Light emitting device and method for manufacturing light emitting device

By setting grooves on the substrate of the light emitting device and forming a containing layer and a light-transmitting layer by centrifugal force, the existing problem of low luminous efficiency is solved, and more efficient light reflection and light distribution characteristics are achieved.

CN111384228BActive Publication Date: 2024-12-03NICHIA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201911326152.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-12-28
Filing Date
2019-12-20
Publication Date
2024-12-03
Estimated Expiration
2039-12-20

AI Technical Summary

Technical Problem

There is room for improvement in the luminous efficiency of the existing light emitting device, especially in the design of the light reflective resin and the groove portion.

Method used

A light emitting element surrounding the groove portion is provided on the substrate, and the groove portion is filled with resin containing a reflective material, and the reflective material settles into a layer containing and a light transmittance layer by centrifugal force to cover the sides of the light emitting element to improve the light reflectivity.

Benefits of technology

The luminescence efficiency is significantly improved, the light loss is reduced, the light distribution characteristics are improved, and the manufacturing process is simplified.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111384228B_ABST
    Figure CN111384228B_ABST
Patent Text Reader

Abstract

Provided are a light-emitting device with high light-emitting efficiency and a method for manufacturing the light-emitting device. The light-emitting device (100) comprises: a substrate (2) having a groove (17) surrounding a first region (16); a light-emitting element (20) placed in the first region (16); a first covering member (30) disposed in the groove of the groove (17) and covering at least a portion of the side surface of the light-emitting element (20); a light-transmitting member (50) disposed on the first covering member (30) and the light-emitting element (20); the first covering member (30) comprising a containing layer (30a) disposed in the groove of the groove (17) and containing a first reflective material and a light-transmitting layer (30b) covering at least a portion of the side surface of the light-emitting element (20).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a light emitting device and a method for manufacturing the light emitting device. Background Art

[0002] In the past, there is known a light-emitting device in which a light-emitting element is mounted on a substrate. For example, Patent Document 1 discloses a light-emitting device comprising: a package having a concave portion having side surfaces and a bottom surface, the bottom surface having a linear or dot-shaped groove portion that is separated from the side surfaces and surrounds a component mounting region; a light-emitting element mounted on the component mounting region; a light-transmitting resin that covers the light-emitting element and is in contact with the inner surface of the groove portion; and a light-reflecting resin that is continuously formed from the side surfaces of the concave portion to the outer upper edge of the groove portion.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: (Japanese) Patent Publication No. 2017-204623 Summary of the invention

[0006] Problems that the invention will solve

[0007] In the technology of the above-mentioned patent document, there is room for further improvement in light emission efficiency.

[0008] An object of the embodiments of the present disclosure is to provide a light-emitting device having high light-emitting efficiency and a method for manufacturing the light-emitting device.

[0009] Technical means to solve problems

[0010] The light-emitting device of the embodiment of the present disclosure comprises: a substrate comprising a groove portion surrounding a first area; a light-emitting element placed in the first area; a first covering member disposed in a groove of the groove portion and covering at least a portion of a side surface of the light-emitting element; a light-transmitting member disposed on the first covering member and the light-emitting element; the first covering member comprising a containing layer and a light-transmitting layer, the containing layer being disposed in the groove of the groove portion and containing a first reflective material, the light-transmitting layer covering at least a portion of a side surface of the light-emitting element.

[0011] The manufacturing method of the light-emitting device of the embodiment of the present disclosure includes the following steps: preparing a substrate, the substrate having a groove portion surrounding a first area; placing a light-emitting element in the first area; filling a first resin containing a first reflective material in the groove of the groove portion; applying centrifugal force to the first resin to cause the first reflective material contained in the first resin to settle to form a first covering component, the first covering component having a containing layer and a translucent layer, the containing layer being arranged in the groove of the groove portion and containing the first reflective material, the translucent layer covering at least a portion of the side surface of the light-emitting element; forming a translucent component on the first covering component and the light-emitting element.

[0012] Effects of the Invention

[0013] The light emitting device according to the embodiment of the present disclosure can improve light emitting efficiency.

[0014] The method for manufacturing a light-emitting device according to the embodiment of the present disclosure can manufacture a light-emitting device with high light-emitting efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1A It is a perspective view schematically showing the structure of a light emitting device according to an embodiment.

[0016] Figure 1B It is a plan view schematically showing the structure of the light emitting device according to the embodiment, and is a plan view in a state where a part is seen through.

[0017] Figure 1C yes Figure 1A Cross-sectional view of the IC-IC line.

[0018] Figure 2 This is a flowchart of a method for manufacturing a light-emitting device according to an embodiment.

[0019] Figure 3A It is a cross-sectional view showing a step of placing a light-emitting element in the method for manufacturing a light-emitting device according to an embodiment.

[0020] Figure 3B It is a cross-sectional view showing a step of forming a second covering member in the method for manufacturing a light emitting device according to the embodiment.

[0021] Figure 3C It is a cross-sectional view showing a step of filling a first resin in the method for manufacturing a light emitting device according to an embodiment.

[0022] Figure 3D It is a schematic diagram showing a step of forming a first covering member in the method for manufacturing a light emitting device according to the embodiment, and is a schematic diagram showing a step of settling a first reflecting material by centrifugal force.

[0023] Figure 3EIt is a cross-sectional view showing a step of forming a first covering member in the method for manufacturing a light emitting device according to an embodiment, and is a cross-sectional view showing a state after the first reflecting material is precipitated by centrifugal force.

[0024] Figure 3F It is a cross-sectional view showing a step of forming a light-transmitting member in the method for manufacturing a light-emitting device according to an embodiment.

[0025] Figure 4 It is a cross-sectional view schematically showing the structure of a light emitting device according to another embodiment.

[0026] Figure 5A It is a plan view schematically showing the structure of a groove portion of a light emitting device according to another embodiment.

[0027] Figure 5B It is a plan view schematically showing the structure of a groove portion of a light emitting device according to another embodiment.

[0028] Figure 5C It is a plan view schematically showing the structure of a groove portion of a light emitting device according to another embodiment.

[0029] Figure 6 This is an image showing the structure of the light emitting device used in the first embodiment.

[0030] Fig. 7A : is a graph showing the relationship between the coating amount of the first resin and the light beam in the first embodiment.

[0031] Figure 7B : is a graph showing the deviation of the chromaticity coordinate x according to the directivity angle in the first embodiment.

[0032] Figure 7C : is a graph showing the deviation of the chromaticity coordinate y according to the directivity angle in the first embodiment.

[0033] Fig.7D : is a graph showing the deviation of the chromaticity coordinate x according to the directivity angle in the first embodiment.

[0034] Fig. 7E : is a graph showing the deviation of the chromaticity coordinate y according to the directivity angle in the first embodiment.

[0035] Fig. 8A This is an image showing a state of the light emitting device used in the second embodiment after a light emitting element is mounted and a second resin is applied.

[0036] Figure 8B It is an image showing a state after further coating of the first resin with respect to the light emitting device used in the second embodiment.

[0037] Figure 8CThis is an image showing a state in which a centrifugal force is further applied to the first resin and the reflective material is centrifugally precipitated, with respect to the light emitting device used in the second embodiment.

[0038] Fig.8D It is an image showing element electrodes regarding the light emitting device used in the second embodiment.

[0039] Fig. 8E This is an image showing a state after a light-transmitting member is formed with respect to the light-emitting device used in the second embodiment.

[0040] Fig.9A : is a graph showing the relationship between the color tone and the light beam in the second embodiment.

[0041] Fig. 9B This is a graph showing the relationship between each sample and the light beam in the second example.

[0042] Description of Reference Numerals

[0043] 2 substrate

[0044] 2a First lead electrode

[0045] 2b Second lead electrode

[0046] 2c Resin molded body

[0047] 3 Resin wall

[0048] 10 Packaging

[0049] 15 concavity

[0050] 16. Area 1

[0051] 17 Groove

[0052] 20 Light-emitting element

[0053] 21 Support base plate

[0054] 22 Semiconductor layer

[0055] 23 lines

[0056] 24 lines

[0057] 25 lines

[0058] 30 first covering member

[0059] 30a Containing layer

[0060] 30b Light-transmitting layer

[0061] 31 First Resin

[0062] 40 second covering member

[0063] 50 Translucent parts

[0064] 60 Protection element

[0065] 90° Rotation Axis

[0066] 100, 100A light emitting device

[0067] A Package rotation direction

[0068] B Direction parallel to the bottom of the concave part

[0069] C The direction of the first reflective material settling

[0070] D Coating position DETAILED DESCRIPTION

[0071] Hereinafter, the embodiments will be described with reference to the accompanying drawings. However, the methods shown below illustrate the light-emitting device and the method for manufacturing the light-emitting device for specifically realizing the technical idea of ​​the present embodiment, and are not limited to the following. In addition, the size, material, shape, relative arrangement, etc. of the structural components described in the embodiments are not intended to limit the scope of the present invention to these unless otherwise specified, but are merely examples. In addition, the size, positional relationship, etc. of the components shown in the drawings are sometimes exaggerated for the purpose of clarifying the description.

[0072] Implementation Method

[0073] [Light-emitting device]

[0074] Figure 1A It is a perspective view schematically showing the structure of a light emitting device according to an embodiment. Figure 1B It is a plan view schematically showing the structure of the light emitting device according to the embodiment, and is a plan view in a state where a part is seen through. Figure 1C yes Figure 1A Cross-sectional view of the IC-IC line.

[0075] The light emitting device 100 includes: a substrate 2 having a groove portion 17 surrounding a first region; a light emitting element 20 placed in the first region; a first covering member 30 provided in the groove of the groove portion 17 and covering at least a portion of the side surface of the light emitting element 20; and a light transmissive member 50 provided on the first covering member 30 and the light emitting element 20. The first covering member 30 of the light emitting device 100 includes a containing layer 30a provided in the groove of the groove portion 17 and containing a first reflective material, and a light transmissive layer 30b covering at least a portion of the side surface of the light emitting element 20.

[0076] That is, the light emitting device 100 includes a package 10 including a substrate 2 , a light emitting element 20 , a first cover member 30 , a second cover member 40 , and a light transmissive member 50 .

[0077] Hereinafter, each structure of the light emitting device 100 will be described.

[0078] The package 10 has a recess 15 formed by a bottom surface formed by the substrate 2 and side surfaces formed by the resin wall 3. The opening of the recess 15 is formed into a substantially rectangular shape by changing the shape of one corner and the other corners in a plan view, for example.

[0079] The substrate 2 is composed of a pair of lead electrodes consisting of a first lead electrode 2a and a second lead electrode 2b, and a resin molded body 2c that holds the first lead electrode 2a and the second lead electrode 2b.

[0080] The first lead electrode 2a is exposed at the bottom surface of the recess 15 and is connected to the light emitting element 20 and the wire 23. The second lead electrode 2b is exposed at the bottom surface of the recess 15 and is connected to the wire 24.

[0081] The first lead electrode 2a includes a groove 17 that surrounds the first region 16, which is a region for placing the light emitting element 20. The groove 17 is formed here so that the portion directly below the side surface of the light emitting element 20 is located at the inner upper edge of the groove 17. That is, the groove 17 is formed at a position along the outer side surface of the light emitting element 20. The groove 17 surrounds the first region 16 in a rectangular ring shape in a plan view. However, the groove 17 may surround the first region 16 in other shapes such as a circular ring shape or a diamond ring shape.

[0082] The width of the groove 17 surrounding the first region may be substantially the same over the entire circumference, or may be partially thickened. The width of the groove 17 is preferably 30 μm or more and 200 μm or less. If the width of the groove 17 is 30 μm or more, the containing layer 30a described later can be easily accommodated in the groove of the groove 17. On the other hand, if it is 200 μm or less, the amount of the first covering member 30 can be reduced. In addition, the strength of the substrate 2 is improved.

[0083] The depth of the groove 17 is preferably 10 μm or more and 150 μm or less. If the depth of the groove 17 is 10 μm or more, the containing layer 30a described later can be easily accommodated in the groove of the groove 17. In addition, it is easy to make the first reflective material settle. On the other hand, if it is 150 μm or less, the amount of the first covering member 30 can be reduced.

[0084] The groove 17 is preferably provided close to the light emitting element 20. Specifically, the groove 17 is preferably formed at a distance of 100 μm or less from the light emitting element 20. That is, the distance between the side surface of the light emitting element 20 and the inner upper edge of the groove 17 is preferably formed to be 100 μm or less. If the distance from the light emitting element 20 is 100 μm or less, the light from the light emitting element 20 is easily reflected by the containing layer 30a, and the luminous efficiency is improved. In addition, in the case where it is easier to improve the luminous efficiency, the groove 17 is preferably closer to the light emitting element 20, and it is more preferred that the inner side surface of the groove 17 is formed at a position of 0 μm from the light emitting element 20 along the outer side surface of the light emitting element 20. In addition, as long as the outer upper edge of the groove 17 is located outside the outer edge of the light emitting element 20 when viewed from above, the portion directly below the side surface of the light emitting element 20 may also be located on the groove 17. In this case, considering the mountability and heat dissipation of the light emitting element 20 , the distance between the side surface of the light emitting element 20 and the inner upper edge of the groove 17 is preferably 50 μm or less.

[0085] As the first lead electrode 2 a and the second lead electrode 2 b , for example, Fe, Cu, Ni, Al, Ag, Au, or an alloy containing any of these materials can be used.

[0086] In addition, the first lead electrode 2a and the second lead electrode 2b may also have a plating layer formed on the surface. The plating layer can be made of, for example, Au, Ag, Cu, Pt, or an alloy containing one of them. As long as the plating layer is made of these materials, the reflectivity of light emitted from the light emitting element 20 to the lead electrode side can be further improved.

[0087] The resin wall 3 is formed on the periphery of the upper surface side of the substrate 2. The resin wall 3 forms an outer wall surface along the outer side surface of the substrate 2, and the inner wall surface is formed inclined so as to widen the opening from the substrate 2 toward the opening direction of the recess 15. In addition, the resin wall 3 is also provided in the groove formed on the upper surface of the substrate 2, thereby improving the close contact between the resin wall 3 and the substrate 2.

[0088] As the resin wall 3 and the resin molded body 2c, for example, thermoplastic resins such as PA (polyamide), PPA (polyphthalamide), PPS (polyphenylene sulfide), or liquid crystal polymers, epoxy resins, silicone resins, modified epoxy resins, polyurethane resins, or thermosetting resins such as phenolic resins can be used.

[0089] The resin wall 3 and the resin molded body 2c may be integrally molded from the same member.

[0090] The light-emitting element 20 is a semiconductor element that emits light when voltage is applied. The light-emitting element 20 includes a light-transmitting support substrate 21 and a semiconductor layer 22 formed on the support substrate 21. In addition to an insulating substrate, a conductive substrate can also be used for the support substrate 21. The shape, size, etc. of the light-emitting element 20 can be arbitrarily selected. As the light-emitting color of the light-emitting element 20, a light-emitting color of any wavelength can be selected according to the application. For example, as a blue (light with a wavelength of 430 to 490 nm) or green (light with a wavelength of 495 to 565 nm) light-emitting element 20, a nitride-based semiconductor (In X Al Y Ga 1-X-Y As the red (light with a wavelength of 610 to 700 nm) light emitting element 20, in addition to the nitride-based semiconductor element, GaAlAs, AlInGaP, etc. can be used.

[0091] The thickness of the light emitting element 20 (for example, the height from the lower surface of the support substrate 21 to the upper surface of the semiconductor layer 22 ) is, for example, not less than 100 μm and not more than 300 μm.

[0092] The light emitting element 20 has a pair of element electrodes on the upper surface, and is mounted face-up on the first lead electrode 2a on the bottom surface of the recess 15 of the package 10. Here, one element electrode of the light emitting element 20 is bonded to the first lead electrode 2a via a conductive member such as a wire 23, and the other element electrode is bonded to the second lead electrode 2b via a conductive member such as a wire 24.

[0093] By mounting the light emitting element 20 face up, the semiconductor layer 22 of the light emitting element 20 can be arranged on the upper surface side (in other words, the light extraction surface side of the light emitting device 100 ). This can prevent the side surface of the semiconductor layer 22 from being covered by the first covering member 30 .

[0094] This configuration can reduce the loss of primary light due to reflection from the side surface of the light emitting element 20. In addition, the amount of primary light that can be extracted from the side surface of the light emitting element 20 increases, and the light distribution characteristics of the light emitting device 100 can be further improved.

[0095] The first covering member 30 is provided in the groove of the groove portion 17 and is formed to cover a part of the side surface of the light emitting element 20. The first covering member 30 is formed of a first resin containing a first reflective material. Here, the first covering member 30 is provided with a containing layer 30a containing the first reflective material and a light-transmitting layer 30b not containing the first reflective material in the position of the groove portion 17 from the bottom surface side of the recessed portion 15. The containing layer 30a is provided in the groove of the groove portion 17 and fills the groove of the groove portion 17. By providing the containing layer 30a in the groove of the groove portion 17, the containing layer 30a can be prevented from being opposite to the side surface of the light emitting element 20, and it is easier to reflect light from the light emitting element 20, thereby improving the light emitting efficiency.

[0096] The light-transmitting layer 30b is provided on the containing layer 30a, and covers a part of the second covering member 40. In addition, the light-transmitting layer 30b covers a part of the side surface of the light-emitting element 20, but may cover the entire side surface.

[0097] Here, the side surface of the light emitting element 20 refers to a portion where the side surface of the supporting substrate 21 and the side surface of the semiconductor layer 22 are combined.

[0098] The containing layer 30a is a layer formed by the precipitation of the first reflective material, and the first reflective material is arranged in a high-concentration region in the depth direction of the first covering member 30. The light-transmitting layer 30b is a layer mainly composed of resin formed on the upper side by the precipitation of the first reflective material. That is, no clear interface is formed between the containing layer 30a and the light-transmitting layer 30b.

[0099] The containing layer 30a is preferably provided so as not to cover the side surfaces of the light emitting element 20. With this configuration, the efficiency of extracting light from the side surfaces of the light emitting element 20 is improved, and the light distribution characteristics in the lateral area of ​​the light emitting element 20 can be improved.

[0100] Examples of the resin material used for the first resin include thermosetting resins such as epoxy resins, modified epoxy resins, silicone resins, and modified silicone resins.

[0101] The viscosity of the first resin is preferably 0.3 Pa·s or more and 15 Pa·s or less at room temperature (20±5°C). If the viscosity of the first resin is 0.3 Pa·s or more, it is easy to easily arrange the first resin on the bottom surface of the recess 15 by potting. In addition, if the viscosity of the first resin is 15 Pa·s or less, the shape of the first covering member 30 is easily changed by centrifugal force. It is then easy to use centrifugal force to settle the first reflective material. In addition, in order to obtain the above-mentioned effect, it is more preferable that the viscosity of the first resin is 0.5 Pa·s or more and 6 Pa·s or less.

[0102] The viscosity of the first resin here refers to the viscosity in a state where the first reflective material is contained, and refers to the viscosity before the first reflective material contained in the first resin is precipitated by centrifugal force as described later.

[0103] Examples of the light reflecting material used as the first reflecting material include titanium oxide, silicon dioxide, silicon oxide, aluminum oxide, zirconium oxide, magnesium oxide, potassium titanate, zinc oxide, and boron nitride. Among them, titanium oxide having a relatively high refractive index is preferably used from the viewpoint of light reflection.

[0104] As the first reflective material, it is preferable to use a material having a higher specific gravity than the resin material used for the first resin. By utilizing the difference in specific gravity between the first reflective material and the resin material, it is easy to use centrifugal force to make the first reflective material settle in the groove of the groove portion 17. In addition, by using a material having a large particle diameter as the first reflective material, the first reflective material can be settled in the groove of the groove portion 17 more quickly.

[0105] Furthermore, by using centrifugal force, the first reflective material is densely arranged, so that the intervals between particles become smaller, light leakage and light transmission are suppressed, and the light reflectance in the containing layer 30 a can be improved.

[0106] The particle diameter of the first reflective material is preferably 0.1 μm or more and 1.0 μm or less. If the particle diameter of the first reflective material is 0.1 μm or more, it is easy to precipitate the first reflective material by centrifugal force. In addition, if the particle diameter of the first reflective material is 1.0 μm or less, it is easy to reflect visible light. From the above viewpoint, the particle diameter of the first reflective material is more preferably 0.4 μm or more and 0.6 μm or less.

[0107] The second covering member 40 is a member that reflects light emitted from the light emitting element 20 .

[0108] In order to prevent light emitted from the light emitting element 20 from being transmitted through and absorbed by the bottom and side surfaces of the recess 15 , the surface inside the recess 15 other than where the groove 17 exists is preferably covered with the second covering member 40 .

[0109] The second covering member 40 is formed to cover the side surface of the recess 15 of the package 10. In addition, the second covering member 40 continuously covers the side surface of the recess 15 to the outer upper end edge of the groove 17. That is, the second covering member 40 is continuously covered from the upper end of the side surface of the recess 15 to the outer upper end edge of the groove 17. The second covering member 40 is formed of a second resin containing a second reflective material. Although it is more preferable that the second covering member 40 covers substantially all of the side surface of the recess 15 in the height direction, it is at least preferable that the side surface of the recess 15 is covered in such a manner that the upper end of the second reflective material is higher than the upper surface of the light emitting element 20 when the light emitting device 100 is viewed in cross section. The second covering member 40 is provided between the inner wall surface of the resin wall 3 and the front of the groove 17. In addition, the second covering member 40 is formed so that the upper surface is covered by the light-transmitting layer 30b between the outer side of the groove 17 and a predetermined position.

[0110] The second reflective material of the second covering member 40 is dispersed in the second resin. Here, the second reflective material is dispersed in the second resin to the extent that the reflective material can function as a reflective layer, for example, the dispersed state when the resin containing the reflective material is coated by a conventionally known method. In addition, as long as the second covering member 40 functions as a reflective layer, the second reflective material may be partially offset.

[0111] The content concentration of the second reflective material in the second covering member 40 is, for example, 10 mass % or more and 50 mass % or less.

[0112] By covering the bottom surface and the side surfaces of the recessed portion 15 with the second covering member 40 , it is possible to prevent the bottom surface and the side surfaces of the recessed portion 15 from transmitting and absorbing light.

[0113] As the resin material used for the second resin, for example, thermosetting resins such as epoxy resin, modified epoxy resin, silicone resin, and modified silicone resin can be cited. As the light reflecting material used for the second reflecting material, for example, titanium oxide, silicon dioxide, silicon oxide, aluminum oxide, zirconium oxide, magnesium oxide, potassium titanate, zinc oxide, boron nitride, etc. can be cited. Among them, from the viewpoint of light reflection, it is preferred to use titanium oxide with a relatively high refractive index.

[0114] The light-transmitting member 50 is formed so as to be disposed on the first covering member 30, the light-emitting element 20, and the second covering member 40. The light-transmitting member 50 is formed of a resin that transmits light.

[0115] As the resin material used for the resin of the light-transmitting component 50, for example, thermosetting resins such as epoxy resin, modified epoxy resin, silicone resin, and modified silicone resin can be cited. The resin material used for the resin of the light-transmitting component 50 can be the same resin material as the first resin and the second resin, or a different resin material. In addition, a resin with high heat resistance can be used for the first resin and the second resin, and a hard resin can be used for the resin of the light-transmitting component 50.

[0116] In addition, the first resin is preferably softer than the resin of the light-transmitting member 50. The first resin is a member disposed near the bonding region between the light-emitting element 20 and the substrate 2, and therefore, it is preferred to use a material that is not easily expanded by heat and is flexible to heat to avoid excessive stress due to thermal expansion.

[0117] Compared with epoxy resin, silicone resin generally has higher light resistance at about 450nm and below 500nm, and epoxy resin is harder than silicone resin. Therefore, silicone resin can be used in the first resin and the second resin, and epoxy resin can be used in the resin of the light-transmitting component 50.

[0118] The light-transmitting member 50 may also contain a wavelength conversion member. As the wavelength conversion member, for example, a fluorescent substance can be cited. In addition, the light-transmitting member 50 may also contain a diffusion material, a filler, etc. according to the purpose.

[0119] As the phosphor, a phosphor known in the art can be used. For example, YAG (Y3Al5O 12 :Ce), yellow phosphors such as silicates, red phosphors such as CASN (CaAlSiN3:Eu), KSF (K2SiF6:Mn), or chlorosilicates, BaSiO4:Eu 2+ Green phosphors.

[0120] As the diffusion material, a material known in the art can be used, for example, barium titanate, titanium oxide, aluminum oxide, silicon oxide, etc. can be used.

[0121] [Operation of the light emitting device]

[0122] When the light emitting device 100 is driven, current is supplied from an external power source to the light emitting element 20 via the first lead electrode 2a and the second lead electrode 2b, and the light emitting element 20 emits light. The light emitted by the light emitting element 20, which travels upward, is taken out to the outside above the light emitting device 100. In addition, the light traveling downward is reflected by the containing layer 30a and the second covering member 40, and is emitted in the direction of the opening of the recess 15 and is taken out to the outside of the light emitting device 100. In addition, the light traveling in the lateral direction is reflected by the second covering member 40, and is emitted in the direction of the opening of the recess 15 and is taken out to the outside of the light emitting device 100. Thus, it is possible to minimize the leakage of light emitted from the light emitting element 20 from the bottom and side surfaces of the recess 15, and the light extraction efficiency of the light emitting device 100 is improved. In addition, the light emitting device 100 reduces color unevenness. In addition, since the light emitting device 100 is provided with the containing layer 30a in the groove of the groove portion 17, the extraction efficiency is improved, and the light emission efficiency is improved.

[0123] [Method of Manufacturing Light Emitting Device 100]

[0124] Next, an example of a method for manufacturing the light emitting device according to the embodiment will be described.

[0125] Figure 2 This is a flowchart of a method for manufacturing a light-emitting device according to an embodiment. Figure 3A It is a cross-sectional view showing a step of placing a light-emitting element in the method for manufacturing a light-emitting device according to an embodiment. Figure 3B It is a cross-sectional view showing a step of forming a second covering member in the method for manufacturing a light emitting device according to the embodiment. Figure 3C It is a cross-sectional view showing a step of filling a first resin in the method for manufacturing a light emitting device according to an embodiment. Figure 3D It is a schematic diagram showing a step of forming a first covering member in the method for manufacturing a light emitting device according to the embodiment, and is a schematic diagram showing a step of settling a first reflecting material by utilizing centrifugal force. Figure 3E It is a cross-sectional view showing a step of forming a first covering member in the method for manufacturing a light emitting device according to an embodiment, and is a cross-sectional view showing a state after the first reflecting material is precipitated by centrifugal force. Figure 3F It is a cross-sectional view showing a step of forming a light-transmitting member in the method for manufacturing a light-emitting device according to an embodiment.

[0126] The manufacturing method of the light emitting device 100 includes: a step of preparing a substrate 2 having a groove portion 17 surrounding a first region 16, i.e., a step of preparing a substrate S101; a step of placing a light emitting element 20 on the first region 16, i.e., a step of placing a light emitting element S102; a step of forming a second covering member 40 by continuously covering the side of the recess 15 to the outer upper edge of the groove portion 17 with a second resin, i.e., a step of forming a second covering member S103; a step of preparing a first resin S104; a step of filling the groove portion 17 with the first resin containing a first reflective material, i.e., a step of filling the groove portion 17 with the first resin containing a first reflective material. The process of forming a first covering part S106 is a process of applying centrifugal force to the first resin to cause the first reflective material contained in the first resin to settle and form a first covering part 30, wherein the first covering part 30 has a containing layer 30a provided in the groove of the groove portion 17 and containing the first reflective material and a translucent layer 30b covering at least a portion of the side surface of the light-emitting element 20; and a process of forming a translucent part 50 on the first covering part 30 and the light-emitting element 20, i.e., a process of forming a translucent part S107.

[0127] In addition, the material, arrangement, etc. of each component are as described in the description of the light emitting device 100 , and thus the description thereof will be appropriately omitted here.

[0128] (Step of preparing substrate)

[0129] The step S101 of preparing a substrate is a step of preparing a substrate having a groove portion 17 surrounding the first region 16 .

[0130] In step S101 , a package 10 is prepared. The package 10 has a recess 15 including a bottom surface formed by the substrate 2 and side surfaces formed by the resin wall 3 .

[0131] In this step S101, first, a groove 17 surrounding the first area 16 is formed in the first lead electrode 2a. The groove 17 can be formed, for example, by etching or pressing. In addition, the first lead electrode 2a and the second lead electrode 2b form a plating layer on the surface by electroless plating or electrolytic plating as needed. In addition, the first lead electrode 2a and the second lead electrode 2b can also form a groove for setting the resin wall 3 when forming the groove 17. Next, the first lead electrode 2a and the second lead electrode 2b are arranged in a mold for package manufacturing, and the resin for forming the resin wall 3 and the resin molded body 2c is injected into the mold, and the resin is cured. Thus, a package 10 having a groove 17 on the substrate 2 is manufactured.

[0132] Alternatively, as step S101 , a substrate having grooves formed in advance may be prepared.

[0133] (Step of placing light emitting element)

[0134] The light emitting element placement step S102 is a step of placing the light emitting element 20 in the first region 16 .

[0135] In step S102, the light emitting element 20 is placed on the bottom surface of the recess 15 of the package 10. Here, the light emitting element 20 is placed on the first lead electrode 2a. The light emitting element 20 uses the electrode forming surface as the main light extraction surface and the surface on the side opposite to the electrode forming surface as the mounting surface, and is mounted on the bottom surface of the recess 15 with a non-conductive adhesive material facing up. As the non-conductive adhesive material, for example, an adhesive material such as epoxy resin, silicone resin, etc. can be used. In addition, the light emitting element 20 can also be mounted by flip chip, in which case, it is mounted using a conductive adhesive material. As the conductive adhesive material, for example, eutectic solder, conductive paste, bumps, etc. can be used.

[0136] (Step of Forming Second Covering Member)

[0137] The second covering member forming step S103 is a step of forming the second covering member 40 by continuously covering the side surfaces of the recessed portion 15 to the outer upper edge of the groove portion 17 with the second resin.

[0138] In this step S103, the second resin covering the side of the recess 15 is arranged by potting, for example. The arrangement of the second resin to the recess 15 can be performed by discharging an uncured resin material from a nozzle at the front end of a resin discharging device filled with the second resin to the vicinity of the outer edge of the bottom surface of the recess 15 (preferably the boundary with the side surface). The uncured second resin wets and spreads on the side surface of the recess 15, covering the side surface of the recess 15. At this time, the second resin also flows on the bottom surface of the recess 15, so the second resin covers a part of the bottom surface of the recess 15. Here, it is preferable to adjust the viscosity and arrangement position of the second resin so that the second resin flowing on the bottom surface of the recess 15 reaches the outer upper edge of the groove 17 and does not wet and spread in the groove 17, and climbs up to the upper side of the side surface of the recess 15. In the case of forming the second covering member 40 by potting, the viscosity of the second resin is adjusted to be, for example, 1 Pa·s or more and 50 Pa·s or less at room temperature (20±5°C).

[0139] If the second resin flows in groove 17 , there is a concern that the second resin may flow over the inner upper edge of groove 17 and spread to the side of light emitting element 20 , thereby preventing light from being extracted from the side. Therefore, it is preferred that the second resin does not cover the inside of groove 17 .

[0140] In addition, the package 10 can also be preliminarily treated by soaking the inner surface of the recess 15 with an organic solvent. By soaking the inner surface of the recess 15 with an organic solvent, the second resin can be promoted to climb up the side of the recess 15. In addition, even if a material with high wettability is used on the side of the recess 15, or the surface of the side is roughened, climbing up the side of the recess 15 can be promoted.

[0141] The second reflective material is mixed in the second resin before curing, and the content concentration of the second reflective material in the second resin is preferably 10% by mass or more and 50% by mass or less.

[0142] The second resin is disposed near the outer edge of the bottom surface of the recess 15 by potting, so that the second resin wets and spreads on the side surface of the recess 15. In this case, the second cover member 40 is in a state where the second reflective material is dispersed in the second resin.

[0143] Thereafter, the second resin is cured at a temperature of, for example, 120° C. to 200° C. to form the second covering member 40 . The second resin is preferably cured after the second resin has wetted and diffused on the side surfaces of the recess 15 while the package is left standing.

[0144] (Step of Preparing First Resin)

[0145] The step S104 of preparing the first resin is a step of mixing a main component of a two-liquid curable resin material and a first reflective material, and then mixing a curing agent after a certain period of time has passed.

[0146] By using the first resin prepared in this way, the first reflective material and the resin material can be more compatible, and the first reflective material can be easily precipitated by centrifugal force. The temperature before mixing the curing agent is set to about room temperature.

[0147] Examples of the two-component curable resin material include silicone resins, modified silicone resins, epoxy resins, and modified epoxy resins.

[0148] The time elapsed after the main agent of the two-liquid curable resin material is mixed with the first reflective material is preferably 2 hours or more from the viewpoint of making it easier to settle the first reflective material. In addition, the time elapsed is preferably 8 hours or less from the viewpoint of shortening the manufacturing time. In addition, after the curing agent is mixed, the next step is moved to before the first resin is cured.

[0149] The content concentration of the first reflective material relative to the uncured first resin is, for example, approximately 15% by mass or more and 60% by mass or less.

[0150] (Step of Filling with First Resin)

[0151] The first resin filling step S105 is a step of filling the groove of the groove portion 17 with the first resin 31 containing the first reflective material.

[0152] In the process S105, an uncured first resin 31 is arranged between the side of the recess 15 and the outer upper edge of the groove 17, for example, by potting. Specifically, the uncured first resin 31 is arranged on the second covering member 40 that continuously covers from the side of the recess 15 to the outer upper edge of the groove 17. By arranging the first resin on the second covering member 40 near the groove 17, the first resin flows in the groove 17 and fills the groove 17. The uncured first resin 31 is preferably arranged, for example, at two locations near the opposite side surfaces of the light emitting element 20, and flows in the groove under the weight of the first resin itself or the centrifugal force and fills the groove. As a result, the first resin flowing in the groove moves in the groove in parallel with the bottom surface of the recess 15, so that the first resin can be suppressed from wetting and spreading in the vertical direction before the first resin is filled in the groove.

[0153] That is, by not directly pouring the first resin 31 into the groove 17, it is possible to suppress the flow of the first resin toward the light emitting element 20, and suppress the first resin from climbing up the side of the light emitting element 20 before centrifugal rotation. The climbing up of the first resin to the side of the light emitting element 20 can be eliminated by the shape of the first resin changing under centrifugal rotation, but depending on the viscosity of the first resin and the centrifugal rotation speed, there is a concern that the first reflective material in the first resin will remain on the side of the light emitting element 20. Therefore, it is preferable that the first resin before centrifugal rotation does not cover the side of the light emitting element 20.

[0154] Furthermore, when the first resin is difficult to flow in the groove due to the viscosity of the resin or the like, the first resin 31 may be directly placed in the groove by potting or the like.

[0155] (Step of Forming First Covering Member)

[0156] Process S106 for forming a first covering part is the following process: centrifugal force is applied to the substrate in which the first resin is arranged in the groove portion 17, so that the first reflective material contained in the first resin is settled to form a first covering part 30, which has a containing layer 30a arranged in the groove of the groove portion 17 and containing the first reflective material and a light-transmitting layer 30b covering at least a portion of the side surface of the light-emitting element 20.

[0157] In step S106, the substrate 2, i.e., the package 10, is centrifugally rotated in a direction in which a centrifugal force is applied to the bottom surface of the recess 15. By utilizing this centrifugal force, the first reflective material in the first resin is forcibly precipitated on the bottom surface side of the recess 15, thereby forming a containing layer 30a as a sedimentation layer of the first reflective material, in which the first reflective material is densely arranged, and a light-transmitting layer 30b as a supernatant. In this way, by forming the containing layer 30a by centrifugal sedimentation, it is possible to reduce the content of the first reflective material contained in the first resin while arranging the particles of the first reflective material at a high density on the bottom surface side. Thus, the containing layer 30a provided in the groove of the groove portion 17 and the light-transmitting layer 30b covering a portion of the side surface of the light-emitting element 20 can be formed.

[0158] In the step S105 of filling the first resin, when the first resin is made to flow in the groove by utilizing centrifugal force, the centrifugal rotation for making the first resin flow in the groove and the centrifugal rotation performed in the present step S106 can be performed simultaneously.

[0159] like Figure 3D As shown, the rotation of the package 10 is preferably performed by applying centrifugal force to the package 10 by the rotation axis 90 such that the upper surface of the substrate 2, that is, the bottom surface of the recess 15 is on the outside. Specifically, the package 10 is moved in the direction A in which the rotation axis 90 is the axis of revolution so that the upper surface side of the package 10 has the rotation axis 90. In addition, Figure 3D The B direction in FIG. 2 is a direction parallel to the bottom surface of the recessed portion 15 . Figure 3D In FIG. 1 , the B direction is described three times as the package 10 moves, but it is actually continuous.

[0160] The rotation axis 90 is an axis parallel to the bottom surface of the recess 15 and located on a vertical line passing through the approximate center of the bottom surface of the recess 15, and is located on the opening side of the recess 15 relative to the package 10. As a result, centrifugal force acts in the bottom surface direction of the recess 15, and diffusion of the first resin in the height direction of the package 10 is suppressed, and the first reflective material contained in the first resin is moved toward the bottom surface side ( Figure 3D By curing the first resin in this state, a layer 30a containing the first reflective material and a light-transmitting layer 30b are sequentially formed on the bottom surface of the concave portion 15 in the groove portion 17.

[0161] In addition, the amount of the first covering member 30 applied and the content of the first reflective material contained in the first resin can be appropriately adjusted.

[0162] The rotation speed and rotation number when the package 10 is centrifugally rotated also depend on the content of the first reflective material, the particle diameter, etc., but the rotation number and rotation radius may be adjusted so that a centrifugal force of 200×g or more is applied, for example.

[0163] In addition, during the manufacturing process, when the package 10 is centrifugally rotated in the state of the collective substrate before singulation, if the collective substrate is in the form of a flat plate, the larger the flat surface area of ​​the collective substrate (more specifically, the longer the substrate length in the rotation direction A), the more the package 10 at a position away from the center of the collective substrate will deviate from the rotation axis 90. For example, in the collective substrate, if the deviation from the circumference of the revolution to the direction B becomes larger, there is a concern that the surface of the first resin is tilted relative to the bottom surface of the recess 15, and the surface state of the first resin in the collective substrate deviates. In order to suppress this deviation, it can be suppressed by increasing the rotation radius. Specifically, by setting the rotation radius to be more than 70 times the length of the collective substrate arranged in the rotation direction, the deviation can be suppressed.

[0164] In addition, by utilizing centrifugal force, when the assembly substrate uses a flexible resin package 10 that is flexed along the circumference of the rotation radius, the above-mentioned deviation is less likely to occur, so the assembly substrate can be centrifugally rotated with a larger assembly substrate than the assembly substrate of the non-flexible package 10. As a result, the number of pieces that can be processed at one time can be increased. As such an assembly substrate having flexibility, for example, a resin package connected by a lead wire can be cited.

[0165] In addition, in this step S106, it is preferred to solidify the first resin while allowing the first reflective material to settle, that is, while applying centrifugal force. The first reflective material preferably uses a material with a small particle diameter, but the smaller the particle diameter, the more difficult it is to settle, so in this step S106, the first reflective material is forced to settle on the bottom side of the recess 15 by centrifugal force. Therefore, in order to solidify the first reflective material in a settled state, it is preferred to maintain rotation in this step S106, in other words, perform the solidification step of the first resin while rotating.

[0166] Alternatively, the resin can be cured after the rotation is stopped, but if the rotation is stopped, the resin is likely to spread on the side surfaces of the light emitting element 20 due to wettability. Therefore, by curing the first resin while rotating the package 10, it is possible to prevent the first resin from climbing up the side surfaces of the light emitting element 20. By exposing the side surfaces of the light emitting element 20 from the first resin, the light extraction efficiency can be further improved, and the light distribution characteristics of the light emitting device 100 can be further improved.

[0167] At this time, the temperature for curing the first resin can be listed as being above 40°C and below 200°C. By increasing the curing temperature, the time for curing the first resin can be shortened, which is more efficient. In addition, considering that the metal of the centrifugal sedimentation device expands due to heat and causes the rotating shaft 90 to shake, it is preferred that the curing temperature is as low as possible. That is, the temperature for curing the first resin is preferably above 50°C from the perspective of efficiency. In addition, considering the shaking of the rotating shaft 90, the temperature for curing the first resin is preferably below 60°C. When curing at above 80°C, it is preferred to adjust the device so that at least the metal part of the centrifugal rotating device does not become above 80°C.

[0168] In addition, as the resin material constituting the first resin, it is preferable to select a resin material that can at least obtain a temporarily cured state by maintaining the rotating package 10 at a temperature of 40° C. or higher.

[0169] Examples of a method for curing the first resin while allowing the first reflective material to settle include applying hot air and using a plate heater.

[0170] (Step of forming a light-transmitting member)

[0171] The step S107 of forming a light-transmitting member is a step of forming a light-transmitting member 50 on the first covering member 30 , the second covering member 40 , and the light-emitting element 20 .

[0172] In step S107 , the resin of the light-transmitting member 50 is placed in the recess 15 by potting, spraying, etc. Thereafter, the resin of the light-transmitting member 50 is cured at a temperature of, for example, 120° C. to 200° C. to form the light-transmitting member 50 .

[0173] In the above, the light emitting device and the method for manufacturing the light emitting device are specifically described in terms of the embodiments of the invention, but the gist of the invention is not limited to these descriptions and must be interpreted broadly based on the descriptions of the patent claims. In addition, various changes and modifications based on these descriptions are also included in the gist of the invention.

[0174] 《Other Implementation Methods》

[0175] Figure 4 It is a cross-sectional view schematically showing the structure of a light emitting device according to another embodiment. Figure 5A It is a plan view schematically showing the structure of a groove portion of a light emitting device according to another embodiment. Figure 5B It is a plan view schematically showing the structure of a groove portion of a light emitting device according to another embodiment. Figure 5C It is a plan view schematically showing the structure of a groove portion of a light emitting device according to another embodiment.

[0176] Figure 4The light emitting device 100A shown in the figure includes a protection element 60. The protection element 60 includes an element electrode on the upper surface, and is mounted face-up on the second lead electrode 2b on the bottom surface of the recess 15 of the package 10. Here, the electrode of the protection element 60 is bonded to the first lead electrode 2a via a conductive member such as a wire 25. The protection element 60 is, for example, a Zener diode.

[0177] The protection element 60 may be placed on the bottom surface of the recess 15 of the package 10 in the step S102 of placing the light emitting element.

[0178] In addition, the light emitting device may also include a plurality of light emitting elements 20. Moreover, for example, in the case where two light emitting elements 20 are provided, Figure 5A As shown in FIG. 1 , the groove 17 may also be a groove 17 that is rectangular in shape when viewed from above and surrounds two light emitting elements 20. Figure 5B As shown in FIG. 1 , the groove 17 may be a rectangular ring-shaped groove 17 in a plan view, which surrounds the two light emitting elements 20. Figure 5C As shown, the groove 17 may be in a shape in which the grooves 17 of adjacent portions of two light emitting elements 20 are integrated.

[0179] In addition, the light-emitting device described above is configured to mount the light-emitting element face-up, but the light-emitting element may also be mounted flip-chip. In the case of flip-chip mounting the light-emitting element, it is preferred to use a sub-mount, a bump, a columnar electrode, etc. as a pedestal to raise the light-emitting element in the height direction of the light-emitting element. In the case of flip-chip mounting the light-emitting element, the semiconductor layer is arranged on the bottom side of the recess of the substrate (the substrate side of the light-emitting device), but by raising the light-emitting element in the height direction of the light-emitting element, a part or the entire side of the semiconductor layer can be not covered by the first covering member.

[0180] Furthermore, the light emitting device described above uses a package having a recessed portion and places a light emitting element on the bottom surface of the recessed portion. However, the light emitting device may use a flat substrate and place the light emitting element on the substrate.

[0181] In addition, the method for manufacturing a light emitting device may include other steps during or before or after each of the steps, within the range that does not negatively affect each of the steps, such as a foreign matter removal step for removing foreign matter mixed in during the manufacturing process.

[0182] In addition, in the method for manufacturing a light-emitting device, the order of some processes is not limited, and the order can be changed. For example, the method for manufacturing a light-emitting device includes a process for preparing a first resin after the process for forming a second covering member, but the process for preparing the first resin can be performed before the process for forming the second covering member, before the process for placing a light-emitting element, or before the process for preparing a substrate. In addition, the process for preparing the first resin can be omitted.

[0183] In addition, the process of forming the second covering part is performed after the process of placing the light-emitting element and before the process of preparing the first resin, but the process of forming the second covering part can also be performed before the process of placing the light-emitting element, or can also be performed after the process of forming the first covering part and before the process of forming the translucent part.

[0184] [Example]

[0185] Hereinafter, examples will be described.

[0186] Figure 6 is an image showing the structure of the light emitting device used in the first embodiment. Fig. 7A : is a graph showing the relationship between the coating amount of the first resin and the light beam in the first embodiment. Figure 7B : is a graph showing the deviation of the chromaticity coordinate x according to the directivity angle in the first embodiment. Figure 7C : is a graph showing the deviation of the chromaticity coordinate y according to the directivity angle in the first embodiment. Fig.7D : is a graph showing the deviation of the chromaticity coordinate x according to the directivity angle in the first embodiment. Fig. 7E : is a graph showing the deviation of the chromaticity coordinate y according to the directivity angle in the first embodiment. Fig. 8A This is an image showing a state of the light emitting device used in the second embodiment after a light emitting element is mounted and a second resin is applied. Figure 8B This is an image showing a state after further coating of the first resin, regarding the light emitting device used in the second embodiment. Figure 8C This is an image showing a state in which a centrifugal force is further applied to the first resin and the reflective material is centrifugally precipitated, with respect to the light emitting device used in the second embodiment. Fig.8D It is an image showing element electrodes of the light emitting device used in the second embodiment. Fig. 8E This is an image showing a state after a light-transmitting member is formed with respect to the light-emitting device used in the second embodiment. Fig.9A : is a graph showing the relationship between the color tone and the light beam in the second embodiment. Fig. 9B This is a graph showing the relationship between each sample and the light beam in the second example.

[0187] [First embodiment]

[0188] Produced Figure 6 A light emitting device of the structure shown. Figure 6 The light emitting devices of the structure shown are substantially the same except that the coating amount of the first resin is different. First, a package having a groove formed on the bottom surface of the recess is prepared. A first lead electrode and a second lead electrode are arranged on the bottom surface of the recess, and the groove is formed on the first lead electrode. The lead electrode is plated with Au. The groove is substantially semicircular in cross-section with a width of 100 μm and a depth of 100 μm.

[0189] Next, a light emitting element is placed on the bottom surface of the recess. Next, the bottom surface and the side surface of the recess are covered with a second resin containing a second reflective material to form a second covering member. Next, regarding the embodiment, a first resin containing a first reflective material is filled in the groove of the groove portion, and the first reflective material is solidified after being precipitated by centrifugal sedimentation to form a first covering member. The amount of the first resin applied is as follows: Figure 6 , Figure 7A to Figure 7E The coating positions D were set at 2 points. Figure 7B to Figure 7E The value of the item column is the coating amount of the first resin. The concentration of the first reflective material contained in the first resin is set to 37.5% by mass. In addition, in the comparative example, the first covering member is not provided. Next, a translucent member containing a fluorescent body is formed on the first covering member, the second covering member, and the light-emitting element.

[0190] As the light-emitting element, a nitride semiconductor element with a peak emission wavelength of about 442 nm was used. As the first reflective material, titanium oxide with an average particle diameter of about 280 nm was used, and as the second reflective material, titanium oxide with an average particle diameter of about 500 nm was used. YAG:Ce was used as the phosphor. As the first resin, a silicone resin with a resin viscosity of 3.5 Pa·s was used, as the second resin, a silicone resin with a resin viscosity of 1.0 Pa·s was used, and as the resin of the light-transmitting component, a silicone resin with the same resin viscosity of 3.5 Pa·s as the first resin was used.

[0191] For each sample thus produced, the light beam at the hue x=0.32 was measured. The light beam was measured using a total light beam measuring device using an integrating sphere, and the light beam of the light emitting device of the comparative example was set as 100%, and the relative light beam of each sample was calculated. The results are shown in Fig. 7A In. Fig. 7AAs shown in the figure, the sample in which the first covering member is provided in the groove of the groove portion has a higher light beam than the sample in which the first covering member is not provided in the groove of the groove portion. In addition, in the sample of the embodiment, compared with the case where the first covering member is formed without a groove portion, the first resin before the first reflective material is centrifugally precipitated does not flow on the light emitting element side. Therefore, the operation in the manufacturing process is simple and the mass production is excellent.

[0192] In addition, for each sample, the deviation of the chromaticity coordinates x and y based on the directivity angle was measured as a reference. Figure 1A The light distribution chromaticity Δx and Δy are respectively expressed in the direction (0° direction) perpendicular to the IC-IC line. Figure 7B , Figure 7C In the example, the pointing angle will be Figure 1A The light distribution chromaticity Δx and Δy are respectively expressed in the case where the direction of the IC-IC line (90° direction) is taken as the reference. Fig.7D , Fig. 7E Here, the light distribution chromaticity Δx and Δy are based on the chromaticity coordinates in the front direction and represent the deviation of the chromaticity coordinates based on the directional angle of the light emitting device. Figure 7B to Figure 7E As shown, no significant difference was found in the light distribution chromaticity Δx and Δy between the sample in which the first covering member was provided in the groove and the sample in which the first covering member was not provided in the groove.

[0193] That is, in the sample of the embodiment, since the containing layer containing the first reflective material is formed in the groove by centrifugal sedimentation, almost all of the side surface of the light emitting element is exposed from the containing layer, so the light extraction from the side surface of the light emitting element is not hindered by the containing layer. Therefore, the light distribution chromaticity is not deteriorated, and only the light beam can be improved.

[0194] [Second embodiment]

[0195] According to the method for manufacturing the light emitting device of the first embodiment, each sample was manufactured. In the second embodiment, as an example, nine samples were manufactured using a technical machine I (rotation radius 0.65 m) with a rotation speed of 700 rpm to centrifuge the first reflective material, and nine samples were manufactured using a technical machine II (rotation radius 0.1 m) with a rotation speed of 3000 rpm to centrifuge the first reflective material. The first resin coating amount was set to 0.09 mg in all cases. In addition, as a comparative example, nine samples were manufactured in which the first covering member was not provided in the groove of the groove portion (no centrifugal sedimentation). Figure 8A to Figure 8E These are images of each production process of a sample using technical machine I.

[0196] The relationship between the color tone and the light beam was investigated for each sample thus produced. The light beam was measured using a full light beam measuring device using an integrating sphere at room temperature of about 25°C. The results are shown in Fig.9AIn addition, according to Fig.9A As a result, the light beam with hue x = 0.32 is calculated. The result is shown in Fig. 9B In. Fig. 9B As shown, the sample with the first cover member provided in the groove of the groove portion has a higher beam than the sample without the first cover member provided in the groove of the groove portion. In addition, the sample using the technology machine II having a higher centrifugal force than the technology machine I has a higher beam.

[0197] Industrial Applicability

[0198] The light-emitting device of the embodiment of the present disclosure can be used as a backlight light source of a liquid crystal display, various lighting fixtures, large displays, advertisements, destination guides and other display devices, and further as an image reading device in a digital camera, fax machine, copier, scanner, etc., a projector device, etc.

Claims

1. A light emitting device, It is characterized in that have: a substrate having a groove portion surrounding the first region; A light emitting element placed in the first region; a first covering member disposed in the groove of the groove portion and covering at least a portion of a side surface of the light emitting element; a light-transmitting member disposed on the first covering member and the light-emitting element; The first covering member is formed by applying centrifugal force to a first resin containing a first reflecting material to cause the first reflecting material contained in the first resin to settle, and comprises a containing layer and a light-transmitting layer, wherein the containing layer is arranged in the groove of the groove portion and contains the first reflecting material, and the light-transmitting layer covers at least a portion of the side surface of the light-emitting element.

2. The light emitting device according to claim 1, It is characterized in that The light emitting device comprises a package having a recessed portion formed by a bottom surface formed by the substrate and a side surface formed by a resin wall, and further comprises a second covering member that continuously covers from the side surface of the recessed portion to the outer upper end edge of the groove portion and contains a second reflecting material.

3. The light emitting device according to claim 1 or 2, It is characterized in that The width of the groove is greater than or equal to 30 μm and less than or equal to 200 μm.

4. The light emitting device according to claim 1 or 2, It is characterized in that The depth of the groove is not less than 10 μm and not more than 150 μm.

5. The light emitting device according to claim 1 or 2, It is characterized in that The groove portion is formed at a position that is 100 μm or less from the light emitting element.

6. The light emitting device according to claim 1 or 2, It is characterized in that The light-transmitting component includes a wavelength conversion component.

7. A method for manufacturing a light emitting device, It is characterized in that Including the following processes: preparing a substrate having a groove portion surrounding a first region; A light emitting element is placed in the first region; filling a first resin containing a first reflective material in the groove of the groove portion; Applying centrifugal force to the first resin to cause the first reflective material contained in the first resin to settle, thereby forming a first covering member, the first covering member comprising a containing layer and a light-transmitting layer, the containing layer being disposed in the groove of the groove portion and containing the first reflective material, and the light-transmitting layer covering at least a portion of a side surface of the light-emitting element; A light-transmitting member is formed on the first covering member and the light-emitting element.

8. The method for manufacturing a light emitting device according to claim 7, It is characterized in that In the process of preparing the substrate, a package is prepared, which has a recessed portion formed by a bottom surface formed by the substrate and a side surface formed by a resin wall, and before the process of filling the first resin, a process is included to form a second covering part by continuously covering the side surface of the recessed portion to the outer upper end edge of the groove portion with a second resin.

9. The method for manufacturing a light emitting device according to claim 7 or 8, It is characterized in that In the step of forming the first covering member, the first resin is cured in a state where the centrifugal force is applied.

10. The method for manufacturing a light emitting device according to claim 9, It is characterized in that The temperature for curing the first resin is 40° C. or higher and 200° C. or lower.

11. The method for manufacturing a light emitting device according to claim 7 or 8, It is characterized in that The viscosity of the first resin is 0.3 Pa·s or more and 15 Pa·s or less.

12. The method for manufacturing a light emitting device according to claim 7 or 8, It is characterized in that Before the step of filling the first resin, the step of preparing the first resin is included. In the step of preparing the first resin, a main component of a two-component curable resin material and the first reflective material are mixed, and a curing agent is mixed after 2 hours or more.

13. The method for manufacturing a light emitting device according to claim 7 or 8, It is characterized in that The light-transmitting component includes a wavelength conversion component.