the dead zone ratio is reduced by more than 7.4% year-on-year.
[0106] The structural materials, service life and total oxygen content of molten steel in the crystallizer of a turbulence controller for a shaped billet continuous casting tundish disclosed in Examples 1-3 of the present invention and the comparative document CN104707956B (comparison test steel grade Q355B, gas samples are taken from the crystallizer to detect the oxygen content. The oxygen content in steel is the sum of dissolved oxygen and non-metallic oxide inclusion combined oxygen. Since the dissolved oxygen content is not much, it is generally believed that the non-metallic oxide inclusion oxygen content in steel is the total oxygen content, that is, the total oxygen content in steel represents the control level of oxide inclusions in steel) are compared in the application of the shaped billet continuous casting tundish of Laiwu Iron and Steel Group Yinshan Steel Co., Ltd., as shown in Table 2 below:
[0107] The comparison of the application of tundish for continuous casting of special-shaped billets in Laiwu Iron and Steel Group Yinshan Steel Co., Ltd. is shown in Table 2 below.
[0108] Table 2
[0109]
[0110]
[0111] By comparing the data in Table 2 above, the service life of the new turbulence controller for the continuous casting tundish of the profiled blank prepared by the present invention is more than 5 hours longer than that of the turbulence controller for the continuous casting tundish of the profiled blank described in the existing patent technology CN104707956B, and the total oxygen content in the molten steel in the crystallizer is reduced by more than 13% year-on-year.
[0112] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A turbulence controller for a tundish of a profiled blank, comprising a shell (1) and a core (2), wherein the core (2) is arranged in an inner cavity of the shell (1), and a longitudinal centerline of the core (2) coincides with a longitudinal centerline of the inner cavity of the shell (1), and a joint seam (3) is provided between the shell (1) and the core (2), characterized in that: The outer portion of the sleeve core (2) is a truncated cone-shaped magnesium preform, so that the side wall thickness of the upper portion of the sleeve core is greater than the side wall thickness of the lower portion, and the inner and outer walls of the sleeve core are designed as a rotating surface. The sleeve core (2) is a truncated cone-shaped magnesium preform made of magnesium carbon material and is prepared by isostatic pressing. The inner portion of the sleeve core (2) is a parabolic inner cavity, which is divided into an upper portion (4) of the sleeve core inner cavity, a lower portion (5) of the sleeve core inner cavity and a bottom portion (6) of the sleeve core inner cavity. The upper portion (4) of the sleeve core inner cavity is a cylindrical surface, the lower portion (5) of the sleeve core inner cavity is a concave rotating parabola, and the bottom portion (6) of the sleeve core inner cavity is a circular plane. The lower portion (5) of the inner cavity of the core sleeve has a small upper opening and a large lower opening, the upper opening diameter d1 is 380-400 mm, the lower opening diameter d2 is 420-450 mm, the height h of the lower portion (5) of the inner cavity of the core sleeve is 280-320 mm, and the thickness b of the bottom (6) of the inner cavity of the core sleeve is 70-90 mm; The width of the joint seam (3) is larger at the top and smaller at the bottom, with the top width m being 10 to 15 mm and the bottom width n being 5 to 10 mm.
2. The turbulence controller for a profiled blank tundish according to claim 1, characterized in that: The outer portion of the sleeve core is in the shape of a truncated cone with a large upper bottom surface and a small lower bottom surface. The diameter D1 of the upper bottom surface of the truncated cone is 650-700 mm, and the diameter D2 of the lower bottom surface of the truncated cone is 570-620 mm.
3. The turbulence controller for a profiled blank tundish according to claim 2, characterized in that: The upper portion (4) of the inner cavity of the sleeve core is cylindrical, and the cylinder height a is 70 to 90 mm.
4. A method for preparing a turbulence controller for a beam blank tundish according to any one of claims 1 to 3, comprising the following steps:
1. The shell (1) is casted using a magnesium spinel castable material. The shape and size of the shell (1) are designed according to the shape and size of the impact zone of the continuous casting tundish working lining. The shell (1) is casted using magnesium spinel castable material produced by existing technology, and is prepared after natural curing and baking in a heating furnace. The magnesium spinel castable is produced by existing technology, has an MgO content of ≥71 wt%, and a bulk density of ≥3.03 g / cm 3 , flexural strength at 1500℃ ≥9Mpa; 2. The core sleeve (2) is prepared by isostatic pressing and is made of the following raw materials in percentage by weight: Main material: 76-84wt% sintered magnesia mixed with 1mm≤particle size≤3mm, 0.074mm<particle size<1mm, and particle size≤0.074mm. Auxiliary materials: flake graphite 11.5~16wt%, Antioxidant: 2-5 wt% of one or more of aluminum powder, silicon powder, aluminum-magnesium alloy powder, silicon carbide powder Binder: phenolic resin 3.5~4.0wt%, The sum of the weight percentages of all raw materials of the core (2) is 100%. The sintered magnesia is produced by using light-burned magnesia with a MgO content of 95 wt% as raw material through a process of pelletizing and high-temperature vertical kiln calcination. The MgO content is 94-95 wt%. The flake graphite has a purity C content of ≥98wt% and a particle size of 100 mesh. The aluminum powder has a purity of Al content ≥ 99wt% and a particle size of 100 mesh. The silicon powder has a purity Si content of ≥97wt% and a particle size of 100 mesh. The aluminum-magnesium alloy powder has an Al content of 50±3 wt %, an Al+Mg content of ≥97 wt %, and a particle size of 100 mesh. The silicon carbide has a purity SiC content of ≥94wt% and a particle size of 100 mesh. The phenolic resin has a solid content of ≥72wt%, a residual carbon content of ≥42wt%, and a moisture content of ≤5wt%; The core sleeve (2) is prepared by isostatic pressing, which includes the following steps: 1) Ingredients: weigh the above raw materials according to the ratio; 2) Mixing: Preheat the mixer to 40-50℃, add sintered magnesia with a particle size of 1mm≤≤3mm and 0.074mm<particle size<1mm at low speed → dry mix for 1-2 minutes, then add phenolic resin → wet mix for 2-3 minutes, then add flake graphite → wet mix for 2-3 minutes, then add sintered magnesia with a particle size of ≤0.074mm and antioxidant → wet mix for 2-3 minutes → high speed mixing for 10-15 minutes → discharge. During the mixing process, the slurry temperature should be less than 70℃. 3) Green body molding: Fill the clay into the mold, then remove the air in the mold, press it under 200~250MPa with isostatic pressure, and then take it out of the mold. The green body molding is completed; 4) Natural drying and baking: After the green body is formed and naturally dried for 8 to 16 hours, it is then put into the kiln for baking: ① from room temperature, the temperature is raised to 140 to 160°C at a rate of 10°C / h, and kept warm for 4 to 8 hours; ② then the temperature is raised to 200 to 220°C at a rate of 10°C / h, and kept warm for 16 to 24 hours; ③ the fire is stopped, and the green body is naturally cooled to room temperature before being taken out of the kiln. The preparation of the sleeve core (2) is completed, and its compressive strength is ≥40MPa; 3. Apply a layer of magnesium-carbon coating material with a thickness of 25 to 35 mm on the outer surface of the sintered magnesia. The magnesium-carbon coating material refers to the coating material prepared by the existing technology using recycled granular materials of waste magnesia-carbon bricks with a particle size of 1 mm ≤ < 3 mm, recycled magnesia-carbon particles with a particle size of 0.074 mm < < 1 mm, sintered magnesia fine powder, soft clay, silicon powder, and sodium tripolyphosphate in a certain ratio, wherein the weight percentage of the recycled magnesia-carbon particles is 60 to 70%; 4. The core sleeve (2) is placed in the shell (1) of the turbulence controller, ensuring that the longitudinal center line of the core sleeve (2) coincides with the longitudinal center line of the inner cavity of the shell (1), and the joint seam (3) between the shell (1) and the core sleeve (2) is filled with sintered magnesia sand with a particle size of ≤1mm. After natural curing for 1 to 2 days, the preparation of the turbulence controller for the continuous casting tundish of the special-shaped blank is completed.