A combined slab continuous casting tundish turbulence controller and its preparation method

Through the design of the combined slab continuous casting tundish turbulence controller, combined with the optimization of the seam and convex structure, the use of recycled magnesium carbon castables and isostatic pressing molding method, the poor performance of the tundish turbulence controller in the existing technology has been solved. Optimize the problem and achieve the effects of metallurgical functionalization, longevity and low cost.

CN111113634BActive Publication Date: 2024-10-22LAIWU STEEL YINSHAN SECTION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010065260.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-01-20
Publication Date
2024-10-22
Estimated Expiration
2040-01-20

AI Technical Summary

Technical Problem

The existing tundish turbulence controller cannot meet the performance requirements of metallurgical functionalization, longevity and low cost at the same time, and the inner cavity shape design is not conducive to improving the flow characteristics of molten steel, and is prone to debricking and lack of quality stability.

Method used

It adopts a combined slab continuous casting tundish turbulence controller design, including the combined structure of the shell and the casing core. The upper and lower parts of the casing core are made of different materials. The shape of the inner cavity is designed based on simulation research, and the joint design is to prevent steel penetration. , the raised structure optimizes steel flow impact and turbulence control, using recycled magnesium carbon castables and isostatic pressing to reduce costs.

Benefits of technology

It effectively suppresses the turbulent kinetic energy of the steel flow, extends the service life, improves the flow state of the molten steel, reduces production costs, solves the problem of flow injection and slag entrainment in the impact zone, and improves the overall performance and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111113634B_ABST
    Figure CN111113634B_ABST
Patent Text Reader

Abstract

The present invention discloses a combined slab continuous casting tundish turbulence controller and a preparation method thereof, comprising an outer shell and a sleeve core, the sleeve core being arranged in the inner cavity of the outer shell, the sleeve core comprising an upper sleeve core portion and a lower sleeve core portion arranged up and down, the lower sleeve core portion being arranged on the bottom surface of the inner cavity of the outer shell, and the longitudinal center lines of the upper sleeve core portion and the lower sleeve core portion coincide with the longitudinal center line of the inner cavity of the outer shell, a joint seam is arranged between the side walls of the outer shell and the sleeve core, the width of the joint seam is larger at the upper portion and smaller at the lower portion, a protruding structure deviating from the longitudinal center line of the inner cavity of the sleeve core and the casting center of the ladle is arranged at the bottom of the inner cavity of the lower sleeve core, and the protruding structure is truncated cone-shaped. The combined structural design of the main body outer shell, the upper sleeve core portion and the lower sleeve core portion is adopted, the upper sleeve core portion and the lower sleeve core portion are designed as a whole, made of different materials, and prepared separately, and the performance requirements of metallurgical functionalization, longevity, and low cost are met at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of continuous casting refractory materials, and in particular to a combined slab continuous casting tundish turbulence controller and a preparation method thereof. Background Art

[0002] Setting a turbulence controller in the tundish of a continuous casting machine can change the route of molten steel in the tundish, prolong the residence time, and promote the floating and removal of inclusions, which plays an important role in improving the quality of the ingot. At the same time, it can slow down the scouring of the impact zone of the tundish working lining by the ladle injection and increase the continuous casting time of the tundish. In recent years, the production technology of turbulence controllers has developed towards metallurgical functionalization, longevity, and low cost, but the tundish turbulence controllers produced by existing technologies cannot meet the performance requirements of metallurgical functionalization, longevity, and low cost at the same time.

[0003] The patent document with the publication number CN103658577B discloses a preparation method of a composite turbulence controller for a continuous casting tundish. The composite turbulence controller includes a shell, a bottom plate, a sleeve core, an expansion joint, and an anti-oxidation coating. The shell is cast by magnesium castables, the bottom plate is built by machine-pressed magnesium carbon bricks, and the sleeve core is built by machine-pressed "fan-shaped" magnesium carbon bricks. Expansion joints are set between the shell and the bottom plate, and between the shell and the sleeve core, and an anti-oxidation coating is applied on the outer surface of the sleeve core. The shortcomings of this invention are: the inner cavity is "cylindrical", which has a poor effect on suppressing the turbulent kinetic energy of the ladle injection flow, and is not conducive to improving the flow characteristics of the molten steel in the tundish. At the same time, the sleeve core is built by "fan-shaped" magnesium carbon bricks, which has poor overall performance, is prone to brick peeling, lacks quality stability, and has high production costs. Summary of the invention

[0004] In view of the above problems, the present invention provides a combined slab continuous casting tundish turbulence controller and a preparation method thereof, which adopts a combined structural design of a main body shell, an upper sleeve core and a lower sleeve core. The upper sleeve core and the lower sleeve core are designed as an integral whole, made of different materials, and prepared separately. The shape design of the inner cavity of the combined sleeve core is based on the numerical simulation research and application test of the slab continuous casting tundish, and at the same time meets the performance requirements of metallurgical functionality, long life and low cost.

[0005] The technical solution of the present invention to solve the technical problem is:

[0006] A combined slab continuous casting tundish turbulence controller includes an outer shell and a sleeve core, the sleeve core is arranged in the inner cavity of the outer shell, the sleeve core includes an upper sleeve core part and a lower sleeve core part arranged up and down, the lower sleeve core part is arranged on the bottom surface of the inner cavity of the outer shell, and the longitudinal center lines of the upper sleeve core part and the lower sleeve core part coincide with the longitudinal center line of the inner cavity of the outer shell, a joint seam is arranged between the side walls of the outer shell and the sleeve core, the width of the joint seam is larger at the upper part and smaller at the lower part, which can naturally increase the density of the filling material at the lower part of the joint seam, and effectively prevent the problem of steel infiltration from the joint seam from top to bottom. The bottom of the inner cavity of the lower sleeve core part is provided with a protruding structure deviating from the longitudinal center line of the inner cavity of the sleeve core and the casting center of the ladle, and the protruding structure is truncated cone-shaped. The present invention reduces the spraying caused by the steel flow impacting the protruding structure and the scouring of the inner cavity wall of the turbulence controller by arranging the protruding structure deviating from the longitudinal center line of the inner cavity of the core sleeve and the ladle casting center. The eccentric design improves the effect of suppressing the turbulent kinetic energy of the steel flow compared to arranging the protruding structure on the longitudinal center line of the inner cavity of the core sleeve. The protruding structure is arranged in a truncated cone shape, as opposed to a cylindrical or conical shape, which not only avoids the vertical scouring of the molten steel on it, but also ensures its rigidity, which is beneficial for the protruding structure to maintain its shape and prolongs the service life of the turbulence controller.

[0007] Furthermore, the inner cavity of the upper part of the sleeve core is in the shape of a truncated cone with a small inner diameter at the upper part and a large inner cavity at the lower part, the height a of the upper part of the sleeve core is 290-320 mm, the inner diameter d1 of the upper bottom surface is 440-460 mm, the inner diameter d2 of the lower bottom surface is 500-520 mm, the inner cavity bottom surface of the lower part of the sleeve core is an arc curved surface, the inner cavity side wall and the bottom surface of the lower part of the sleeve core are transitioned by an arc chamfer, the radius R of the arc chamfer is 75-85 mm, the height b of the lower part of the sleeve core is 180-200 mm, the diameter d1 of the inner cavity bottom surface circle of the lower part of the sleeve core is 518-538 mm, and the thickness c of the bottom of the lower part of the sleeve core is 80-100 mm. The problem of molten steel splashing is solved by designing the upper part of the sleeve core to have a small upper opening and a large lower inner diameter.

[0008] Furthermore, the outer shape of the upper part of the core sleeve is a truncated cone with a large upper bottom and a small lower bottom, the outer diameter D1 of the upper bottom is 710-730 mm, and the outer diameter D2 of the lower bottom is 650-680 mm. The outer shape of the lower part of the core sleeve is a truncated cone with a large upper bottom and a small lower bottom, the outer diameter D2 of the upper bottom of the lower part of the core sleeve is 650-680 mm, and the outer diameter D3 of the lower bottom of the lower part of the core sleeve is 620-640 mm. The inner diameter of the upper bottom of the lower part of the core sleeve is the same as the inner diameter of the lower bottom of the upper part of the core sleeve, and the outer diameter of the upper bottom of the lower part of the core sleeve is the same as the outer diameter of the lower bottom of the upper part of the core sleeve. According to this design, the side wall of the core sleeve is thick at the upper end and thin at the lower end. Since the steel flow scours the upper part heavier than the lower part during construction, this design overcomes the technical problem that the erosion rate of the upper part is greater than that of the lower part, and prolongs the service life of the turbulence controller.

[0009] Furthermore, the shape of the raised structure is a truncated cone formed by cutting off a 20 mm high top of a cone, the bottom circle diameter d of the cone is 190 to 210 mm, and the height h is 190 to 210 mm. The raised structure is arranged at a point 97 to 98 mm away from the center of the bottom plane circle of the lower inner cavity of the sleeve core, and the distance y between the raised structure and the casting center line of the large ladle is 15 to 25 mm. The bottom plane of the lower inner cavity of the sleeve core and the side wall of the raised structure are transitioned by a circular chamfer, and the radius r of the circular chamfer is 45 to 55 mm.

[0010] Furthermore, the upper width m of the joining seam is 10-15 mm, and the lower width n is 5-10 mm.

[0011] A preparation method for a combined slab continuous casting tundish turbulence controller comprises the following steps: sequentially inserting a sleeve core lower part and a sleeve core upper part into a shell of the turbulence controller from bottom to top, ensuring that the longitudinal center lines of the sleeve core lower part and the sleeve core upper part coincide with the longitudinal center line of the inner cavity of the shell, filling the joints between the shell and the sleeve core lower part and the sleeve core upper part with sintered magnesia sand with a particle size of ≤1 mm, and applying a layer of recycled magnesia carbonaceous coating material with a thickness of 25 to 35 mm on the outer surface of the sintered magnesia sand, and preventing the sintered magnesia sand in the joint from falling off and causing the sleeve core loosening and other quality problems by the coating material; performing natural curing for 1 to 2 days, and the preparation of the combined slab continuous casting tundish turbulence controller is completed;

[0012] The shell is casted by magnesium spinel castable, and is prepared by natural curing and baking in a heating furnace. The shape and size of the shell are designed according to the shape and size of the impact zone of the working lining of the tundish of the profiled blank continuous casting. The magnesium spinel castable is produced by existing technology, and the MgO content is ≥71wt%, and the volume density is ≥3.03g / cm 3 , flexural strength (1500℃) ≥9Mpa;

[0013] The upper part of the sleeve core is cast by recycled magnesium carbon casting material, and the raw material composition of the recycled magnesium carbon casting material is: 20-25% recycled granular material of waste magnesium carbon brick with a particle size of 3mm≦<5mm, 22-25% recycled granular material of waste magnesium carbon brick with a particle size of 1mm≦<3mm, 15-20% recycled granular material of waste magnesium carbon brick with a particle size of 0.074mm≦<1mm, 0-5% sintered magnesia with a particle size of 3mm≦<5mm, 0-5% sintered magnesia with a particle size of 1mm≦<3mm, 0-7% sintered magnesia with a particle size of 0.074mm≦<1mm, and 10% sintered magnesia with a particle size of 0.074mm ~13%, lightly burned magnesium oxide powder with a particle size of ≤0.045mm 3.0~5.0%, silicon powder with a particle size of 200 mesh 2~4%, silicon powder 1.0~1.5%, active α-AI2O3 powder 3.0~5.0%, pure calcium aluminate cement 3.2~3.8%, sodium tripolyphosphate 0.15~0.2%, explosion-proof fiber 0.05~0.1%; the explosion-proof fiber is made of modified polypropylene fiber, has the characteristics of good dispersibility, no sintering, no wire drawing, little residue, good use effect, etc., and is an excellent anti-explosion additive for various amorphous refractory materials, especially high-strength and fast-drying amorphous refractory materials. Length L=6mm, phase diameter D=0.048mm, melting point 165~175℃.

[0014] As is known to all, carbon-containing refractory materials have excellent slag resistance. The carbon source is selected from flake graphite, which is based on the fact that flake graphite has a well-developed crystalline carbon structure, and its corrosion resistance and oxidation resistance are better than amorphous carbon such as asphalt, carbon black, resin, and granular graphite. However, flake graphite has poor wettability and dispersibility to water. It is a well-known technical problem in the field of this technology to develop carbon-containing castables using flake graphite as a carbon source. Prior art research has granulated graphite to improve its wettability and dispersibility for the development of carbon-containing castables. The distinguishing feature of the present invention from the prior art is that the recycled granular material of waste magnesium carbon bricks is used as a carbon source, and an appropriate amount of silicon powder and sodium tripolyphosphate are introduced as a water reducer and dispersant. Lightly burned magnesium oxide powder and α-AI2O3 powder are introduced to react to generate magnesium aluminum spinel, which produces volume expansion, and further improves the resistance of recycled magnesium carbon dry material to slag penetration. The amount of magnesia sand replaced by recycled granular waste magnesia carbon bricks in the material composition of the regenerated magnesia carbon castable of the present invention reaches 60-70%, which greatly reduces the production cost of the regenerated magnesia carbon castable, and further greatly reduces the production cost of the low-cost and high-life slab continuous casting ladle turbulence controller of the present invention.

[0015] The lower part of the sleeve core is prepared by isostatic pressing, and the raw material composition of the lower part of the sleeve core is:

[0016] Main material: 76-84wt% sintered magnesia mixed with 1mm≦particle size≤3mm, 0.074mm<particle size<1mm, and particle size≦0.074mm.

[0017] Auxiliary materials: flake graphite 11.5~16wt%,

[0018] Antioxidant: 2-5wt% of one or a mixture of aluminum powder, silicon powder, silicon carbide powder, all with a particle size of 100 meshes,

[0019] Binder: 3.5-4.0wt% phenolic resin.

[0020] Furthermore, the method for preparing the upper part of the core sleeve comprises the following steps:

[0021] 1) adding the raw materials of the regenerated magnesium carbon castable into a mixer and dry mixing for 2 to 3 minutes;

[0022] 2) Add 6.7-7.2% water of the total weight of the material and wet mix for 4-6 minutes:

[0023] 3) After mixing, put it into the casting membrane on the upper part of the core, vibrate it with a vibrating rod, and when no large bubbles emerge, the green casting on the upper part of the core is completed;

[0024] 4) After solidification for 12 to 24 hours, remove the cast fetal membrane on the top of the core and allow it to cure naturally for 12 to 24 hours;

[0025] 5) Bake in a heating furnace: ① Raise the temperature from room temperature to 120-150℃ at a rate of 10℃ / h; ② Keep warm at 120-150℃ for 8-12h; ③ Raise the temperature to 200-220℃ at a rate of 10℃ / h; ④ Keep warm at 200-220℃ for 16-24h; ⑤ Stop the fire, cool naturally to room temperature, and the core sleeve preparation is completed.

[0026] Furthermore, the preparation method of the lower part of the core sleeve comprises the following steps:

[0027] 1) Ingredients: weigh the raw materials at the bottom of the core according to the above ratio;

[0028] 2) Mixing: preheat the mixer to 40-50°C, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm at low speed, add phenolic resin after dry mixing for 1-2 minutes, add flake graphite after wet mixing for 2-3 minutes, add sintered magnesia with a particle size of ≤0.074mm and antioxidant after wet mixing for 2-3 minutes, wet mix for 2-3 minutes, mix at high speed for 10-15 minutes, and discharge. During the mixing process, the temperature of the mud material is less than 70°C;

[0029] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 200-250MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;

[0030] 4) Natural drying and baking: After the green body is naturally dried for 8 to 16 hours, it is put into the kiln for baking: ① heat up from room temperature to 140-160°C at a rate of 10°C / h, and keep warm for 4 to 8 hours; ② heat up from room temperature to 200-220°C at a rate of 10°C / h, and keep warm for 16 to 24 hours; ③ stop the fire, cool naturally to room temperature, and then take out of the kiln. The preparation of the lower part of the core sleeve is completed.

[0031] Furthermore, the regenerated magnesium carbon coating material is a coating material prepared by treating and processing waste magnesium carbon bricks with a particle size of 1mm≦≤3mm and a particle size of 0.074mm<<1mm, and sintered magnesium sand fine powder with a particle size of ≤0.074mm, soft clay, silicon powder, and sodium tripolyphosphate, wherein the weight percentage of the regenerated magnesium carbon particles is 60-70%, the MgO content is ≥65wt%, and the volume density is ≥1.87g / cm 3 .

[0032] The effects provided in the content of the invention are only the effects of the embodiments, not all the effects of the invention. One of the above technical solutions has the following advantages or beneficial effects:

[0033] 1. The upper and lower parts of the sleeve core of the combined slab continuous casting tundish turbulence controller of the present invention are integrally designed and separately formed. The inner cavity of the upper part of the sleeve core is in the shape of a truncated cone with a small upper bottom surface and a large lower bottom surface. The diameter d1 of the upper bottom surface of the outer truncated cone is 440-460 mm, and the diameter d2 of the lower bottom surface of the outer truncated cone is 500-520 mm; the inner cavity bottom of the lower part of the sleeve core is an arc surface, and the diameter d1 of the inner cavity bottom surface circle is 518-538 mm. A convex structure is arranged at a point 97-98 mm away from the center of the bottom plane circle, and the distance y between the convex structure and the pouring center line of the large ladle is 15-25 mm; the convex structure is in the shape of a truncated cone, formed at the top of the interception height of 20 mm, the bottom surface circle diameter d of the cone is 190-210 mm, and the height h is 190-210 mm. The technical personnel in the field took the slab continuous casting tundish as the research object, and verified through numerical simulation research and application test that the above design has a direct impact on the flow state of the molten steel in the middle of the slab. The bottom of the inner cavity of the sleeve core of the slab continuous casting tundish turbulence controller designed by the present invention is an arc curved surface, and a truncated cone-shaped protrusion structure deviating from the center of the inner cavity of the turbulence controller and an inner cavity side wall with a truncated cone curved surface structure are provided, so that the large ladle injection flow is splashed in different directions in the sleeve core inner cavity of the turbulence controller, collides with each other, dissipates most of the kinetic energy, reduces the degree of turbulence formed by the molten steel, and suppresses the liquid level fluctuation caused by strong turbulence and the slag roll caused by the liquid surface vortex. The numerical simulation calculation results show that the turbulent kinetic energy of the steel flow in the central section of the tundish of the composite turbulence controller of the continuous casting tundish with a straight inner cavity described in CN103658577B is 1.52m 2 s2 , 1.92m 2 s 2 , down 20.8% year on year. By applying the present invention, the total oxygen content in the molten steel in the crystallizer is reduced by more than 11% year on year, and the problem of slag entrapment in the impact zone is effectively solved.

[0034] 2. The upper part of the sleeve core of the present invention adopts a recycled magnesium carbon castable with waste magnesium carbon brick recycled granular material as the main raw material. The amount of magnesium sand replaced by the waste magnesium carbon brick recycled granular material reaches 60-70%. The preparation method of casting and molding with the recycled magnesium carbon castable has achieved beneficial effects: high molding quality, good overall performance, and low production cost. It effectively solves the problems of poor overall performance, high production cost, and service life not being synchronized with the service life of the tundish working lining in the continuous casting tundish composite flow stabilizer sleeve core described in CN103658577B using fan-shaped magnesium carbon bricks for masonry. The service life is increased from 31-35 hours to 35-38 hours year-on-year, and the production cost is reduced by more than 32% year-on-year.

[0035] 3. The lower part of the sleeve core of the combined slab continuous casting tundish turbulence controller of the present invention is prepared by isostatic pressing using sintered magnesia as the main raw material. Isostatic pressing utilizes the incompressible nature of the liquid medium and the property of uniformly transmitting pressure to uniformly pressurize the sample from all directions. The pressure on the powder in all directions is uniform and consistent in size. Therefore, the powder is more densely and evenly molded, which improves the molding quality and overall performance of the arc surface of the inner cavity bottom of the lower part of the sleeve core and the truncated cone-shaped protrusion structure, meeting the requirements of metallurgical functionalization and longevity. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a front view of the structure of the combined slab continuous casting tundish turbulence controller of the present invention;

[0037] Figure 2 It is a top view of the sleeve-core structure of the combined slab continuous casting tundish of the present invention;

[0038] In the figure, 1, outer shell; 2, upper part of the core; 3, lower part of the core; 4, joint seam; 5, raised structure. DETAILED DESCRIPTION

[0039] In order to clearly illustrate the technical features of the present solution, the present invention is described in detail below through specific implementation methods and in conjunction with the accompanying drawings. The disclosure below provides many different embodiments or examples for realizing different structures of the present invention. In order to simplify the disclosure of the present invention, the components and settings of specific examples are described below. In addition, the present invention may repeat reference numbers and / or letters in different examples. This repetition is for the purpose of simplification and clarity, and does not itself indicate the relationship between the various embodiments and / or settings discussed. It should be noted that the components illustrated in the accompanying drawings are not necessarily drawn to scale. The present invention omits the description of known components and processing techniques and processes to avoid unnecessary limitations on the present invention.

[0040] The following examples are further illustrative of the invention, but the invention is not limited thereto. The magnesium spinel castable, recycled granular material of waste magnesium carbon bricks, and recycled magnesium carbon coating used in the examples are produced by existing technology. Other raw materials are commercially available products:

[0041] The sintered magnesia is produced by using light-burned magnesia with a MgO content of 95wt% as raw material through processes such as ball pressing and high-temperature vertical kiln calcination, and the MgO content percentage is 94-95wt%.

[0042] The light-burned magnesium oxide powder has a MgO content of ≥92wt% and a particle size of 325 meshes.

[0043] The silicon powder is a byproduct of producing metallic silicon or ferrosilicon alloy; the SiO2 content in the silicon ash is ≥92wt%, the particle size is all less than 5μm, and the particle size less than 2μm accounts for 80-85%.

[0044] The α-AI2O3 micropowder has an AI2O3 content of ≥99.5wt% and a particle size of 325 meshes.

[0045] The silicon powder has a purity Si content of ≥97wt% and has two particle sizes: 100 mesh and 200 mesh.

[0046] The grade of calcium aluminate cement is CA-70. The specific indicators of pure calcium aluminate cement with the grade of CA-70 are as follows: AI2O3 68.5-71.5%; CaO 26.5-30.5%; SiO2 ≤ 0.5%; Fe2O3 ≤ 0.5%; specific surface area (cm 2 / g)≥5000; initial setting time (min)≥150; final setting (h)≤6; 24h curing strength (MPa) flexural strength (MPa)≥5, compressive strength (MPa)≥40, refractoriness (℃)1680. The testing standard is GB201-2000.

[0047] The explosion-proof fiber is made of modified polypropylene fiber, and has the characteristics of good dispersibility, no sintering, no twisting, little residue, good use effect, etc. It is an excellent explosion-proof additive for various amorphous refractory materials, especially high-strength and fast-drying amorphous refractory materials. Length L = 6mm, phase diameter D = 0.048mm, melting point 165 ~ 175 ℃.

[0048] The flake graphite has a purity C content of ≥98wt% and a particle size of 100 meshes.

[0049] The aluminum powder has a purity AI content of ≥99wt% and a particle size of 100 meshes.

[0050] The silicon carbide powder has a purity SiC content of ≥94wt% and a particle size of 100 meshes.

[0051] The phenolic resin has a solid content of ≥72wt%, a residual carbon content of ≥42wt%, and a moisture content of ≤5wt%.

[0052] Embodiment 1:

[0053] like Figure 1 , Figure 2 As shown, a combined slab continuous casting tundish turbulence controller is composed of an outer shell 1, an upper core 2 and a lower core 3. The upper core 2 and the lower core 3 are designed as a whole and formed separately. The lower core 3 is positioned above the bottom of the inner cavity of the outer shell 1, and the bottom of the inner core 2 of the upper core 2 is positioned above the lower core 3. The longitudinal center lines of the upper core 2 and the lower core 3 coincide with the longitudinal center line of the inner cavity of the outer shell 1. A joint seam 4 is provided between the outer shell 1 and the upper core 2 and the lower core 3. The shape of the inner cavity formed by the upper core 2 and the lower core 3 is designed based on the numerical simulation research and application test of the slab tundish. A protruding structure 5 is provided at the bottom of the inner cavity of the lower core 3, which deviates from the center of the turbulence controller and the casting center of the ladle. The upper core 2 is cast by using a disposable foam inner mold and recycled magnesium-carbon castable, and the lower core 3 is a magnesium-carbon preform prepared by isostatic pressing.

[0054] The outer shape of the core upper part 2 of the turbulence controller is a truncated cone with a large upper bottom surface and a small lower bottom surface, the height a of the outer truncated cone is 300 mm, the circular diameter D1 of the upper bottom surface of the outer truncated cone is 720 mm, and the circular diameter D2 of the lower bottom surface of the outer truncated cone is 665 mm. The inner cavity of the core upper part 2 is a truncated cone with a small upper bottom surface and a large lower bottom surface, the upper bottom circular surface diameter d1 of the inner truncated cone is 450 mm, and the lower bottom circular surface diameter d2 of the inner truncated cone is 510 mm.

[0055] The outer shape of the lower part 3 of the core of the turbulence controller is a truncated cone with a large upper bottom surface and a small lower bottom surface, and the height b of the truncated cone is 190 mm, the upper bottom surface circle diameter D2 of the outer truncated cone is 665 mm, and the lower bottom surface circle diameter D3 of the outer truncated cone is 630 mm. The inner cavity bottom of the lower part 3 of the core is a circular arc surface, and the bottom surface circle diameter d3 of the inner cavity is 528 mm. The thickness c of the inner cavity bottom plane is 100 mm. A protruding structure 5 is set at a point 97.5 mm away from the center of the bottom plane circle. The distance y between the protruding structure 5 and the casting center line of the large ladle injection flow is 20 mm. The protruding structure 5 is in the shape of a truncated cone, formed at the top of the interception height 20 mm, and the bottom surface circle diameter d of the cone is 200 mm, and the height h is 200 mm. The radius R of the curved surface connecting the inner cavity side wall of the lower part 3 of the core sleeve and the inner cavity bottom circle is 80 mm, and the radius r of the curved surface connecting the inner cavity bottom plane circle of the lower part 3 of the core sleeve and the conical bottom circle is 50 mm.

[0056] The width of the joint seam 4 is larger at the top and smaller at the bottom, with the upper width m being 15 mm and the lower width n being 10 mm.

[0057] The shape and size of the shell 1 are designed according to the shape and size of the impact zone of the working lining of the tundish for continuous casting of special-shaped blanks, and are cast by using magnesium spinel castable produced by existing technology, and are prepared by natural curing and baking in a heating furnace.

[0058] The upper part 2 of the core sleeve is cast by adopting recycled magnesium carbon castable. The recycled magnesium carbon castable for the upper part 2 of the core sleeve is composed of the following materials by weight percentage: 25% recycled granular material of waste magnesium carbon brick with a particle size of 3mm≦<5mm, 25% recycled granular material of waste magnesium carbon brick with a particle size of 1mm≦<3mm, 20% recycled granular material of waste magnesium carbon brick with a particle size of 0.074mm≦<1mm, 5% sintered magnesia sand with a particle size of 0.074mm≦<1mm, 10% sintered magnesia sand with a particle size of 0.074mm≦≦0.074mm, 3.0% light-burned magnesia powder with a particle size of 0.045mm, 4% silica powder, 1.5% silica powder, 3.0% α-AI2O3 powder, 3.2% pure calcium aluminate cement, 0.2% sodium tripolyphosphate, and 0.1% explosion-proof fiber.

[0059] The preparation method of the core upper part 2 casted by regenerated magnesium carbon castable comprises the following steps: adding the regenerated magnesium carbon castable for the core upper part 2 into a mixer and dry mixing for 2 minutes, adding 7.2% of the total weight of the material water, wet mixing for 6 minutes, putting into the casting film of the core upper part after mixing, vibrating with a vibrating rod, and when no large bubbles emerge, the casting of the green body of the core upper part 2 is completed, and the casting film of the core upper part is removed after solidification for 12 hours, and naturally cured for 12 hours, and then baked in a heating furnace: ① heating from room temperature to 120℃ at a heating rate of 10℃ / h; ② keeping warm at 120℃ for 8h; ③ heating from 10℃ / h to 200℃; ④ keeping warm at 200℃ for 24h; ⑤ stopping the fire, cooling naturally to room temperature, and the preparation of the core upper part 2 is completed.

[0060] The core lower part 3 is prepared by isostatic pressing and is made of the following raw materials in percentage by weight:

[0061] Main material: 84wt% sintered magnesia mixed with 1mm≦particle size≤3mm, 0.074mm<particle size<1mm, and particle size≦0.074mm

[0062] Auxiliary materials: flake graphite 10.5wt%

[0063] Antioxidant: Aluminum powder 2.0wt%

[0064] Binder: 3.5wt% phenolic resin.

[0065] The core lower part 3 is prepared by isostatic pressing, which includes the following steps:

[0066] 1) Ingredients: weigh the above raw materials according to the above ratio;

[0067] 2) Mixing: preheat the mixer to 40°C, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm at low speed, add phenolic resin after dry mixing for 1 minute, add flake graphite after wet mixing for 3 minutes, add sintered magnesia with a particle size of ≤0.074mm and antioxidant after wet mixing for 2 minutes, wet mix for 3 minutes, mix at high speed for 10 minutes, and discharge. The mud temperature is less than 70°C during the mixing process;

[0068] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 200MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;

[0069] 4) Natural drying and baking: After the green body is naturally dried for 8 hours, it is put into the kiln for baking: ① heat it from room temperature to 140℃ at a heating rate of 10℃ / h and keep it warm for 8 hours; ② heat it from room temperature to 200℃ at a heating rate of 10℃ / h and keep it warm for 24 hours; ③ stop the fire, cool it naturally to room temperature and then take it out of the kiln. The preparation of the lower part 3 of the core sleeve is completed, and its compressive strength is ≥40MPa.

[0070] A preparation method for a combined slab continuous casting tundish turbulence controller comprises the following steps: sequentially inserting a sleeve core lower part 3 and a sleeve core upper part 2 into a shell 1 of the turbulence controller from bottom to top, ensuring that the longitudinal center lines of the sleeve core lower part 3 and the sleeve core upper part 2 coincide with the longitudinal center line of the inner cavity of the shell 1, filling a joint 4 between the shell 1 and the sleeve core lower part 3 and the sleeve core upper part 2 with sintered magnesia sand with a particle size of ≤1mm, and applying a layer of recycled magnesia carbonaceous coating material with a thickness of 35mm on the outer surface thereof, and naturally curing for 2 days, thereby completing the preparation of the combined slab continuous casting tundish turbulence controller.

[0071] Embodiment 2:

[0072] As described in Example 1, except that:

[0073] The cone height a of the upper core part 2 of the turbulence controller is 290 mm, the upper bottom diameter D1 of the outer cone is 710 mm, the lower bottom diameter D2 of the outer cone is 650 mm, the upper bottom diameter d1 of the inner cone of the inner cavity is 440 mm, and the lower bottom diameter d2 of the inner cone is 500 mm.

[0074] The height b of the truncated cone of the lower core part 3 of the turbulence controller is 180mm, the upper bottom circle diameter D2 of the outer truncated cone is 650mm, the lower bottom circle diameter D3 of the outer truncated cone is 620mm, the inner cavity bottom of the lower core part 3 is a circular arc surface, the diameter d3 of the inner cavity bottom circle is 518mm, the thickness c of the inner cavity bottom plane is 80mm, and a protruding structure 5 is set at a point 97mm away from the center of the bottom plane circle, and the distance y between the protruding structure 5 and the casting center line of the large ladle injection flow is 15mm. The protruding structure 5 is in the shape of a truncated cone, formed at the top of the interception height of 20mm, the bottom circle diameter d of the cone is 190mm, and the height h is 190mm. The radius R of the curved surface connecting the inner cavity side wall of the lower part 3 of the core sleeve and the inner cavity bottom circle is 75 mm, and the radius r of the curved surface connecting the inner cavity bottom plane circle of the lower part 3 of the core sleeve and the conical bottom circle is 45 mm.

[0075] The upper width m of the joint seam 4 is 10 mm, and the lower width n is 5 mm.

[0076] The upper part 2 of the core sleeve is cast by adopting recycled magnesium carbon castable. The recycled magnesium carbon castable for the upper part 2 of the core sleeve is composed of the following materials by weight percentage: 20% recycled granular material of waste magnesium carbon brick with a particle size of 3mm≦<5mm, 22% recycled granular material of waste magnesium carbon brick with a particle size of 1mm≦<3mm, 20% recycled granular material of waste magnesium carbon brick with a particle size of 0.074mm≦<1mm, 5% sintered magnesia sand with a particle size of 3mm≦<5mm, 5% sintered magnesia sand with a particle size of 1mm≦<3mm, 13% sintered magnesia sand with a particle size of ≦0.074mm, 5.0% light-burned magnesia powder with a particle size of ≦0.045mm, 2% silica powder, 2.0% silica powder, 5.0% α-AI2O3 powder, 3.8% pure calcium aluminate cement, 0.15% sodium tripolyphosphate, and 0.05% explosion-proof fiber.

[0077] The preparation method of the core sleeve upper part 2 is cast by using recycled magnesium carbon castable, which comprises the following steps: adding the recycled magnesium carbon castable for the core sleeve 2 into a mixer and dry mixing for 3 minutes, adding water of 6.7% of the total weight of the material, wet mixing for 6 minutes, putting it into the casting film of the core sleeve upper part after mixing, vibrating it with a vibrating rod, and when no large bubbles emerge, the casting of the green body of the core sleeve 2 is completed, and the casting film of the core sleeve upper part is removed after solidification for 24 hours, and naturally cured for 24 hours, and then baked in a heating furnace: ① heating from room temperature to 150℃ at a heating rate of 10℃ / h; ② keeping warm at 150℃ for 12h; ③ heating from 10℃ / h to 220℃; ④ keeping warm at 220℃ for 16h; ⑤ stopping the fire, cooling naturally to room temperature, and the preparation of the core sleeve upper part 2 is completed.

[0078] The core lower part 3 is prepared by isostatic pressing and is made of the following raw materials in percentage by weight:

[0079] Main material: 76wt% sintered magnesia mixed with 1mm≦particle size≤3mm, 0.074mm<particle size<1mm, and particle size≦0.074mm

[0080] Auxiliary materials: flake graphite 16wt%

[0081] Antioxidant: Silicon powder 2wt%, Silicon carbide powder 2wt%

[0082] Binder: 4.0wt% phenolic resin.

[0083] The core lower part 3 is prepared by isostatic pressing, which includes the following steps:

[0084] 1) Ingredients: weigh the above raw materials according to the above ratio;

[0085] 2) Mixing: preheat the mixer to 50°C, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm at low speed, add phenolic resin after dry mixing for 2 minutes, add flake graphite after wet mixing for 2 minutes, add sintered magnesia with a particle size of ≤0.074mm and antioxidant after wet mixing for 3 minutes, wet mix for 2 minutes, mix at high speed for 15 minutes, and discharge. During the mixing process, the temperature of the mud is less than 70°C;

[0086] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 250MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;

[0087] 4) Natural drying and baking: After the green body is naturally dried for 16 hours, it is put into the kiln for baking: ① heat up from room temperature to 160℃ at a heating rate of 10℃ / h and keep warm for 4 hours; ② heat up from room temperature to 220℃ at a heating rate of 10℃ / h and keep warm for 16 hours; ③ stop the fire, cool naturally to room temperature and then take out of the kiln. The preparation of the lower part 3 of the core sleeve is completed, and its compressive strength is ≥40MPa.

[0088] A preparation method for a combined slab continuous casting tundish turbulence controller comprises the following steps: sequentially inserting a sleeve core lower part 3 and a sleeve core upper part 2 into a shell 1 of the turbulence controller from bottom to top, ensuring that the longitudinal center lines of the sleeve core lower part 3 and the sleeve core upper part 2 coincide with the longitudinal center line of the inner cavity of the shell 1, filling a joint seam 4 between the shell 1 and the sleeve core lower part 3 and the sleeve core upper part 2 with sintered magnesia sand with a particle size of ≤1mm, and applying a layer of recycled magnesia carbonaceous coating material with a thickness of 25mm on the outer surface thereof, and naturally curing for 1 day, thereby completing the preparation of the combined slab continuous casting tundish turbulence controller.

[0089] Embodiment 3:

[0090] As described in Example 1, except that:

[0091] The cone height a of the upper core part 2 of the turbulence controller is 310 mm, the upper bottom diameter D1 of the outer cone is 730 mm, the lower bottom diameter D2 of the outer cone is 680 mm, the upper bottom diameter d1 of the inner cone of the inner cavity is 460 mm, and the lower bottom diameter d2 of the inner cone is 520 mm.

[0092] The height b of the truncated cone of the lower core part 3 of the turbulence controller is 200mm, the upper bottom circle diameter D2 of the outer truncated cone is 680mm, the lower bottom circle diameter D3 of the outer truncated cone is 640mm, the inner cavity bottom of the lower core part 3 is a circular arc surface, the diameter d3 of the inner cavity bottom circle is 538mm, the thickness c of the inner cavity bottom plane is 90mm, and a protruding structure 5 is set at a point 98mm away from the center of the bottom plane circle, and the distance y between the protruding structure 5 and the casting center line of the large ladle injection flow is 25mm. The protruding structure 5 is in the shape of a truncated cone, formed at the top of the interception height of 20mm, the bottom circle diameter d of the cone is 210mm, and the height h is 210mm. The radius R of the curved surface connecting the inner cavity side wall of the lower part 3 of the core sleeve and the inner cavity bottom circle is 85 mm, and the radius r of the curved surface connecting the inner cavity bottom plane circle of the lower part 3 of the core sleeve and the conical bottom circle is 55 mm.

[0093] The upper width m of the joint seam 4 is 10 mm, and the lower width n is 5 mm.

[0094] The upper part 2 of the core sleeve is cast by adopting recycled magnesium carbon castable. The recycled magnesium carbon castable for the upper part 2 of the core sleeve is composed of the following materials by weight percentage: 22% recycled granular material of waste magnesium carbon brick with a particle size of 3mm≦<5mm, 23% recycled granular material of waste magnesium carbon brick with a particle size of 1mm≦<3mm, 15% recycled granular material of waste magnesium carbon brick with a particle size of 0.074mm≦<1mm, 5% sintered magnesia with a particle size of 1mm≦<3mm, 7% sintered magnesia with a particle size of 0.074mm≦<1mm, 12% sintered magnesia with a particle size of ≦0.074mm, 4.0% light-burned magnesia powder with a particle size of ≦0.045mm, 3% silica powder, 1.25% silica powder, 4.0% α-AI2O3 powder, 3.5% pure calcium aluminate cement, 0.17% sodium tripolyphosphate, and 0.08% explosion-proof fiber.

[0095] The preparation method of the core sleeve upper part 2 by casting with recycled magnesium carbon casting material comprises the following steps: adding the recycled magnesium carbon casting material for the core sleeve 2 into a mixer and dry mixing for 2 minutes, adding water of 7.0% of the total weight of the material, wet mixing for 5 minutes, putting into the casting film of the core sleeve upper part after mixing, vibrating with a vibrating rod, and when no large bubbles emerge, the green casting of the core sleeve upper part 2 is completed, and the casting film of the core sleeve upper part is removed after solidification for 16 hours, and naturally cured for 16 hours, and then baked in a heating furnace: ① heating from room temperature to 135℃ at a heating rate of 10℃ / h; ② keeping warm at 135℃ for 10h; ③ heating from 10℃ / h to 210℃; ④ keeping warm at 210℃ for 20h; ⑤ stopping the fire, cooling naturally to room temperature, and the preparation of the core sleeve upper part 2 is completed.

[0096] The core lower part 3 is prepared by isostatic pressing and is made of the following raw materials in percentage by weight:

[0097] Main material: 79wt% sintered magnesia mixed with 1mm≦particle size≤3mm, 0.074mm<particle size<1mm, and particle size≦0.074mm

[0098] Auxiliary materials: flake graphite 14wt%

[0099] Antioxidant: Aluminum-magnesium alloy powder 3.3wt%

[0100] Binder: 3.7wt% phenolic resin.

[0101] The core lower part 3 is prepared by isostatic pressing, which includes the following steps:

[0102] 1) Ingredients: weigh the above raw materials according to the above ratio;

[0103] 2) Mixing: preheat the mixer to 45°C, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm at low speed, add phenolic resin after dry mixing for 1 minute, add flake graphite after wet mixing for 3 minutes, add sintered magnesia with a particle size of ≤0.074mm and antioxidant after wet mixing for 3 minutes, wet mix for 2 minutes, mix at high speed for 10 minutes, and discharge. During the mixing process, the temperature of the mud material is less than 70°C;

[0104] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 220MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;

[0105] 4) Natural drying and baking: After the green body is naturally dried for 12 hours, it is put into the kiln for baking: ① heat up from room temperature to 150℃ at a heating rate of 10℃ / h and keep warm for 6 hours; ② heat up from room temperature to 210℃ at a heating rate of 10℃ / h and keep warm for 20 hours; ③ stop the fire, cool naturally to room temperature and then take out of the kiln. The preparation of the lower part 3 of the core sleeve is completed, and its compressive strength is ≥40MPa.

[0106] A preparation method for a combined slab continuous casting tundish turbulence controller comprises the following steps: sequentially inserting a sleeve core lower part 3 and a sleeve core upper part 2 into a shell 1 of the turbulence controller from bottom to top, ensuring that the longitudinal center lines of the sleeve core lower part 3 and the sleeve core upper part 2 coincide with the longitudinal center line of the inner cavity of the shell 1, filling a joint seam 4 between the shell 1 and the sleeve core lower part 3 and the sleeve core upper part 2 with sintered magnesia sand with a particle size of ≤1mm, and applying a layer of recycled magnesia carbonaceous coating material with a thickness of 30mm on the outer surface thereof, and naturally curing for 2 days, thereby completing the preparation of the combined slab continuous casting tundish turbulence controller.

[0107] Comparative Example 1: CN201244677B discloses a preparation method for a composite turbulence controller for a continuous casting tundish, including an outer shell, a bottom plate, a core sleeve, an expansion joint, and an anti-oxidation coating. The outer shell is cast by using a magnesium castable, the bottom plate is built by using machine-pressed magnesium-carbon bricks, and the core sleeve is built by using machine-pressed "fan-shaped" magnesium-carbon bricks. Expansion joints are arranged between the outer shell and the bottom plate, and between the outer shell and the core sleeve, and an anti-oxidation coating is applied to the outer surface of the core sleeve.

[0108] The structural materials, service life, slag entrainment in the impact zone of the tundish injection flow, and total oxygen content in the molten steel in the crystallizer (comparison test steel grade SPHC) of the embodiments 1-3 of the present invention and the comparative document CN201244677B, which discloses a method for preparing a composite turbulence controller for a continuous casting tundish, are compared in the application test of the slab continuous casting tundish of Laiwu Iron and Steel Group Yinshan Steel Co., Ltd., as shown in the following table:

[0109]

[0110] By comparing the data in Table 1 above, the service life of the combined slab continuous casting tundish turbulence controller prepared by the present invention is more than 4 hours longer than that of the composite turbulence controller produced by the existing patent technology CN103658577B, the total oxygen content in the molten steel in the crystallizer is reduced by more than 11% year-on-year, the production cost is reduced by more than 32% year-on-year, and the problem of slag entanglement in the impact zone of the tundish is effectively solved.

[0111] Although the above describes the specific implementation mode of the invention in conjunction with the drawings, it is not intended to limit the scope of protection of the invention. Based on the technical solution of the present invention, various modifications or variations that can be made by those skilled in the art without creative work are still within the scope of protection of the present invention.

Claims

1. A combined slab continuous casting tundish turbulence controller, comprising a shell (1) and a sleeve core, wherein the sleeve core is arranged in the inner cavity of the shell, characterized in that: The core sleeve comprises a core upper portion (2) and a core lower portion (3) arranged in a vertical direction. The core lower portion (3) is arranged on the bottom surface of the inner cavity of the shell (1), and the longitudinal center lines of the core upper portion (2) and the core lower portion (3) coincide with the longitudinal center line of the inner cavity of the shell (1). A joint seam (4) is provided between the side walls of the shell (1) and the core sleeve. The width of the joint seam is larger at the upper portion and smaller at the lower portion, which effectively prevents the problem of steel penetration from the joint seam from top to bottom. The inner cavity bottom of the core lower portion (3) is provided with a protruding structure (5) deviating from the longitudinal center line of the inner cavity of the core sleeve and the ladle casting center. The protruding structure is truncated cone-shaped. The bottom surface of the inner cavity of the lower part (3) of the sleeve core is a circular arc curved surface, and the inner cavity side wall and the bottom surface of the lower part (3) of the sleeve core are transitioned through a circular arc chamfer.

2. A combined slab continuous casting tundish turbulence controller as claimed in claim 1, characterized in that: The inner cavity of the upper part (2) of the sleeve core is in the shape of a truncated cone with a small inner diameter at the upper part and a large inner cavity at the lower part; The height a of the upper part (2) of the sleeve core is 290-320 mm, the inner diameter d1 of the upper bottom surface is 440-460 mm, and the inner diameter d2 of the lower bottom surface is 500-520 mm.

3. A combined slab continuous casting tundish turbulence controller as claimed in claim 2, characterized in that: The outer shape of the upper part (2) of the sleeve core is a truncated cone with a large upper bottom surface and a small lower bottom surface, and the outer shape of the lower part (3) of the sleeve core is a truncated cone with a large upper bottom surface and a small lower bottom surface.

4. The combined slab continuous casting tundish turbulence controller according to claim 1, characterized in that: The shape of the protruding structure is a truncated cone formed by cutting off a 20 mm high top of a cone, and the bottom circle diameter d of the cone is 190 to 210 mm, and the height h is 190 to 210 mm.

5. The combined slab continuous casting tundish turbulence controller according to claim 1, characterized in that: The upper width m of the joining seam (4) is 10 to 15 mm, and the lower width n is 5 to 10 mm.

6. A method for preparing the combined slab continuous casting tundish turbulence controller according to claim 1, wherein the shell (1) is casted with magnesium spinel castable material, and is prepared by natural curing and baking in a heating furnace, characterized in that: The following steps are involved: The lower part (3) and the upper part (2) of the core sleeve are sequentially mounted in the outer shell (1) of the turbulence controller from bottom to top, ensuring that the longitudinal center lines of the lower part (3) and the upper part (2) of the core sleeve coincide with the longitudinal center line of the inner cavity of the outer shell (1), the joint seam (4) between the outer shell (1) and the lower part (3) and the upper part (2) of the core sleeve is filled with sintered magnesia sand with a particle size of ≤1 mm, and a layer of recycled magnesia carbonaceous coating material with a thickness of 25 to 35 mm is applied to the outer surface of the sintered magnesia sand, and naturally cured for 1 to 2 days, and the combined slab continuous casting tundish turbulence controller is prepared; The upper part of the sleeve core (2) is casted by recycled magnesium carbon casting material, and the raw material composition of the recycled magnesium carbon casting material is: 20-25% recycled granular material of waste magnesium carbon brick with a particle size of 3mm≦<5mm, 22-25% recycled granular material of waste magnesium carbon brick with a particle size of 1mm≦<3mm, 15-20% recycled granular material of waste magnesium carbon brick with a particle size of 0.074mm≦<1mm, 0-5% sintered magnesia sand with a particle size of 3mm≦<5mm, and 0-5% sintered magnesia sand with a particle size of 1mm≦<3mm. , 0.074mm≦sintered magnesia with a particle size of <1mm 0~7%, sintered magnesia with a particle size of ≦0.074mm 10~13%, light-burned magnesia powder with a particle size of ≦0.045mm 3.0~5.0%, silica powder with a particle size of 200 mesh 2~4%, silica powder 1.0~1.5%, active α-Al2O3 powder 3.0~5.0%, pure calcium aluminate cement 3.2~3.8%, sodium tripolyphosphate 0.15~0.2%, explosion-proof fiber 0.05~0.1%; The core lower part (3) is prepared by isostatic pressing, and the raw material composition of the core lower part (3) is: Main material: 76-84wt% sintered magnesia mixed with 1mm≦particle size≤3mm, 0.074mm<particle size<1mm, and particle size≦0.074mm. Auxiliary materials: flake graphite 11.5~16wt%, Antioxidant: 2-5wt% of one or a mixture of aluminum powder, silicon powder, silicon carbide powder, all with a particle size of 100 meshes, Binder: 3.5-4.0wt% of phenolic resin, the weight percentage of all raw materials added up to 100%.

7. The method for preparing a combined slab continuous casting tundish turbulence controller according to claim 6, characterized in that: The method for preparing the core upper part (2) comprises the following steps: 1) adding the raw materials of the regenerated magnesium carbon castable into a mixer and dry mixing for 2 to 3 minutes; 2) Add 6.7-7.2% water of the total weight of the material and wet mix for 4-6 minutes: 3) After mixing, put it into the casting membrane on the upper part of the core and vibrate it with a vibrating rod. When no large bubbles emerge, the green casting of the upper part of the core (2) is completed; 4) After solidification for 12 to 24 hours, remove the cast fetal membrane on the top of the core and allow it to cure naturally for 12 to 24 hours; 5) Baking in a heating furnace: ① Raise the temperature from room temperature to 120-150°C at a rate of 10°C / h; ② Keep at 120-150°C for 8-12h; ③ Raise the temperature again to 200-220°C at a rate of 10°C / h; ④ Keep at 200-220°C for 16-24h; ⑤ Stop heating and cool naturally to room temperature. The upper part of the core sleeve (2) is now ready.

8. The method for preparing a combined slab continuous casting tundish turbulence controller according to claim 6, characterized in that: The preparation method of the core lower part (3) comprises the following steps: 1) Ingredients: weigh the raw materials of the lower part of the core (3) according to the above-mentioned proportions; 2) Mixing: preheat the mixer to 40-50°C, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm at low speed, add phenolic resin after dry mixing for 1-2 minutes, add flake graphite after wet mixing for 2-3 minutes, add sintered magnesia with a particle size of ≤0.074mm and antioxidant after wet mixing for 2-3 minutes, wet mix for 2-3 minutes, mix at high speed for 10-15 minutes, and discharge. During the mixing process, the mud temperature is less than 70°C; 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 200-250MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed; 4) Natural drying and baking: After the green body is naturally dried for 8 to 16 hours, it is put into the kiln for baking: ① heating from room temperature to 140 to 160°C at a heating rate of 10°C / h, and keeping warm for 4 to 8 hours; ② heating from room temperature to 200 to 220°C at a heating rate of 10°C / h, and keeping warm for 16 to 24 hours; ③ stopping the fire, cooling naturally to room temperature, and then taking out of the kiln. The preparation of the lower part of the core sleeve (3) is completed.

9. The method for preparing a combined slab continuous casting tundish turbulence controller according to claim 6, characterized in that: The regenerated magnesium carbon coating material is a coating material prepared by treating and processing waste magnesium carbon bricks with a particle size of 1mm≦≤3mm and a particle size of 0.074mm<<1mm, and sintered magnesium sand fine powder with a particle size of ≤0.074mm, soft clay, silicon powder, and sodium tripolyphosphate, wherein the weight percentage of the regenerated magnesium carbon particles is 60-70%, the MgO content is ≥65wt%, and the volume density is ≥1.87g / cm 3 .