A method and a special device for preparing a thin-walled pipe flattening texture test specimen
By using the devices of pressure components, load-bearing components and adjustment components to flatten thin-walled pipe samples on the Gleeble thermal simulation testing machine, the problem of texture measurement of thin-walled pipes is solved, and efficient and low-cost texture analysis is achieved, which is suitable for Determined by XRD and EBSD.
Patent Information
- Application Number
- CN202010145648.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-01-02
- Filing Date
- 2020-03-05
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
It is difficult to effectively measure the texture of thin-walled pipes with existing technology. In particular, during the sample preparation process, there are problems such as difficult grinding and polishing of curved surfaces, low sample resolution, and complicated and high-cost sample preparation processes.
Provide a special device consisting of a pressure component, a load-bearing component and an adjustment component, combined with a Gleeble thermal simulation testing machine, to flatten thin-walled pipe specimens by applying true strain conditions to form a flat specimen suitable for XRD and EBSD measurements. It solves the problems of sample preparation complexity and high cost.
It realizes the true measurement of the texture of thin-walled pipes, simplifies the sample preparation process, reduces the cost, and expands the scope of application. It can be used for both macro texture analysis and micro texture analysis.
Smart Images

Figure CN111175325B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal material analysis, relates to a technology for measuring the texture of metal materials, and in particular provides a method for preparing a thin-walled tube flattening texture measurement sample and a special device. Background Art
[0002] The pipe industry is closely related to social production and people's lives. my country's metal pipe industry has been developed for more than 50 years, and its scale has been quite large, and it has a trend of continuous growth in recent years. Metal structural parts made of metal pipes have the advantages of good rigidity, high strength, light weight and low cost. Its application range in industrial products is constantly expanding with the development of modern manufacturing technology.
[0003] At present, metal pipes have been widely used in industrial piping systems in various industries such as construction, food, petroleum, chemical industry, nuclear power, aviation, etc., and have become the core components of pipe equipment in piping systems. In various industries, the most commonly used pipes include steel pipes, copper pipes, aluminum pipes, titanium pipes, zirconium pipes and other metal pipes.
[0004] The manufacturing process of metal pipes mainly includes rolling, extrusion and drawing. Metal pipes are prone to texture when plastic deformation occurs. Crystal texture is formed in the process of hot and cold processing and plastic forming. The grains in the polycrystalline are arranged around certain special orientations to varying degrees, so that the orientations of each grain tend to be consistent, that is, to form a preferred orientation. Studies have found that the greater the deformation, the stronger the texture produced, and the more obvious the anisotropy of the polycrystalline. The texture not only affects the orientation and mechanical properties of the pipe, but is also related to properties such as stress corrosion cracking, which in turn affects the service life of the pipe. Texture is the best bridge for analyzing the relationship between pipe processing parameters and performance. A clear understanding of the texture characteristics and evolution laws during pipe processing is of great significance for predicting product performance, exerting material potential, and rationally formulating process parameters.
[0005] At present, the most commonly used methods for measuring the texture of metal materials are XRD and EBSD. Both XRD and EBSD are based on the principle of crystal diffraction. The difference is that the XRD method uses X-rays. With the help of a fully automatic X-ray diffractometer, it is suitable for texture measurement of large quantities of samples, and obtains macroscopic statistical texture information of the sample, which is unique in evaluating the overall macroscopic performance of the material. The EBSD method uses an electron beam to reveal the characteristics and laws of microscopic textures by studying the diffraction Kikuchi line pattern. The two methods have different focuses, each with its own characteristics, and complement each other.
[0006] The XRD method focuses on the analysis of macroscopic areas, and can make thousands of grains in the material participate in diffraction. It has high statistics and obtains all the texture information in the concept of macroscopic statistical distribution. It does not have high requirements for the test sample. XRD uses characteristic X-rays to irradiate the sample and perform texture analysis based on the difference in diffraction intensity of the sample in different directions. Its basic principle is to place the X-ray detector at the 2θ position that conforms to the Bragg equation, and rotate the sample around the incident point in space so that the grains in all directions enter the diffraction direction one after another, and continuously measure the diffraction intensity. If the sample has no texture, the intensity remains unchanged; if the sample has texture, the intensity varies with the orientation of the sample. The diffraction intensity is proportional to the pole density of the crystal plane where the diffraction occurs. The intensity is graded and marked on the polar projection diagram according to its corresponding orientation to obtain the pole figure, from which the texture information of the sample can be analyzed. Texture is closely related to the performance of materials. The texture information obtained by the XRD method can provide a theoretical basis for further optimizing the production process through mathematical calculations and research on the relationship between production process parameters and texture. Combined with the performance prediction theory, the physical properties of the material can be inferred, and the evaluation of the overall macroscopic performance of the material is unique.
[0007] The EBSD method can study the orientation of each grain in the material and the orientation difference between grains from a microscopic perspective, making the material texture measurement technology enter the submicron order of magnitude, especially in the study of the mechanism of some texture evolution and the study of local microtexture. It has great application value and represents the highest level of microtexture analysis today. The EBSD method requires that the sample surface is flat and there is no damage during the sample preparation process to avoid damaging the grain boundaries between grains. There should be no stress layer on the surface of the sample. EBSD uses an electron beam to bombard the sample surface, hitting the atoms in the crystal to produce scattering. These scattered electrons produce diffraction effects at certain specific angles due to the different types of crystal planes they hit, producing diffraction cones in space and diverging infinitely into space. A series of Kikuchi bands are obtained by intercepting the diffraction cone using a fluorescent screen, and then the texture is analyzed based on the characteristics of the Kikuchi line. In addition to providing the orientation information of a single grain, EBSD can also obtain the orientation difference between adjacent grains and the grain boundary angle, which provides an excellent experimental means for studying the changes in the grains and grain boundaries of the internal structure of the material with the process and the influence on the material properties.
[0008] At present, there are few technologies for measuring texture of thin-walled pipes. The surface of thin-walled pipes is a curved surface, which is difficult to grind, difficult to polish, and has low sample resolution. In addition, the general method for preparing pipe samples for measuring texture is relatively limited. For example, it can only be used to prepare XRD samples to measure macro texture, or it can only be used to prepare EBSD samples to measure micro texture, or when using EBSD measurement, it cannot simultaneously meet the texture analysis under low magnification (such as 100 times) and high magnification (such as 10,000 times), or the process of preparing thin-walled pipe samples is complicated and costly, or the prepared sample effect is not good. JE Lewis mentioned in (Texture Measurement Techniques for Zircaloy Clading: A Sound-Robin Study, Zirconium in the Nuclear Industry, Proceedings of the Fifth International Conference, Boston, 1980: pp39-60) that the zirconium tube is cut into small pieces along the axial direction, and then bonded together in the direction to obtain a plane sample. This method cannot ensure that each strip is in the same direction after cutting and bonding. Li Xingrong et al. mentioned the tube thinning and flattening method in (Texture Measurement and Analysis of Small-caliber TA18 Aviation Titanium Alloy Tubes [J]. Rare Metal Materials and Engineering, 2012, 41(7): 1243-1246). The tube wall thickness is corroded and thinned to about 0.05 mm. The tube is cut into small pieces with scissors and spread on a glass slide and glued with glue. A layer of plastic film is covered on the surface of the sample, and another glass slide is pressed on it. The sample is spread into a plane and the texture is measured using a general flat plate texture measurement method. This method is difficult to control the thickness and uniformity of corrosion thinning. The invention patent with application number 201210129928.0 provides a method and device for measuring the texture of metal tubes. The sample preparation process of this method is complicated, and a non-textured standard sample needs to be prepared. The tube sample and the non-textured standard sample need to be measured at the same time, and it can only be used for XRD method to test macro texture. Summary of the invention
[0009] The purpose of the present invention is to provide a method and a special device with excellent technical effect and suitable for preparing a thin-walled tube flattening texture measurement sample, so as to solve the defects of the prior art and realize the real measurement of the texture of the thin-walled tube. The device has a simple structure, is easy to operate, has low cost, high sample preparation efficiency, and a wide range of applications.
[0010] The present invention provides a device for preparing a thin-walled tube flattening texture test sample, which is characterized by comprising a pressure member 1, a bearing member 2, an adjusting member 3 and a Gleeble thermal simulation test machine 6, wherein:
[0011] The pressure member 1 is composed of a pressure end 1a and a pressing end 1b, and the overall shape is a T-shaped structure consisting of two rectangular parallelepipeds. The pressure end 1a is a large rectangular parallelepiped part, the outer side of which contacts the pressure head 6a of the Gleeble thermal simulation test machine, and the pressing end 1b is a small rectangular parallelepiped.
[0012] The carrier 2 is composed of a sample carrier 2a and a rectangular groove 2b. The overall shape is a rectangular parallelepiped structure with a rectangular groove at one end. The sample carrier 2a is cut into a U-shaped structure along the axis, the inner side of which is used to carry the thin-walled pipe sample 11, and the outer side of which is in contact with the pressure head 6b of the Gleeble thermal simulation test machine. The size of the rectangular groove 2b matches the pressing end 1b of the pressure-applying member 1, so that it can accommodate the pressing end 1b that penetrates into the rectangular groove 2b.
[0013] The main part of the adjusting member 3 is a functional gasket 3a, which is a rectangular parallelepiped structure, and is provided with a rectangular through hole 3b that penetrates the rectangular parallelepiped structure along the thickness direction. The size of the rectangular through hole 3b matches the pressing end 1b of the pressure-applying member 1, so that the pressing end 1b can pass through the rectangular through hole 3b and penetrate into the rectangular groove 2b of the carrier 2;
[0014] After the pressure member 1, the bearing member 2 and the adjusting member 3 are combined together, a rectangular hole 4 is formed between the bottom of the rectangular groove 2b and the pressing end 1b. The length and width of the rectangular hole 4 are equal to those of the rectangular groove 2b, and the thickness is equal to that of the functional gasket 3a and the thin-walled pipe sample 11. The thickness of the functional gasket 3a is equal to that of the thin-walled pipe sample 11, and can be adjusted and selected according to the thickness of different thin-walled pipe samples 11.
[0015] As the preferred technical solution:
[0016] The pressure member 1, the bearing member 2 and the adjusting member 3 of the device are all made of the same material, and under the test conditions, their strength should be greater than that of the thin-walled pipe.
[0017] The device flattening process is carried out on a Gleeble thermal simulation test machine, and the test conditions are selected according to the material and size of the thin-walled pipe sample 11.
[0018] A pair of thermocouples 5 is welded at the middle of the side wall of the pressure member 1 of the device, and another pair of thermocouples 5 is welded at the middle of the side wall of the carrier 2. The type of the thermocouples 5 matches the material of the device.
[0019] After the device is loaded with the thin-walled pipe sample 11, the pressure member 1, the bearing member 2 and the adjusting member 3 can be fixed together on the outer layer using copper conductive glue.
[0020] The length L of the thin-walled pipe sample 11 is 14 Not larger than the width L of the rectangular groove 2b3 , whose arc length is L 13 Not greater than the length L of the rectangular groove 2b 1 , and the arc length L 13 Not greater than half of the circumference corresponding to the outer diameter of the original thin-walled pipe.
[0021] The thickness of the thin-walled pipe sample 11 is L 6 -L 5 After flattening, it is the same as before flattening, and is exactly equal to the rectangular hole 4.
[0022] The device is suitable for thin-walled pipes, especially pipes with a wall thickness of no more than 2 mm.
[0023] The length and width of the device press-in end 1b, the rectangular groove 2b and the rectangular through hole 3b are not greater than 15 mm.
[0024] The roughness of each contact surface of the device is better than 3.2um.
[0025] The thin-walled tube sample 11 can be used to prepare XRD samples for measuring macro textures or EBSD samples for measuring micro textures after being flattened. The device has a wide range of applications, including but not limited to steel tubes, copper tubes, aluminum tubes, titanium tubes, and zirconium tubes.
[0026] The device of the present invention is suitable for flattening and measuring the texture of thin-walled pipes. The method for flattening and measuring the texture of thin-walled pipes meets the following specific operation requirements:
[0027] First, the carrier 2 is placed horizontally, and the adjusting member 3 is placed on the carrier 2. The thickness of the adjusting member 3 is L 6 -L 5 Equal to the thickness L of the thin-walled pipe sample 11 12 -L 11 , while maintaining the length L of the bearing member 2 and the adjusting member 3 2 and width L 4 The length L of the rectangular groove 2b and the rectangular through hole 3b is consistent. 1 and width L 3 The length L of the thin-walled pipe sample 11 is also equal to that of the rectangular groove 2b, so that it can accommodate the pressed end 1b that goes deep into the rectangular groove 2b; then, a thin-walled pipe sample 11 is placed on the rectangular groove 2b, and the bottom of the thin-walled pipe sample 11 is close to the bottom of the rectangular groove 2b. 14 Not larger than the width L of the rectangular groove 2b 3 , its width L 10 and arc length L 13 Not greater than the length L of the rectangular groove 2b 1 , and the arc length L 13 Not greater than half of the circumference corresponding to the outer diameter of the original thin-walled pipe;
[0028] Next, a pressure piece 1 is placed on the rectangular groove 2b, and the pressure end 1a of the pressure piece 1 is in close contact with the thin-walled pipe sample 11. The thickness of the pressure end 1a is L 5 There is no specific requirement, and it can be set according to needs, but the length and width of the pressure end 1a and the length L of the bearing member 2 and the adjusting member 3 2 and width L 4 Keep the same, the thickness L of the rectangular slot 4 7 -L 8 The thickness L of the adjusting member 3 6 -L 5 and the thickness L of the thin-walled pipe sample 11 before and after flattening 12 -L 11 are equal, the length and width of the press-in end 1b are equal to the length L of the rectangular groove 2b 1 and width L 3 Match so that it can penetrate into the rectangular groove 2b;
[0029] Next, after loading the thin-walled pipe sample 11, the pressure member 1, the support member 2 and the adjusting member 3 are kept as a rectangular structure as a whole, and then the pressure member 1, the support member 2 and the adjusting member 3 are fixed together with copper conductive glue on the outer layer.
[0030] Finally, in order to ensure that the thickness of the thin-walled pipe sample 11 is consistent before and after flattening, and that there is no arc surface after being pressed, nor is there a situation where the thickness is thinned due to deformation after being pressed, the entire flattening process is carried out on a Gleeble thermal simulation test machine to accurately set and control conditions such as temperature, strain, strain rate, etc. A pair of thermocouples 5 is welded at the middle of the side wall of the pressure member 1, and another pair of thermocouples 5 is welded at the middle of the side wall of the support member 2. The type of thermocouples matches the material of the device. The pressure member 1, the support member 2 and the adjustment member 3 are all made of the same material, so the two pairs of thermocouples should be made of the same material. The purpose of welding the two pairs of thermocouples is to allow the flattening process to be carried out when the temperature of the pressure member 1 and the support member 2 reaches the same level. The outer side of the pressure end 1a contacts the pressure head 6a of the Gleeble thermal simulation test machine, and the outer side of the sample carrier 2a contacts the pressure head 6b of the Gleeble thermal simulation test machine.
[0031] The present invention also provides a method for preparing a thin-walled tube flattening texture test sample using the device, characterized in that: the thin-walled tube sample is placed in a rectangular hole slot, and then a pressure piece, a bearing piece and an adjusting piece are installed in a Gleeble thermal simulation test machine, and the flattening test parameters are set. The strain condition input during the test is the true strain, and the calculation formula of the true strain is shown in formula (I):
[0032] ε t =ln(1+ε) (Ⅰ)
[0033] Where, ε is the engineering strain; εt For true resilience.
[0034] The calculation formula for engineering strain is shown in formula (II):
[0035]
[0036] Where, L 12 -L 11 is the thickness of the sample after flattening, that is, the original thickness of the thin-walled pipe sample, in mm; L 12 L is the height corresponding to the outer diameter of the sample before flattening, in mm; 11 It is the height corresponding to the inner diameter of the sample before flattening, in mm. After the thin-walled pipe sample is flattened using the Gleeble thermal simulation test machine, it is made into the sample required for texture measurement according to the test requirements.
[0037] There is no obvious difference between the appearance of thin-walled pipe samples after flattening and normal flat samples. Conventional XRD sample preparation methods can be used to prepare XRD samples for macro texture analysis, and conventional electrolytic polishing methods can be used to prepare EBSD samples for micro texture analysis. XRD samples should be ground into a plane and simply polished, which can not only remove the oxide film on the metal surface, but also eliminate the surface strain layer, and then use ultrasonic cleaning to remove surface impurities. Electrolytic polishing is simple and convenient to operate, so it is widely used in the preparation of EBSD samples. EBSD samples are first ground (coarse grinding and fine grinding), then mechanically polished (samples with less roughness can be directly mechanically polished), then ultrasonically cleaned, and then electrolytically polished. The electrolytic polishing parameters are selected according to different materials. After electrolytic polishing, ultrasonic cleaning is used again to obtain a perfect EBSD sample.
[0038] The device of the present invention solves the problem of the complicated sample preparation process, difficult grinding and polishing of the texture measurement of thin-walled pipe samples, and also solves the problem of the limited application scope of the general pipe sample preparation method. It can be used to prepare XRD samples for macro texture measurement and EBSD samples for micro texture measurement. Compared with the prior art, the present invention has the advantages of simple structure, diverse functions, easy operation, low cost and wide applicability. Its technical solution is standardized and reasonable, and its technical effect is excellent. The device of the present invention has predictable and relatively huge economic value and social value. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a three-view diagram of the combination of the pressure-applying member, the bearing member and the adjusting member of the device of the present invention;
[0040] Figure 2 It is a cross-sectional view of the device of the present invention taken along plane AA;
[0041] Figure 3It is a three-view drawing of the pressure-applying member of the device of the present invention;
[0042] Figure 4 It is a three-view drawing of the carrier of the device of the present invention;
[0043] Figure 5 It is a three-view drawing of the adjusting member of the device of the present invention;
[0044] Figure 6 This is a schematic diagram of the location of the thin-walled pipe sample of the device of the present invention;
[0045] Figure 7 It is a schematic diagram of the location of the thermocouple of the device of the present invention;
[0046] Figure 8 It is a schematic diagram of the structure of a thin-walled pipe sample before and after being flattened by the device of the present invention;
[0047] Fig. 9 Schematic diagram of the electrolytic polishing principle for preparing EBSD samples in Examples 1 and 2;
[0048] Fig.10 is the phase distribution diagram of the zirconium thin-walled tube sample analyzed by EBSD in Example 2;
[0049] Fig.11 The IPF diagram and legend of the EBSD analysis of the zirconium thin-walled tube sample in Example 2;
[0050] Fig.12 This is the PF image of the EBSD analysis of the zirconium thin-walled tube sample in Example 2.
[0051] Figure numerals: 1, pressure-applying member, 2, bearing member, 3, adjusting member, 4, rectangular hole groove, 5, thermocouple, 6, Gleeble thermal simulation test machine, 1a, pressure-applying end, 1b, pressing end, 2a, sample carrier, 2b, rectangular groove, 3a, functional gasket, 3b, rectangular through hole, 6a, pressure head at the pressure-applying end, 6b, pressure head at the pressure-receiving end. DETAILED DESCRIPTION
[0052] Example 1
[0053] A method and a special device for preparing a thin-walled pipe flattening texture test specimen, the device is composed of a Gleeble thermal simulation test machine, a pressure member 1, a bearing member 2 and an adjusting member 3, wherein:
[0054] The pressure member 1 is composed of a pressure end 1a and a pressing end 1b, and the overall shape is a T-shaped structure consisting of two rectangular parallelepipeds. The pressure end 1a is a large rectangular parallelepiped part, the outer side of which contacts the pressure head 6a of the Gleeble thermal simulation test machine, and the pressing end 1b is a small rectangular parallelepiped.
[0055] The carrier 2 is composed of a sample carrier 2a and a rectangular groove 2b. The overall shape is a rectangular parallelepiped structure with a rectangular groove at one end. The sample carrier 2a is cut into a U-shaped structure along the axis, and the inner side is used to carry the thin-walled pipe sample 11 (such as Figure 6 As shown), its outer side contacts with the pressure head 6b of the Gleeble thermal simulation test machine, and the size of the rectangular groove 2b matches the pressing end 1b of the pressure member 1 so that it can accommodate the pressing end 1b deep into the rectangular groove 2b;
[0056] The main part of the adjusting member 3 is a functional gasket 3a, which is a rectangular parallelepiped structure, and is provided with a rectangular through hole 3b that penetrates the rectangular parallelepiped structure along the thickness direction. The size of the rectangular through hole 3b matches the pressing end 1b, so that the pressing end 1b can pass through the rectangular through hole 3b and penetrate into the rectangular groove 2b of the bearing member 2;
[0057] After the pressure member 1, the bearing member 2 and the adjusting member 3 are combined together, a rectangular hole 4 is formed between the bottom of the rectangular groove 2b and the pressing end 1b. The length and width of the rectangular hole 4 are equal to those of the rectangular groove 2b, and the thickness is equal to that of the functional gasket 3a and the thin-walled pipe sample 11. The thickness of the functional gasket 3a is equal to that of the thin-walled pipe sample 11, and can be adjusted and selected according to the thickness of different thin-walled pipe samples 11.
[0058] The pressure member 1, the bearing member 2 and the adjusting member 3 of the device are all made of the same material, and under the test conditions, their strength should be greater than that of the thin-walled pipe.
[0059] A pair of thermocouples 5 is welded at the middle of the side wall of the pressure member 1 of the device, and another pair of thermocouples 5 is welded at the middle of the side wall of the carrier 2. The type of the thermocouples 5 matches the material of the device.
[0060] After the device is loaded with the thin-walled pipe sample 11, the pressure member 1, the bearing member 2 and the adjusting member 3 can be fixed together on the outer layer using copper conductive glue.
[0061] The length L of the thin-walled pipe sample 11 is 14 Not larger than the width L of the rectangular groove 2b 3 , whose arc length is L 13 Not greater than the length L of the rectangular groove 2b 1 , and the arc length L 13 Not greater than half of the circumference corresponding to the outer diameter of the original thin-walled pipe.
[0062] The thickness of the thin-walled pipe sample 11 is L 6 -L 5 After flattening, it is the same as before flattening. Figure 8 As shown, it is exactly equal to the rectangular hole 4.
[0063] The length and width of the device press-in end 1b, the rectangular groove 2b and the rectangular through hole 3b are not greater than 15 mm.
[0064] The roughness of each contact surface of the device is better than 3.2um.
[0065] After being flattened, the thin-walled tube sample 11 can be used to prepare XRD samples for measuring macro textures, and can also be used to prepare EBSD samples for measuring micro textures. The device has a wide range of applications, including but not limited to steel tubes, copper tubes, aluminum tubes, titanium tubes, and zirconium tubes.
[0066] The outer side of the pressure end 1a contacts the pressure head of the Gleeble thermal simulation test machine, and the outer side of the sample carrier 2a contacts the pressure head 6a of the Gleeble thermal simulation test machine. After the pressure member 1, the bearing member 2 and the adjusting member 3 are installed on the Gleeble thermal simulation test machine, the flattening test parameters are set. The strain condition input during the test is the true strain, and the calculation formula of the true strain is shown in formula (I):
[0067] ε t =ln(1+ε) (Ⅰ)
[0068] Where, ε is the engineering strain; ε t For true resilience.
[0069] The calculation formula for engineering strain is shown in formula (II):
[0070]
[0071] Where, L 12 -L 11 is the thickness of the sample after flattening, that is, the original thickness of the thin-walled pipe sample, in mm; L 12 L is the height corresponding to the outer diameter of the sample before flattening, in mm; 11 It is the height corresponding to the inner diameter of the sample before flattening, in mm.
[0072] There is no obvious difference in appearance between the thin-walled pipe sample after flattening treatment and the normal flat sample. Conventional XRD sample preparation method can be used to prepare XRD samples for macro texture analysis, and conventional electrolytic polishing method can be used to prepare EBSD samples for micro texture analysis. XRD samples should be ground into a flat surface and simply polished, which can not only remove the oxide film on the metal surface, but also eliminate the surface strain layer, and then use ultrasonic cleaning to remove surface impurities. Electrolytic polishing is simple and convenient to operate, so it is widely used in the preparation of EBSD samples. EBSD samples are first ground (coarse grinding and fine grinding), then mechanically polished (samples with less roughness can be directly mechanically polished), then ultrasonically cleaned, and then electrolytically polished, such as Fig. 9As shown, the electrolytic polishing parameters are selected according to different materials. After electrolytic polishing, ultrasonic cleaning is used again to obtain a perfect EBSD sample.
[0073] This embodiment solves the problem of the complicated sample preparation process, difficult grinding and polishing of the texture measurement of thin-walled pipe samples, and also solves the problem of the limited application scope of the general pipe sample preparation method. It can be used to prepare XRD samples for macro texture measurement and EBSD samples for micro texture measurement. Compared with the prior art, this embodiment has the advantages of simple structure, diverse functions, easy operation, low cost and wide applicability. Its technical solution is standardized and reasonable, and the technical effect is excellent. The device described in this embodiment has a predictable and relatively huge economic value and social value.
[0074] Example 2
[0075] Example 2 is specifically implemented based on the method and special device for preparing thin-walled pipe flattening texture test specimens in Example 1, and is hereby explained.
[0076] The material used in this embodiment is a Zr-4 alloy tube with a size of Φ6.00×δ0.80mm (diameter×wall thickness). The sample is 10.0mm long, 5.2mm wide, and the height corresponding to the outer diameter is 1.5mm.
[0077] The pressure piece 1, the bearing piece 2 and the adjusting piece 3 of the device for measuring the texture of thin-walled pipes are made of H13 steel, with a length of 15 mm and a width of 12 mm. The rectangular groove 2b and the rectangular through hole 3b are 12 mm long and 10 mm wide. The pressing end 1 cooperates with the two. The thickness of the pressure end 1a is 4 mm, the thickness of the pressing end 1b is 3 mm, the thickness of the sample stage 2a is 4 mm, the thickness of the rectangular groove 2b is 3 mm, and the thickness of the functional gasket 3a is 0.8 mm. Load the thin-walled pipe sample 11 (such as Figure 6 As shown in the figure), the pressure member 1, the bearing member 2 and the adjusting member 3 are fixed together on the outer layer with copper conductive glue.
[0078] Thermocouple 5 is welded firmly at the center of the surface of pressure member 1 and bearing member 2, such as Figure 7 As shown. The sample is then installed on the Gleeble3800 thermal simulation testing machine, with the outer side of the pressing end 1b in contact with the pressure head at the pressure-applying end of the thermal simulation testing machine, and the outer side of the sample carrier 2a in contact with the pressure head at the pressure-receiving end. The engineering strain calculated according to formula (Ⅱ) is -0.467, and the true strain calculated according to formula (Ⅰ) is -0.629. In order to eliminate the residual stress inside the pipe after flattening, the flattening temperature of the zirconium tube is set to 400°C, and the annealing process parameters after hot flattening are 635°C and kept for 3 hours and cooled with the furnace. The schematic diagram of the structure of the thin-walled pipe sample 11 before and after flattening is shown in Figure 8As shown, after flattening, the length is 10.0 mm, the width is 6.3 mm, and the thickness is 0.80 mm.
[0079] When preparing EBSD samples, they can be finely ground, then mechanically polished, then ultrasonically cleaned, and then electrolytically polished. The schematic diagram of the principle is shown below. Fig. 9 As shown, the electrolytic polishing solution is 10% perchloric acid + 90% alcohol, the voltage is 50V, and the current is 0.3A. After electrolytic polishing, ultrasonic cleaning is used again. The prepared EBSD sample has a resolution of 99.5%. Fig.10 This is the phase distribution diagram of the EBSD analysis of the zirconium thin-walled tube sample prepared in this example. Fig.11 The IPF diagram and legend of the EBSD analysis of the zirconium thin-walled tube sample prepared in this embodiment are as follows: Fig.12 This is the PF image of the EBSD analysis of the zirconium thin-walled tube sample prepared in this example. Figure 10-12 It can be seen that the c-axis of most α grains is close to parallel to the radial direction of the thin-walled tube, that is, the RD direction, and most of the {11-20} planes are perpendicular to the axial direction of the thin-walled tube, that is, the AD direction. The Kearns coefficient of the {0001} plane in the AD direction is 0.553, indicating that there is a strong radial basal texture in the material.
[0080] Example 3
[0081] Example 3 is specifically implemented based on the method and special device for preparing thin-walled tube flattening texture test specimens in Example 1, and is hereby explained.
[0082] The material used in this example is a Zr-4 alloy tube with a size of Φ6.00×δ0.80mm (diameter×wall thickness). The sample is 10.0mm long, 5.2mm wide, and 1.5mm high. The XRD sample is prepared by flattening according to the steps in Example 2.
[0083] The XRD sample preparation steps are simpler. First, grind it into a flat surface and then perform simple polishing. This can not only remove the oxide film on the metal surface, but also eliminate the surface strain layer. Then use ultrasonic cleaning to remove surface impurities. According to the EBSD sample preparation steps, the sample prepared by electrolytic polishing can also be used for XRD technology to test macro texture. During the XRD test, the acceleration voltage is 40kV, the current is 40mA, the ray source is CuKα, and the incident wavelength λ is The scanning step length is 0.02°, the scanning range is 10° to 90°, and the scanning rate is 1° / min. The full pole figure and orientation distribution function of the Zr-4 alloy thin-walled tube sample are calculated using the pole figure test data. The c-axis of most grains is close to the radial direction of the thin-walled tube, indicating that there is a strong radial basal texture in the material.
[0084] This embodiment can provide a theoretical basis for optimizing the production process of zirconium thin-walled pipes, provide technical support for the design and implementation of subsequent experiments, and can deduce the physical properties of the material by combining the performance prediction theory, and has its own uniqueness in evaluating the overall macroscopic performance of the material.
[0085] Matters not covered by the present invention are known technologies.
[0086] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A device for preparing a thin-walled tube flattening texture test specimen, characterized in that: The device is composed of a pressure-applying member (1), a bearing member (2), an adjusting member (3) and a Gleeble thermal simulation test machine (6), wherein the pressure-applying member (1) is pressed onto the bearing member (2) through the adjusting member (3), wherein: The pressure member (1) is composed of a pressure end (1a) and a pressing end (1b), and the overall appearance is a T-shaped structure composed of two rectangular blocks. The pressure end (1a) is a large rectangular block, the outer side of which contacts the pressure head (6a) of the Gleeble thermal simulation test machine, and the pressing end (1b) is a small rectangular block. The carrier (2) is composed of a sample carrier (2a) and a rectangular groove (2b), and its overall appearance is a rectangular parallelepiped structure with a rectangular groove at one end. The sample carrier (2a) is cut along the axis to form a U-shaped structure, the inner side of which is used to carry the thin-walled pipe sample (11), and the outer side of which is in contact with the pressure head (6b) of the Gleeble thermal simulation test machine. The size of the rectangular groove (2b) matches the pressing end (1b) of the pressure-applying member (1), so that it can accommodate the pressing end (1b) that penetrates into the rectangular groove (2b); The adjusting member (3) is a functional gasket (3a) having a rectangular parallelepiped structure and is provided with a rectangular through hole (3b) penetrating the rectangular parallelepiped structure in the thickness direction. The size of the rectangular through hole (3b) matches the pressing end (1b) of the pressure-applying member (1), so that the pressing end (1b) can pass through the rectangular through hole (3b) and penetrate into the rectangular groove (2b) of the bearing member (2); After the pressure-applying member (1), the bearing member (2) and the adjusting member (3) are assembled together, a rectangular hole groove (4) is formed between the bottom of the rectangular groove (2b) and the pressing end (1b), and the length and width of the rectangular hole groove (4) are equal to those of the rectangular groove (2b), and the thickness is equal to that of the functional gasket (3a) and the thin-walled pipe sample (11); The roughness of each contact surface of the device is better than 3.2um; After the device is loaded with the thin-walled pipe sample (11), the pressure-applying member (1) and the The bearing member (2) and the adjusting member (3) are fixed together.
2. The device for preparing a thin-walled tube flattening texture test sample according to claim 1, characterized in that: The pressure-applying member (1), the bearing member (2) and the adjusting member (3) of the device are all made of the same material.
3. The device for preparing a thin-walled tube flattening texture test specimen according to claim 1, characterized in that: A pair of thermocouples (5) is welded at the middle of the side wall of the pressure member (1) of the device, and another pair of thermocouples (5) is welded at the middle of the side wall of the support member (2).
4. The device for preparing a thin-walled tube flattening texture test sample according to claim 1, characterized in that: The length of the thin-walled pipe sample (11) is not greater than the width of the rectangular groove (2b), the arc length is not greater than the length of the rectangular groove (2b), and the arc length is not greater than half of the circumference corresponding to the outer diameter of the original thin-walled pipe.
5. The device for preparing a thin-walled tube flattening texture test sample according to claim 1, characterized in that: The thickness of the thin-walled pipe sample (11) after flattening is the same as that before flattening, and is not greater than 2 mm.
6. The device for preparing thin-walled tube flattening texture test specimens according to claim 1, characterized in that the length and width of the pressing end (1b), the rectangular groove (2b) and the rectangular through hole (3b) of the device are not greater than 15 mm.
7. A method for preparing a thin-walled tube flattening texture test sample using the device of claim 1, characterized in that: A pressure member (1), a bearing member (2) and an adjusting member (3) are installed on a Gleeble thermal simulation test machine (6), and the flattening test parameters are set: the strain condition input during the test is the true strain, and the calculation formula of the true strain is shown in formula (I): e t =ln(1+ε) (Ⅰ) Where, ε is the engineering strain; ε t For true strain; The calculation formula for engineering strain is shown in formula (II): Where, L 12 -L 11 is the thickness of the sample after flattening, i.e. the thickness of the original thin-walled pipe sample (11), in mm; L 12 L is the height corresponding to the outer diameter of the thin-walled pipe sample (11) before flattening, in mm; 11 is the height corresponding to the inner diameter of the thin-walled pipe sample (11) before flattening, in mm; After the thin-walled pipe sample (11) is flattened by using a Gleeble thermal simulation test machine (6), it is made into a sample required for texture measurement according to test requirements.
8. The method for preparing a thin-walled tube flattening texture test specimen according to claim 7, characterized in that: The samples prepared by this method can be used to prepare XRD samples for measuring macro texture, and can also be used to prepare EBSD samples for measuring micro texture.