A nuclear main pump test bench main circuit and its inner wall surfacing and circumferential seam butt welding method
By using WB36 alloy steel inner wall surfacing stainless steel and nickel-based alloy layers in the main circuit system of the nuclear main pump test bench, and performing ring-slit butt welding technology, the problems of high weight and cost of all stainless steel pipes are solved, and mechanical performance optimization is achieved and cleanliness guarantee, meeting high-pressure test and water quality standards.
Patent Information
- Application Number
- CN202010026141.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-01-10
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-01-10
AI Technical Summary
The main circuit system of the existing nuclear main pump test bench uses all stainless steel pipes, which leads to increased weight and high cost. At the same time, there is a problem of media corrosion when using WB36 material, which requires frequent passivation treatment, which increases time and cost.
WB36 alloy steel is used as the main pipe material, the inner wall is surfacing 309MoL stainless steel and 347 stainless steel layers, and the nickel-based alloy layer is surfacing on the inner wall of the elbow. Through the ring seam butt welding technology of the multi-layer nickel-based alloy layer, combining argon arc welding and Heat treatment achieves optimization of the mechanical and thermodynamic performance of the pipeline.
It reduces the weight and cost of the pipeline system, improves mechanical properties, simplifies supporting equipment, ensures pipeline cleanliness and welding quality, and passes high-pressure tests and water quality inspections, meeting the Class A water standard.
Smart Images

Figure CN111151845B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a main circuit of a nuclear main pump test bench and an inner wall surfacing welding and annular seam butt welding method thereof, and is mainly used in the main circuit of a CAP1400 nuclear main pump test bench. Background Art
[0002] my country's nuclear power technology is constantly developing. It has digested and innovated the AP1000 technology to form my country's third-generation nuclear power technology CAP1400 with completely independent intellectual property rights. The design and construction of the CAP1400 nuclear main pump test bench is a complex technical task, among which the design of the test loop system is particularly important. Figure 1 and Figure 2 As shown, it includes a main pipeline, a main pump casing 5, a main flow meter 6, and a main regulating valve 7. The main pipeline includes four types of components: a straight pipe 1, an elbow 2, a tee 3, and a reducer 4. The main pump casing 5, the main flow meter 6, and the main regulating valve 7 are welded and fixed to the main pipeline, and the straight pipe 1, the elbow 2, the tee 3, and the reducer 4 are welded and fixed together. The main pipeline takes the nuclear main pump as the base point to form a closed-loop test circuit. The main pipeline is divided into two paths by a tee 3 at the outlet of the nuclear pump, and merged into one path after passing through two groups of main regulating valves 7 and a tee 3. In the second-layer flow measurement section, the main pipeline is divided into two paths by a tee 3 again, and merged into one pipeline after passing through two groups of main flow meters 6, and connected to the inlet of the nuclear pump to form a complete main pipeline system. The main specifications of the pipeline are DN800~DN1000, and the pipeline wall thickness varies from 40 to 112 mm.
[0003] Due to the high temperature and high pressure characteristics of the test bench and the need for pipeline cleaning, the part of the test loop that contacts the medium must be made of stainless steel. Due to the large thickness of stainless steel pipes, if all stainless steel is used, the weight of the main pipeline will almost double, and the cost of stainless steel pipes is too high, and the investment in the pipeline system will increase greatly. At present, there is also a solution that the material of the main pipeline is WB36. WB36 has very high yield and tensile strength values. The mechanical properties of WB36 at room temperature have a minimum yield strength of 440MPa and a tensile strength of 610~780MPa. The mechanical properties are very consistent with the design requirements of the main loop of the test bench. However, if the test main pipeline is all made of WB36, deionized water as the test medium will cause corrosion to the pipeline and cause medium pollution. In order to prevent damage to the tested nuclear power main pump, the test loop needs to be passivated after the medium is emptied with water for a period of time. Each passivation takes 3 weeks. Although the cost is reduced compared to stainless steel pipes, the passivation cost and the time cost caused by the time consumed are also very large.
[0004] A Chinese patent application numbered 2016100320935 also discloses a similar nuclear power main pump test device, in which the main loop pipe is made of WB36 material, and stainless steel is welded inside the main loop pipe. However, the specific welding structure and welding method are not disclosed. Summary of the invention
[0005] The purpose of the present invention is to overcome the above-mentioned deficiencies in the prior art and to provide a nuclear main pump test bench main circuit with a reasonable structural design and a method for surfacing welding the inner wall and butt welding the circumferential seam, which is low in cost and enables the pipeline to have good mechanical and thermodynamic properties.
[0006] The technical solution adopted by the present invention to solve the above problems is: a main circuit of a nuclear main pump test bench, including a main pipeline, a main pump casing, a main flow meter and a main regulating valve. The main pipeline is made of WB36 alloy steel, which includes four types of components: straight pipes, elbows, tees and reducers. The main pump casing, the main flow meter and the main regulating valve are welded and fixed to the main pipeline, and the straight pipes, elbows, tees and reducers are welded and fixed together; it is characterized in that: a layer of 3 is welded on the inner walls of the three pipe fittings: the straight pipe, the tee and the reducer. 09MoL stainless steel layer as a transition layer, and a layer of 347 stainless steel layer is welded on the transition layer as a surface layer; a layer of nickel-based alloy is welded on the inner wall of the elbow as a surface layer; among the four components of straight pipe, elbow, tee and reducer, the inner wall cladding layers of the two components welded together are all stainless steel, and a layer of 309MoL stainless steel layer is welded on the inner wall weld as a transition layer, and one or more layers of 347 stainless steel are welded on the transition layer as a surface layer; the cladding layers of the two components welded together There is a nickel-based alloy layer in it, and a nickel-based alloy layer is welded on the inner wall weld as a transition layer, and one or more nickel-based alloy layers are welded on the transition layer as a surface layer; the weld between the main pipeline and the main pump casing is divided into two layers, the first layer is a nickel-based alloy layer, which is welded on the main pipeline butt joint surface, and the other layer is also a nickel-based alloy layer, which is located between the first nickel-based alloy layer and the main pump casing butt joint surface; the weld between the main pipeline and the main flowmeter is divided into two layers, the first layer is a nickel-based alloy layer, A nickel-based alloy layer is welded on the main pipeline butt joint surface, and another layer is also a nickel-based alloy layer, which is located between the first nickel-based alloy layer and the main flowmeter butt joint surface; the weld between the main pipeline and the main regulating valve is divided into three layers, the first layer is a nickel-based alloy layer, which is welded on the main pipeline butt joint surface, the second layer is also a nickel-based alloy layer, which is welded on the main regulating valve butt joint surface, and the third layer is also a nickel-based alloy layer, which is located between the first nickel-based alloy layer and the second nickel-based alloy layer.
[0007] The present invention has a boss welded on the main pipeline, and the boss is used to be connected with a high-pressure auxiliary loop pipeline.
[0008] The boss material of the present invention is WB36.
[0009] The surface layer thickness of the inner wall of the elbow described in the present invention is 2.5-3.5 mm.
[0010] The surface layer thickness of the inner wall of the elbow described in the present invention is 3 mm.
[0011] In the inner walls of the three types of pipe fittings, namely the straight pipe, the tee and the reducing joint described in the present invention, the thickness of the transition layer and the surface layer are both 1.6 mm.
[0012] A method for inner wall cladding and girth butt welding of a main circuit of a nuclear main pump test bench, characterized in that it includes the following processes:
[0013] A. Surfacing stainless steel on the inner wall of the main pipeline, the process is:
[0014] 1) The process of cladding stainless steel on the inner wall of three types of pipe fittings, namely straight pipe, tee and reducer, is as follows: (1) rust removal on the inner wall of the pipe fitting; (2) preheating the inner wall of the pipe fitting to 120℃~150℃; (3) cladding a layer of 309MoL stainless steel on the inner wall of the pipe fitting as a transition layer; (4) cooling the transition layer; (5) cladding a layer of 347 stainless steel on the transition layer as a surface layer; (6) grinding the surface layer; (7) heat treatment of the cladding layer; (8) spraying glass beads on the surface of the surface layer;
[0015] 2) The process of cladding stainless steel on the inner wall of the elbow is as follows: (1) rust removal on the inner wall of the elbow; (2) preheating the inner wall of the elbow to 120℃~150℃; (3) cladding a layer of nickel-based alloy on the inner wall of the elbow as the surface layer; (4) cooling the surface layer; (5) grinding the surface layer; (6) heat treatment of the cladding layer; (7) spraying glass beads on the surface of the surface layer;
[0016] B. The main pipeline components and equipment are connected by girth butt welding, the process is as follows;
[0017] 1) Process of circumferential butt welding of main pipeline components: (1) Preheating around the weld to 120℃~150℃; (2) Base welding; (3) Full welding of the weld; (4) Heat treatment of the weld; (5) Grinding of the weld on the inner wall of the pipeline; (6) Preheating of the weld to 120℃~150℃; (7) The weld overlay of the main pipeline components is all stainless steel. A layer of 309MoL stainless steel is welded on the inner wall of the pipeline as a transition layer. After the transition layer cools down, one or more layers of 347 stainless steel are welded on the transition layer as a surface layer; if there is a nickel-based alloy layer in the weld overlay of the main pipeline components, a layer of nickel-based alloy is first welded on the inner wall of the pipeline as a transition layer. After the transition layer cools down, one or more layers of nickel-based alloy are welded on the transition layer as a surface layer; (8) Surface layer cooling; (9) Heat treatment of the weld overlay; (10) Grinding of the weld overlay and weld;
[0018] 2) Circumferential butt welding process between the main pipeline and the main pump casing: The main pump casing butt surface material is austenitic stainless steel 304L. It is necessary to first build up a layer of nickel-based alloy on the main pipeline butt surface, anneal the nickel-based alloy layer at 580-620℃, and then use nickel-based alloy welding materials for circumferential butt welding;
[0019] 3) Circumferential butt welding process between main pipeline and main flowmeter: The main flowmeter butt surface material is austenitic stainless steel 304L. It is necessary to first build up a layer of nickel-based alloy on the main pipeline butt surface, anneal the nickel-based alloy layer at 580-620℃, and then use nickel-based alloy welding materials for circumferential butt welding;
[0020] 4) The process of butt welding the main pipeline and the main regulating valve: The main regulating valve butt surface material is SA351. First, a layer of nickel-based alloy welding materials shall be welded on the main regulating valve butt surface and the main pipeline butt surface respectively. The preheating temperature is 120℃~150℃. After the butt surface welding is completed, the main pipeline welding layer and the main regulating valve welding layer shall be heat treated, and then the main pipeline welding layer and the main regulating valve welding layer shall be butt welded with nickel-based alloy welding materials.
[0021] 5) Circumferential butt welding process between the main pipeline and the high-pressure auxiliary loop pipeline: A boss made of WB36 is provided between the main pipeline and the high-pressure auxiliary loop pipeline. The boss is welded on the main pipeline. When the boss is connected to the high-pressure auxiliary loop pipeline, a layer of nickel-based alloy layer is welded on the butt surface where the boss and the high-pressure auxiliary loop pipeline are connected. After the nickel-based alloy layer is annealed at 580-620℃, the nickel-based alloy welding material is used to perform circumferential butt welding with the high-pressure auxiliary pipeline.
[0022] In the above process B of the present invention, after the butt surfaces of the main pipeline components and equipment are processed before butt welding, circumferential butt welding is performed according to the following process:
[0023] 1) Inspection before jointing: Before jointing, clean the weld until it emits metallic luster; before welding each weld, perform 100% PT or MT inspection on the pipe end, and weld only after passing the inspection;
[0024] 2) Set up argon-filled plugs: During welding, the inside of the weld needs argon protection. To ensure the protection effect and save argon, plugs are set on both sides of the weld. Before the joints are connected, put the argon-filled tool into the pipe. The distance between the two plugs should not be less than 400mm, and they should be evenly distributed on both sides of the groove. Stop filling argon after welding is completed.
[0025] 3) Matching inspection: Before matching, perform PT inspection on the groove surface and inner wall, and only match after confirming that there are no surface defects; when matching welds, make sure that the inner wall is flush, if there is misalignment, the local misalignment value shall not exceed 10% of the wall thickness and shall not exceed 1mm; the matching straightness shall be ≤3 / 200; the matching gap shall be 3-4mm, and if it is too large or too small, it shall be trimmed to the specified size, and no strong matching shall be performed or fillers shall be added in the gap;
[0026] 4) Spot welding of welds: When spot welding of welds, plugs are used to spot weld them in the groove, and the spot welding positions are arranged symmetrically; preheating is performed before spot welding, and the preheating temperature is 200-250℃;
[0027] 5) Preheating: The main pipeline weld should be preheated before welding;
[0028] 6) Argon filling: Argon needs to be filled in the pipe during root welding; when filling argon, the initial flow rate is 10-20L / min. After the argon is full, root welding can be carried out;
[0029] 7) Use argon arc welding for base welding: supply argon gas 1.5 to 4 seconds in advance when striking the arc, and remove the air in the argon gas delivery hose and at the weld; after the arc is extinguished, delay 5 to 15 seconds to extinguish the gas, protect the tungsten electrode and the molten pool that have not yet cooled down, and reduce the degree of oxidation on the weld surface; when welding to the plug, remove the plug and grind the weld joint; the argon arc welding base is at least 2 layers, each layer is 2.8 to 3.2 mm thick;
[0030] 8) Interlayer welding and cover welding: The preheating temperature of interlayer welding and cover welding is 120-150℃; pay attention to the cleaning between layers, and stagger the joints of each layer of welds by 10-15mm during welding; during the interruption of welding, the weld seam should always maintain a temperature of 150-200℃;
[0031] 9) Post-weld heat treatment: After the main pipeline weld is completed, the weld is post-heat treated at a temperature of 330-370°C and kept warm for 3 hours; after the surfacing welding of the inner wall of the main pipeline is completed, the weld is finally heat treated at a temperature of 580-620°C and kept warm for 2 hours;
[0032] 10) Stainless steel cladding on the inner wall of each butt weld:
[0033] After the butt welds of the main pipeline and various components and equipment are completed, the welds on the inner wall of the pipeline need to be clad, and the surface of the cladding layer is polished and smooth: first, the inner wall is polished, and after polishing, the preheating temperature of the inner wall of the pipeline is between 120 and 150°C; the weld cladding layer on the inside of the main pipeline is divided into two parts: a transition layer and a surface layer; the cladding layers of the butt pipe components are all made of stainless steel, a layer of 309MoL stainless steel is clad as a transition layer, and then a layer of 347 stainless steel is clad as a surface layer; if there is a nickel-based alloy layer in the cladding layer of the butt pipe components, first a layer of nickel-based alloy is clad as a transition layer, and then one or more layers of nickel-based alloy are clad on the transition layer as a surface layer.
[0034] In the above process A of the present invention, the tees and reducers are welded by automatic TIG welding, and the straight pipes are welded by automatic MIG welding.
[0035] In the circumferential butt welding process between the main pipeline and the main pump casing, the circumferential butt welding process between the main pipeline and the main flowmeter, and the circumferential butt welding process between the main pipeline and the high-pressure auxiliary loop pipeline, the annealing temperature is 600°C.
[0036] Compared with the prior art, the present invention has the following advantages and effects:
[0037] 1. Based on the characteristics of the two main pipelines in the background technology, the present invention adopts a structure in which the base material is WB36 alloy steel and the inner wall is welded with stainless steel. At the same time, compared with the traditional all-stainless steel pipeline system, the present invention has good comprehensive mechanical properties of its base material, so that the pipeline has good mechanical properties and thermodynamic properties, which not only greatly reduces the weight of the pipeline system, but also reduces the weight of the steel structure accordingly, simplifies the supporting equipment, and reduces the manufacturing cost; at the same time, according to the welding requirements between different materials in the main pipeline, through multiple test welding and process evaluation, for different types of welds, a new butt welding process and structure are adopted to optimize the performance of butt welds of pipelines of different materials.
[0038] 2. By using the present invention, the main pipeline successfully completed the welding connection of WB36 pipeline components with main regulating valves of different specifications and materials, main flowmeters, main pump casings, and high-pressure auxiliary circuit pipelines. Each weld passed 2 UT, 2 MT and 4 PT, and all 8 inspections were qualified, and successfully passed the pressure test of up to 22.9MPa conducted by the main pump casing and the main pipeline system. At the same time, the main pipeline has high internal cleanliness requirements, and no visible particles are required in the pipeline. The water quality test must meet the A-level water standard. The welding process of this technology is efficient and clean, without excess residue splashing, which effectively ensures the cleanliness of the main pipeline loop. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a structural schematic diagram of the test main circuit of the CAP1400 nuclear main pump test bench of the present invention.
[0040] Figure 2 yes Figure 1 Schematic diagram of the structure of direction A.
[0041] Figure 3 It is a structural schematic diagram of the connection between a straight pipe and an elbow of the present invention.
[0042] Figure 4 It is a schematic structural diagram of two straight pipes connected in the present invention.
[0043] Figure 5It is a schematic diagram of the structure of the main pipeline and the high-pressure auxiliary loop pipeline after circumferential butt welding in the present invention.
[0044] Figure 6 It is a structural schematic diagram of the connection of a straight pipe, a reducing joint and a main pump casing of the present invention.
[0045] Figure 7 It is a structural schematic diagram of the connection between the main pipeline and the main flow meter of the present invention.
[0046] Figure 8 It is a structural schematic diagram of the connection between the main pipeline and the main regulating valve of the present invention. DETAILED DESCRIPTION
[0047] The present invention will be further described in detail below with reference to the accompanying drawings and by way of examples. The following examples are intended to explain the present invention but the present invention is not limited to the following examples.
[0048] See also Figure 1-Figure 8 The main circuit system of the CAP1400 nuclear main pump test bench described in this embodiment includes a main pipeline, a main pump casing 5, a main flow meter 6, and a main regulating valve 7. The main pipeline includes four types of components: a straight pipe 1, an elbow 2, a tee 3, and a reducer 4. The main pump casing 5, the main flow meter 6, and the main regulating valve 7 are welded and fixed to the main pipeline. The straight pipe 1, the elbow 2, the tee 3, and the reducer 4 are welded and fixed together to form the main pipeline. The main pipeline is made of WB36 alloy steel.
[0049] A 1.6 mm thick 309MoL stainless steel layer 8 is welded on the inner walls of the three pipe fittings, namely the straight pipe 1, the tee 3 and the reducer 4, as a transition layer, and a 1.6 mm thick 347 stainless steel layer 9 is welded on the transition layer as a surface layer.
[0050] A 2.5-3.5 mm thick nickel-based alloy layer 10 is built-up welded on the inner wall of the elbow 2 as a surface layer.
[0051] Among the four components, namely, the straight pipe 1, the elbow 2, the tee 3 and the reducer 4, the inner wall cladding layers of the two components welded together are both made of stainless steel, that is, the two components welded together are the straight pipe 1, the tee 3 and the reducer 4, and a 1.6 mm thick 309MoL stainless steel layer 8 is welded on the weld seam at the inner wall as a transition layer, and one or more 1.6 mm thick 347 stainless steel layers 9 are welded on the transition layer as a surface layer; the cladding layers of the two components welded together include a nickel-based alloy layer 10, that is, one of the two components welded together is the elbow 2, and a nickel-based alloy layer 10 is welded on the weld seam at the inner wall as a transition layer, and one or more nickel-based alloy layers 10 are welded on the transition layer as a surface layer.
[0052] The weld between the main pipeline and the main pump casing 5 is divided into two layers. The first layer is a nickel-based alloy layer 10 with a thickness of 6 mm. The nickel-based alloy layer 10 is welded on the butt joint surface of the main pipeline. The other layer is also a nickel-based alloy layer 10. The nickel-based alloy layer 10 is located between the first nickel-based alloy layer 10 and the butt joint surface of the main pump casing 5, fixing the main pipeline and the main pump casing 5 together.
[0053] The weld between the main pipeline and the main flowmeter 6 is divided into two layers. The first layer is a nickel-based alloy layer 10 with a thickness of 6 mm. The nickel-based alloy layer 10 is welded on the butt joint surface of the main pipeline. The other layer is also a nickel-based alloy layer 10. The nickel-based alloy layer 10 is located between the first nickel-based alloy layer 10 and the butt joint surface of the main flowmeter 6, fixing the main pipeline and the main flowmeter 6 together.
[0054] The weld between the main pipeline and the main regulating valve 7 is divided into three layers. The first layer is a nickel-based alloy layer 10, which is welded on the main pipeline docking surface. The second layer is also a nickel-based alloy layer 10, which is welded on the main regulating valve docking surface. The first layer is also a nickel-based alloy layer 10, which is located between the first nickel-based alloy layer 10 and the second nickel-based alloy layer 10, fixing the main pipeline and the main regulating valve 7 together.
[0055] A boss 12 made of WB36 is welded on the main pipeline, and the boss 12 is used to connect with the high-pressure auxiliary circuit pipeline 11.
[0056] The main circuit of the nuclear main pump test bench and the inner wall surfacing and annular seam butt welding method thereof include the following processes:
[0057] A. Surfacing stainless steel on the inner wall of the main pipeline, the process is:
[0058] The inner wall cladding work of the main pipeline is completed in the pipeline manufacturing factory. If the usual submerged arc welding and strip electrode cladding methods are used, the welding thickness is too large and cannot meet the requirements. Therefore, different welding methods and welding materials are needed to complete this work according to the different specifications and types of pipeline components in the main circuit.
[0059] The process of welding stainless steel on the inner wall of the three types of pipe fittings, 1, straight pipe 1, tee 3, and reducer 4, is as follows: (1) rust removal on the inner wall of the pipe fitting; (2) preheating the inner wall of the pipe fitting to 120℃~150℃; (3) welding a 1.6mm thick 309MoL stainless steel layer 8 on the inner wall of the pipe fitting as a transition layer; (4) performing PT inspection after the transition layer is cooled; (5) welding another 1.6mm thick 347 stainless steel layer 9 on the transition layer as a surface layer; (6) performing PT inspection after the surface layer is cooled; (7) grinding the surface layer; (8) heat treating the weld layer to eliminate welding stress; (9) performing PT inspection on the weld layer; (10) spraying glass beads on the surface of the surface layer to remove the oxide layer on the heat-treated surface.
[0060] Since the 347 stainless steel layer 9 cannot be directly overlaid on the WB36 alloy steel, a 309MoL stainless steel layer 8 is first overlaid between the 347 stainless steel layer 9 and the inner wall of the straight pipe 1 as a transition layer.
[0061] The tee 3 and the reducer 4 are welded by automatic TIG welding, and the straight pipe 1 is welded by automatic MIG welding.
[0062] 2. The process of surfacing stainless steel on the inner wall of the elbow 2 is as follows: (1) rust removal on the inner wall of the elbow 2; (2) preheating the inner wall of the elbow 2 to 120°C to 150°C; (3) surfacing a layer of nickel-based alloy 10 with a thickness of 2.5 to 3.5 mm on the inner wall of the elbow 2 as a surface layer, preferably, the thickness of the surface layer is 3 mm; (4) performing PT inspection after the surface layer is cooled; (5) grinding the surface layer; (6) heat treating the surfacing layer to eliminate welding stress; (7) performing PT inspection on the surfacing layer; (8) spraying glass beads on the surface of the surface layer to remove the oxide layer on the heat-treated surface.
[0063] Since the weight of elbow 2 exceeds the carrying capacity of the automatic welding machine, manual welding can be used.
[0064] B. The main pipeline components and equipment are connected by girth butt welding, the process is as follows;
[0065] 1. Circumferential butt welding process of main pipeline components:
[0066] (1) Preheat the area around the weld to 120℃~150℃; (2) Use TIG welding to make the base weld; (3) Full weld the weld; (4) Heat treatment of the weld; (5) Grind the weld on the inner wall of the pipeline; (6) PT inspection of the weld; (7) Preheat the weld to 120℃~150℃; (8) The weld overlay layer of the main pipeline components is all stainless steel. A 1.6mm thick 309MoL stainless steel layer 8 is welded on the weld on the inner wall of the pipeline as a transition layer. After the transition layer is cooled, a PT inspection is carried out, and then another layer of cladding is welded on the transition layer. A 1.6 mm thick 347 stainless steel layer 9 is used as the surface layer; if there is a nickel-based alloy layer in the weld layer of the main pipeline component, a layer of nickel-based alloy layer is first welded on the inner wall of the pipeline as a transition layer. After the transition layer is cooled, a PT test is performed, and then one or more nickel-based alloy layers are welded on the transition layer as the surface layer; (9) After the surface layer is cooled, a PT test is performed; (10) Heat treatment of the weld layer to eliminate welding stress; (11) Grinding of the weld layer and weld; (12) PT test of the weld layer; (13) UT / RT weld test.
[0067] 2. Butt welding process of main pipeline and main pump casing:
[0068] The material of the main pump casing 5 is austenitic stainless steel 304L, which is butt-jointed with the main pipeline. Due to the butt joint of dissimilar materials, a layer of nickel-based alloy layer 10 with a thickness of 6 mm needs to be firstly welded on the butt surface of the main pipeline. After the nickel-based alloy layer 10 is subjected to PT inspection and stress relief annealing treatment at an annealing temperature of 580-620°C, the circumferential butt welding is performed with nickel-based alloy welding materials. The weld does not need annealing treatment. In this embodiment, the annealing temperature is 600°C.
[0069] 3. The process of butt welding of the main pipeline and the main flow meter:
[0070] The main flow meter 6 is made of austenitic stainless steel 304L and is butt-jointed with the main pipeline. Due to the butt joint of dissimilar materials, a 6mm thick nickel-based alloy layer 10 needs to be firstly welded on the butt surface of the main pipeline. After the nickel-based alloy layer 10 is subjected to PT inspection and stress relief annealing treatment at an annealing temperature of 580-620°C, a circumferential butt welding is performed with a nickel-based alloy welding material. The weld does not need to be annealed. In this embodiment, the annealing temperature is 600°C.
[0071] 4. Butt welding process of main pipeline and main regulating valve ring seam:
[0072] The material of the main regulating valve 7 is SA351, which is connected to the main pipeline. If it is directly welded, the preheating temperature must meet its material requirements, which is as high as 690°C. However, this temperature is not suitable for stainless steel. Therefore, first, a layer of nickel-based alloy welding material with the grade of INCONEL152M is welded on the docking surface of the main regulating valve 7 and the docking surface of the main pipeline respectively. The preheating temperature is 120°C~150°C. After the docking surface is welded, the main pipeline welding layer and the main regulating valve 7 welding layer are heat treated at a constant temperature of 550°C for 2 hours, and then the main pipeline welding layer and the main regulating valve 7 welding layer are circumferentially butt-welded with nickel-based alloy welding materials.
[0073] 5. Circumferential butt welding process of main pipeline and high-pressure auxiliary circuit pipeline:
[0074] Between the main pipeline and the high-pressure auxiliary loop pipeline 11, a boss 12 made of WB36 is provided. The boss 12 is welded on the main pipeline. When the boss 12 is connected to the high-pressure auxiliary loop pipeline 11, a layer of 6mm thick nickel-based alloy layer 10 is welded on the butt surface where the boss 12 and the high-pressure auxiliary loop pipeline 11 are connected. After the nickel-based alloy layer 10 is subjected to PT inspection and stress relief annealing treatment at an annealing temperature of 580-620°C, a nickel-based alloy welding material is used to perform circumferential butt welding with the high-pressure auxiliary pipeline 8. The weld does not need annealing treatment. In this embodiment, the annealing temperature is 600°C.
[0075] 6. In the above process, after the butt surfaces of the main pipeline components and equipment are processed before butt welding, circumferential butt welding is carried out according to the following process flow:
[0076] 1) Pre-matching inspection:
[0077] Before joining, clean the oil, dirt, rust, paint, etc. on the inner and outer walls of the pipe within 15 to 20 mm on each side of the weld until a metallic luster is emitted;
[0078] The base material at the groove is free of defects such as cracks, heavy skin, groove damage and burrs; before welding each weld, the pipe end shall be subjected to 100% PT or MT inspection, and welding shall be carried out after passing the inspection;
[0079] The groove processing dimensions meet the requirements of the drawings.
[0080] 2) Set up the argon filling plug:
[0081] When welding stainless steel pipes, argon protection is required on the inside of the weld. To ensure the protection effect and save argon, plugs are installed on both sides of the weld. Before joining, the argon filling tool is placed in the pipe. The distance between the two plugs is not less than 400mm and they are evenly distributed on both sides of the groove. Argon filling is stopped after two layers of argon arc welding and one layer of electric arc welding are completed.
[0082] 3) Counterpart inspection:
[0083] Before jointing, the groove surface and inner wall shall be subjected to PT inspection within 20mm from the groove edge. Jointing can only be carried out after confirming that there are no surface defects.
[0084] Before connection, confirm that the air chamber for argon filling is sealed properly;
[0085] When welding parts, the inner walls should be flush. If there is misalignment, the local misalignment value should not exceed 10% of the wall thickness and should not be greater than 1mm. The straightness of the weld should be ≤3 / 200.
[0086] The gap between the joints is 3 to 4 mm. If it is too large or too small, it will be trimmed to the specified size. No forceful jointing or filling in the gap will be performed.
[0087] 4) Welding point fixation:
[0088] When spot-fixing the weld, plugs are used to spot-fix in the groove, and the spot-fixing positions are arranged symmetrically; the welding materials, welding process, and welder qualifications for spot-fixing are the same as those for formal welding;
[0089] Before spot welding, flame preheating should be used appropriately at a temperature of 200-250°C. After the spot welding of the weld is completed, the spot welds should be checked and any defects should be dealt with in a timely manner.
[0090] 5) Preheating:
[0091] The main pipeline weld is preheated before welding. The preheating method adopts electric heating. The preheating temperature is 120-150℃. The temperature is based on actual measurement and records should be kept.
[0092] 6) Argon filling:
[0093] When welding the pipeline, the pipe needs to be filled with argon; when filling with argon, the initial flow rate is 10-20L / min. After the argon is full, the argon is adjusted to the flow rate specified in the welding process card, and then the argon arc welding is performed. During the root welding process, the filling degree of the argon in the gas chamber should be checked frequently, and the argon flow rate should be adjusted at any time to ensure that the gas chamber is always filled with argon, effectively ensuring the quality of the base weld.
[0094] When the argon arc welding is nearing the end, that is, when the argon arc welding is sealed, the argon gas in the gas chamber rushes out from this port, so the argon filling flow rate is reduced, and the specific flow rate is adjusted during construction.
[0095] 7) Use argon arc welding for base welding:
[0096] When striking the arc, deliver argon gas 1.5 to 4 seconds in advance to expel the air in the argon gas delivery hose and at the weld. After extinguishing the arc, delay extinguishing the gas for 5 to 15 seconds to protect the tungsten electrode and molten pool that have not yet cooled down and reduce the degree of oxidation on the weld surface.
[0097] During the argon arc welding primer process, use a flashlight to carefully check the root weld to ensure that there are no visible defects at the root. After the primer is completed, the secondary layer welding is immediately carried out. If the argon arc welding primer fails the inspection, the argon filling device is difficult to install, the argon filling space is large, the argon filling effect is not ideal, and the repair is extremely difficult. Therefore, it is required to grind all the parts that are considered to be in doubt during the argon arc welding primer process.
[0098] When welding to the plug, remove the plug and grind the welding spot and weld with an angle grinder or electric grinder to leave no traces such as weld scars. After checking with the naked eye or a magnifying glass to confirm that there are no defects such as cracks, continue welding.
[0099] The argon arc welding primer is at least 2 layers, each layer is 2.8 to 3.2 mm thick.
[0100] In order to improve the quality of argon arc welding primer, the swing rolling welding process is adopted.
[0101] 8) Interlayer welding and cover welding:
[0102] Interlayer welding and cap welding adopt manual arc welding method, preheating temperature 120 ~ 150 ℃, two people symmetrical welding;
[0103] The multi-layer and multi-pass welding joints are staggered and the arc is not closed at one place to avoid excessive local temperature affecting the welding quality;
[0104] Pay attention to the cleaning between layers. During welding, stagger the joints of each layer of welds by 10 to 15 mm. At the same time, pay attention to the smoothness of the weld to facilitate slag removal and avoid "dead corners". After each layer of welds is welded, use a grinder or wire brush to clean the slag, spatter and other debris, paying special attention to the middle joints and groove edges. Only after passing the self-inspection can the next layer be welded;
[0105] During the welding interruption process, the weld temperature is always maintained at 150-200℃ to prevent defects such as cracks. When re-welding, carefully check and confirm that there are no cracks, and then continue welding according to the process requirements.
[0106] During welding, pay attention to the quality of the joint and arc ending. Fill the molten pool when ending the arc to avoid arc pits.
[0107] 9) Self-inspection after welding:
[0108] After welding, the welding slag, spatter, etc. on the weld surface should be cleaned in time, and the appearance defects that exceed the standard should be polished and repaired. The process requirements for repair welding are the same as those for formal welding.
[0109] 10) Post-weld heat treatment:
[0110] Post-weld heat treatment is carried out after the main weld of the main pipe base material is completed: heat treatment temperature is 330-370℃, and insulation time is 3 hours; after the main pipe weld is completed, post-weld heat treatment is carried out immediately.
[0111] The final heat treatment of the weld is carried out after the surfacing of the inner wall of the main pipeline is completed: the heat treatment temperature is 580-620℃, the insulation time is 2 hours, and the heating and cooling rates are in accordance with the heat treatment regulations.
[0112] 11) Stainless steel cladding on the inner wall of each butt weld:
[0113] After the butt welds of the main pipeline and various components and equipment are completed, the inner wall welds of the pipeline need to be clad with a corrosion-resistant layer and the surface must be polished smooth.
[0114] First, the inner wall is polished, and after the polished surface passes the PT inspection, the inner wall of the pipeline is preheated to 120-150℃;
[0115] The weld cladding layer on the inside of the main pipeline is divided into two parts: the transition layer and the surface layer. The cladding layers of the butt-jointed pipe components are all made of stainless steel. A layer of 309MoL stainless steel layer 8 is clad as the transition layer. After the surface of the transition layer passes the PT inspection, a layer of 347 stainless steel layer 9 with a thickness of 1.6 mm is clad as the surface layer. If there is a nickel-based alloy layer 10 in the cladding layer of the butt-jointed pipe components, a layer of nickel-based alloy layer 10 is clad first as the transition layer. After the surface of the transition layer passes the PT inspection, one or more nickel-based alloy layers 10 are clad on the transition layer as the surface layer.
[0116] Before surfacing the transition layer, the metal temperature inside the weld must be heated to 120-150°C; considering that when welding inside the pipe, the welder works inside the pipe in a small space, and the welder's tolerance to high temperatures, the metal temperature at the weld can be reduced to 60-80°C during surface layer welding.
[0117] Before surfacing, grind the base weld to make it smooth, and then proceed with surfacing after the PT is qualified. During surfacing, use small current multi-pass welding, first weld the two sides and then the middle, and ensure the quality of arc starting and arc ending during welding.
[0118] C. Weld heat treatment:
[0119] Heat treatment is required during the butt welding of all components and equipment of the main pipeline and the cladding of the inner wall stainless steel layer. The weld heat treatment adopts crawler-type ceramic heating plate for heating, and the heating plate is placed on the outer wall of the weld, and the heating width is not less than 300mm from the center of the weld; because the main pipeline has a large diameter and thick wall, in order to reduce the temperature difference between the inside and outside of the pipe wall, the inner and outer walls of the weld are required to be covered with aluminum silicate blankets of high-temperature fiber cloth; temperature monitoring adopts thermocouples, and four temperature measuring points are placed at 3 o'clock, 6 o'clock, 9 o'clock and 12 o'clock on the outer wall, and one temperature measuring point is placed at 6 o'clock on the inner wall; during the heating process, the heating and cooling speed above 350℃ is controlled at 100℃ / h, the constant temperature time of the weld is 1 hour, and during the insulation period of the weld, the difference between the highest and lowest temperatures in the heating zone should not be greater than 30℃. Considering the temperature gradient of the inner and outer pipe walls, the inner wall temperature is required to be no less than 540℃, and the outer wall temperature is controlled within 620℃.
[0120] When the main pump casing is welded to the main pipeline, after the main pipeline side bevel cladding is completed, the main pipeline and its cladding layer need to be subjected to stress relief heat treatment at a temperature of 540-560°C for 1 hour.
[0121] When the valve body of the main regulating valve 7 is welded to the main pipeline, after the surfacing welding is completed at the groove of the valve body of the main regulating valve 7, the surfacing layer is subjected to a heat treatment at a temperature of 690°C for 2 hours; and after the butt welding with the main pipeline is completed, a stress relief heat treatment is performed at a temperature of 540-560°C for 1 hour.
[0122] After the heat treatment of each weld is completed, each weld is hardness tested at three different welding positions, and the hardness value shall not exceed 252HB.
[0123] D. Nondestructive testing:
[0124] In addition to meeting the requirements of the specifications, the inspection of the main pipeline welds also needs to undergo more stringent inspection requirements. After each weld is completed, it must undergo 2 UT, 2 MT and 4 PT. Only when all 8 inspections are qualified can the non-destructive testing of this weld be considered qualified. The specific steps are as follows:
[0125] (1) After the main pipeline is welded and post-heat treated and cooled for 48 hours, the weld is subjected to 100% UT, 100% MT and 100% PT after inner grinding. The weld is required to meet Grade I qualification.
[0126] (2) After the above inspection is passed, a 100% PT inspection is carried out on the transition layer cladding surface, which is required to meet the requirements of Level I. Then a 100% PT inspection is carried out on the surface layer, which is required to meet the requirements of Level I.
[0127] (3) After all the above tests are qualified, the welds are heat treated. After completion, 100% UT, 100% MT and 100% PT of the inner welds are performed, and the welds are required to meet Level I qualification.
[0128] (4) After the water pressure test, all welds are subject to a 10% MT inspection and are required to meet Level I standards.
[0129] The above contents described in this specification are merely examples of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, as long as they do not deviate from the contents of the present specification or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for inner wall cladding and circumferential butt welding of the main circuit of a nuclear main pump test bench, characterized in that: The main circuit of the nuclear main pump test bench comprises a main pipeline, a main pump casing, a main flow meter and a main regulating valve. The main pipeline is made of WB36 alloy steel, which comprises four types of components: a straight pipe, an elbow, a tee and a reducing joint. The main pump casing, the main flow meter and the main regulating valve are welded and fixed to the main pipeline, and the straight pipe, the elbow, the tee and the reducing joint are welded and fixed together; a layer of 309MoL stainless steel layer is welded on the inner walls of the three pipe fittings: the straight pipe, the tee and the reducing joint as a transition layer, and a layer of 347 stainless steel layer is welded on the transition layer as a surface layer; a layer of nickel-based alloy layer is welded on the inner wall of the elbow as a surface layer; among the four components: the straight pipe, the elbow, the tee and the reducing joint, the inner wall cladding layers of the two components welded together are both stainless steel, a layer of 309MoL stainless steel layer is welded on the weld seam at the inner wall as a transition layer, and more than one layer of 347 stainless steel layer is welded on the transition layer as a surface layer; if one of the cladding layers of the two components welded together is a nickel-based alloy layer, the inner wall The weld is welded with a nickel-based alloy layer as a transition layer, and one or more nickel-based alloy layers are welded on the transition layer as a surface layer; the weld between the main pipeline and the main pump casing is divided into two layers, the first layer is a nickel-based alloy layer, which is welded on the main pipeline butt joint surface, and the other layer is also a nickel-based alloy layer, which is located between the first nickel-based alloy layer and the main pump casing butt joint surface; the weld between the main pipeline and the main flowmeter is divided into two layers, the first layer is a nickel-based alloy layer, which is welded on the main pipeline butt joint surface, and the other layer is also a nickel-based alloy layer, which is located between the first nickel-based alloy layer and the main pump casing butt joint surface. The main pipe is welded on the butt joint surface, and the other layer is also a nickel-based alloy layer, which is located between the first nickel-based alloy layer and the butt joint surface of the main flow meter; the weld between the main pipe and the main regulating valve is divided into three layers, the first layer is a nickel-based alloy layer, which is welded on the butt joint surface of the main pipe, the second layer is also a nickel-based alloy layer, which is welded on the butt joint surface of the main regulating valve, and the third layer is also a nickel-based alloy layer, which is located between the first nickel-based alloy layer and the second nickel-based alloy layer; The process includes the following: A. Surfacing stainless steel on the inner wall of the main pipeline, the process is: 1) The process of cladding stainless steel on the inner wall of three types of pipe fittings, namely straight pipe, tee and reducer, is as follows: (1) rust removal on the inner wall of the pipe fitting; (2) preheating the inner wall of the pipe fitting to 120℃~150℃; (3) cladding a layer of 309MoL stainless steel on the inner wall of the pipe fitting as a transition layer; (4) cooling the transition layer; (5) cladding a layer of 347 stainless steel on the transition layer as a surface layer; (6) grinding the surface layer; (7) heat treatment of the cladding layer; (8) spraying glass beads on the surface of the surface layer; 2) The process of cladding stainless steel on the inner wall of the elbow is as follows: (1) rust removal on the inner wall of the elbow; (2) preheating the inner wall of the elbow to 120℃~150℃; (3) cladding a layer of nickel-based alloy on the inner wall of the elbow as the surface layer; (4) cooling the surface layer; (5) grinding the surface layer; (6) heat treatment of the cladding layer; (7) spraying glass beads on the surface of the surface layer; B. The main pipeline components and equipment are connected by girth butt welding, the process is as follows; 1) Process of circumferential butt welding of main pipeline components: (1) Preheating around the weld to 120℃~150℃; (2) Base welding; (3) Full welding of the weld; (4) Heat treatment of the weld; (5) Grinding of the weld on the inner wall of the pipeline; (6) Preheating of the weld to 120℃~150℃; (7) The weld overlay of the main pipeline components is all stainless steel. A layer of 309MoL stainless steel is welded on the inner wall of the pipeline as a transition layer. After the transition layer cools down, one or more layers of 347 stainless steel are welded on the transition layer as a surface layer; if there is a nickel-based alloy layer in the weld overlay of the main pipeline components, a layer of nickel-based alloy is first welded on the inner wall of the pipeline as a transition layer. After the transition layer cools down, one or more layers of nickel-based alloy are welded on the transition layer as a surface layer; (8) Surface layer cooling; (9) Heat treatment of the weld overlay; (10) Grinding of the weld overlay and weld; 2) Circumferential butt welding process between the main pipeline and the main pump casing: The main pump casing butt surface material is austenitic stainless steel 304L. It is necessary to first build up a layer of nickel-based alloy on the main pipeline butt surface, anneal the nickel-based alloy layer at 580-620℃, and then use nickel-based alloy welding materials for circumferential butt welding; 3) Circumferential butt welding process between main pipeline and main flowmeter: The main flowmeter butt surface material is austenitic stainless steel 304L. It is necessary to first build up a layer of nickel-based alloy on the main pipeline butt surface, anneal the nickel-based alloy layer at 580-620℃, and then use nickel-based alloy welding materials for circumferential butt welding; 4) The process of butt welding the main pipeline and the main regulating valve: The main regulating valve butt surface material is SA351. First, a layer of nickel-based alloy welding materials shall be welded on the main regulating valve butt surface and the main pipeline butt surface respectively. The preheating temperature is 120℃~150℃. After the butt surface welding is completed, the main pipeline welding layer and the main regulating valve welding layer shall be heat treated, and then the main pipeline welding layer and the main regulating valve welding layer shall be butt welded with nickel-based alloy welding materials. 5) Circumferential butt welding process between the main pipeline and the high-pressure auxiliary loop pipeline: A boss made of WB36 is provided between the main pipeline and the high-pressure auxiliary loop pipeline. The boss is welded on the main pipeline. When the boss is connected to the high-pressure auxiliary loop pipeline, a layer of nickel-based alloy layer is welded on the butt surface where the boss and the high-pressure auxiliary loop pipeline are connected. After the nickel-based alloy layer is annealed at 580-620℃, the nickel-based alloy welding material is used to perform circumferential butt welding with the high-pressure auxiliary pipeline.
2. The inner wall cladding and circumferential seam butt welding method of the main circuit of the nuclear main pump test bench according to claim 1 is characterized in that: In the above process B, after the butt surfaces of the main pipeline components and equipment are processed before butt welding, circumferential butt welding is carried out according to the following process: 1) Inspection before jointing: Before jointing, clean the weld until it emits metallic luster; before welding each weld, perform 100% PT or MT inspection on the pipe end, and weld only after passing the inspection; 2) Set up argon-filled plugs: During welding, the inside of the weld needs argon protection. To ensure the protection effect and save argon, plugs are set on both sides of the weld. Before the joints are connected, put the argon-filled tool into the pipe. The distance between the two plugs should not be less than 400mm, and they should be evenly distributed on both sides of the groove. Stop filling argon after welding is completed. 3) Matching inspection: Before matching, perform PT inspection on the groove surface and inner wall, and only match after confirming that there are no surface defects; when matching welds, make sure that the inner wall is flush, if there is misalignment, the local misalignment value shall not exceed 10% of the wall thickness and shall not exceed 1mm; the matching straightness shall be ≤3 / 200; the matching gap shall be 3-4mm, and if it is too large or too small, it shall be trimmed to the specified size, and no strong matching shall be performed or fillers shall be added in the gap; 4) Spot welding of welds: When spot welding of welds, plugs are used to spot weld them in the groove, and the spot welding positions are arranged symmetrically; preheating is performed before spot welding, and the preheating temperature is 200-250℃; 5) Preheating: The main pipeline weld should be preheated before welding; 6) Argon filling: Argon needs to be filled in the pipe during root welding; when filling argon, the initial flow rate is 10-20L / min. After the argon is full, root welding can be carried out; 7) Use argon arc welding for base welding: supply argon gas 1.5 to 4 seconds in advance when striking the arc, and remove the air in the argon gas delivery hose and at the weld; after the arc is extinguished, delay 5 to 15 seconds to extinguish the gas, protect the tungsten electrode and the molten pool that have not yet cooled down, and reduce the degree of oxidation on the weld surface; when welding to the plug, remove the plug and grind the weld joint; the argon arc welding base is at least 2 layers, each layer is 2.8 to 3.2 mm thick; 8) Interlayer welding and cover welding: The preheating temperature of interlayer welding and cover welding is 120-150℃; pay attention to the cleaning between layers, and stagger the joints of each layer of welds by 10-15mm during welding; during the interruption of welding, the weld seam should always maintain a temperature of 150-200℃; 9) Post-weld heat treatment: After the main pipeline weld is completed, the weld is post-heat treated at a temperature of 330-370°C and kept warm for 3 hours; after the surfacing welding of the inner wall of the main pipeline is completed, the weld is finally heat treated at a temperature of 580-620°C and kept warm for 2 hours; 10) Stainless steel cladding on the inner wall of each butt weld: After the butt welds of the main pipeline and various components and equipment are completed, the welds on the inner wall of the pipeline need to be clad, and the surface of the cladding layer is polished and smooth: first, the inner wall is polished, and after polishing, the preheating temperature of the inner wall of the pipeline is between 120 and 150°C; the weld cladding layer on the inside of the main pipeline is divided into two parts: a transition layer and a surface layer; the cladding layers of the butt pipe components are all made of stainless steel, a layer of 309MoL stainless steel is clad as a transition layer, and then a layer of 347 stainless steel is clad as a surface layer; if there is a nickel-based alloy layer in the cladding layer of the butt pipe components, first a layer of nickel-based alloy is clad as a transition layer, and then one or more layers of nickel-based alloy are clad on the transition layer as a surface layer.
3. The inner wall cladding and girth butt welding method of the main circuit of the nuclear main pump test bench according to claim 1 is characterized in that: In the above process A, the tees and reducers are welded by machine automatic TIG welding, and the straight pipes are welded by machine automatic MIG welding.
4. The inner wall cladding and girth butt welding method of the main circuit of the nuclear main pump test bench according to claim 1 is characterized in that: The annealing temperature is 600°C during the circumferential butt welding process between the main pipeline and the main pump casing, the circumferential butt welding process between the main pipeline and the main flow meter, and the circumferential butt welding process between the main pipeline and the high-pressure auxiliary loop pipeline.
Citation Information
Patent Citations
Nuclear island primary device connection tube safe end dissimilar metal welding technology
CN101890562A
Curved surface weld overlay method and lance manufacturing method employing same
CN103917321A
Welding method of temperature pipe and main water feeding pipe
CN104384673A
Nuclear power main pump test device
CN105508234A
Compound welding method for large-diameter compound steel pipe with pipe ends provided with corrosion resistant alloy through surfacing