A ceramic integrated packaging shell and its manufacturing process

By introducing a stress release layer and a nickel-coated layer into the metal film wiring layer of the ceramic substrate, and brazing with gold and tin solder, the problems of cracking and sealing failure of the welding area of ​​the ceramic integrated packaging shell are solved, and the seal reliability is improved and production pass rate, meeting the requirements of high temperature environment testing.

CN111446212BActive Publication Date: 2024-12-06NO 43 INST OF CHINA ELECTRONICS TECH GRP CETC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202010302088.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-04-16
Publication Date
2024-12-06
Estimated Expiration
2040-04-16

AI Technical Summary

Technical Problem

The existing thick film mixed multi-layer ceramic integrated packaging shell has problems such as cracking of welding zones, seal failure risks and poor seal reliability during the welding process, and the process window is narrow and cannot meet the requirements of high-temperature environmental testing.

Method used

Introduce a stress release layer, such as Au or Cu, into the metal film wiring layer of the ceramic substrate, as part of the metal film wiring layer, to release welding stress during welding, avoid damage to the ceramic and the underlying film Ti layer, and to the metal The surface of the enclosure is coated with nickel and gold layers, and is brazed with gold-tin solder to ensure sealing.

Benefits of technology

Effectively improve the seal reliability of ceramic substrate and metal frame gold-tin brazing. After the environmental test of temperature circulating 100 times and thermal shock of -65℃ to +175℃ for 15 times, the airtightness is better than that of 1.0×10-9Pa.m3.s-1 broadens the production process window and improves the production pass rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111446212B_ABST
    Figure CN111446212B_ABST
Patent Text Reader

Abstract

The present invention discloses a ceramic integrated package shell and its manufacturing process, which is composed of a thick film ceramic substrate and a metal film wiring layer arranged on the surface of the thick film ceramic substrate, characterized in that the metal film wiring layer is a six-layer film system of Ti / M / N / Ti / K / Au from the inside to the outside, wherein the M layer and the K layer are independently selected from Pt or Ni, and the N layer is a stress release layer, and the stress release layer is Au or Cu. The ceramic integrated package shell in the present invention has high sealing reliability and good air tightness, and broadens the production process window of thick film hybrid multilayer ceramic integrated package shell, and improves the production qualification rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electronic packaging shells, and in particular relates to a ceramic integrated packaging shell and a manufacturing process thereof. Background Art

[0002] Electronic packaging shell refers to the shell used to install semiconductor integrated circuit chips. On the one hand, it plays the role of placing, fixing, sealing, protecting chips and enhancing thermal conductivity. On the other hand, it is also a bridge between the internal world of the chip and the external circuit. Specifically, the contacts on the chip are connected to the pins of the packaging shell with wires, and these pins are connected to other devices through wires on the printed circuit board. Therefore, for many integrated circuit products, the packaging technology of electronic packaging shells is a very critical link.

[0003] In order to match the development trend of miniaturization, integration and high frequency of RF components, the integrated packaging shell with a certain enclosed space formed by the combination of thick-film hybrid multilayer ceramic substrate and metal frame is becoming more and more widely used. The characteristics of thick-film ceramic substrate are easy multi-layer wiring and can be interconnected in three dimensions, but its disadvantage is that the microwave transmission loss is relatively large, and the line width and line spacing are generally above 50 microns; while the metallization flatness of thin-film ceramic substrate is higher, the microwave transmission loss is relatively small, the line width and line spacing can be about 20 microns, which meets the requirements of high-density wiring. Its disadvantage is that only thin-film metallization can be done on the surface of ceramic. Thick-film hybrid multilayer ceramic substrate combines the advantages of the above two. For the inner layer circuit, thick film process is used to achieve multi-layer wiring, and for the surface circuit, thin-film circuit is used to meet the requirements of high-density wiring and lower microwave transmission loss. Therefore, it is widely used in the field of high-reliability packaging.

[0004] At present, the common manufacturing process of thick-film hybrid multilayer ceramic integrated package shell in the industry is to use magnetron sputtering method to sputter Ti / Pt / Au thin film wiring layer or Ti / Ni / Au thin film wiring layer from the inside to the outside on the surface of the ceramic substrate, and then weld the metal frame ring frame with gold tin or lead tin on the surface of the ceramic substrate along the four sides of the thin film metallization layer to form an integrated package shell structure. In this thin film system, the thin film Ti layer is the adhesion layer of the ceramic, the thin film Pt or Ni layer is the welding barrier layer and the wetting layer of the solder, and the thin film Au layer is used as an anti-oxidation layer to protect the Ti, Pt and Ni layers. However, this process also has certain problems. For example, when using lead-tin alloy solder for brazing, due to the melting temperature of the solder of 163°C, the subsequent use temperature of the thick-film hybrid multilayer ceramic integrated package shell cannot exceed 163°C (to avoid failure due to secondary melting of the lead-tin alloy), and the use of the shell is greatly restricted, and it cannot meet the above-mentioned environmental test requirements. However, if a higher temperature gold-tin eutectic solder is used for brazing (gold-tin eutectic solder has a melting point of 280°C), the intermediate phase generated by gold-tin brazing is relatively brittle, and there is a risk of cracking in the welding area and sealing failure in the ceramic integrated packaging shell. The reliability of the integrated packaging shell is poor and the pass rate is low.

[0005] In addition, when soldering chips with gold and tin on the ceramic thin film wiring layer, vacuum welding or eutectic friction welding in air atmosphere is generally used. After the actual solder melts, it needs to be cooled quickly (the solder melting point is kept above the heat preservation time within 1 minute during soldering). The process window is narrow and does not involve indicators such as airtightness. While the thick film hybrid multi-layer ceramic integrated package shell serves as a mechanical support carrier for the internal circuit, it also plays a role in sealing and protecting the internal circuit, and its airtightness requirements must meet the requirements. Summary of the invention

[0006] In view of this, it is necessary for the present invention to provide a ceramic integrated packaging shell and its manufacturing process. The ceramic integrated packaging shell in the present invention is provided with a stress release layer in the thin film system, and the stress release layer is fully utilized. When the welding stress is transmitted to the stress release layer, the material therein is soft and easy to plastically deform, and the welding stress can be effectively released, thereby avoiding the damage to the adhesion between the ceramic and the underlying thin film Ti layer, and solving the technical problems of welding cracking, sealing failure risk and poor sealing reliability of the integrated packaging shell in the prior art.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A ceramic integrated packaging shell comprises a thick-film multilayer ceramic substrate, wherein the thick-film multilayer ceramic substrate is composed of a thick-film ceramic substrate and a metal film wiring layer arranged on the surface of the thick-film ceramic substrate, wherein the metal film wiring layer is a six-layer film system of Ti / M / N / Ti / K / Au from the inside to the outside, wherein the M layer and the K layer are independently selected from Pt or Ni, and the N layer is a stress release layer, and the stress release layer is Au or Cu.

[0009] Furthermore, it also includes a metal frame, which is arranged on the thick-film multilayer ceramic substrate, and a gold-tin soldering layer is arranged between the metal frame and the thick-film multilayer ceramic substrate.

[0010] Furthermore, the material of the metal frame is selected from one of 4J42, 4J33, and 4J29 fixed expansion alloys, and the surface of the metal frame is provided with a nickel layer and a gold layer in sequence from the inside to the outside.

[0011] Preferably, on the surface of the metal frame, the thickness of the nickel layer is 1.27-8.9 μm, and the thickness of the gold layer is 0.75-5.7 μm.

[0012] Furthermore, the thick film ceramic substrate is selected from one of an alumina ceramic substrate, an aluminum nitride ceramic substrate, and a LTCC substrate.

[0013] Preferably, the stress release layer is Au.

[0014] Furthermore, in the metal thin film wiring layer, the thickness of the Ti layer is 0.1-0.6 μm, the thickness of the M layer and the K layer is 1-3 μm, and the thickness of the N layer is 0.75-3 μm.

[0015] Another object of the present invention is to provide a process for manufacturing the aforementioned ceramic integrated packaging shell, comprising the following steps:

[0016] Green porcelain is obtained by pressing and casting, the green porcelain is sintered or patterned to prepare a thick film ceramic substrate with built-in passive components, and the surface of the thick film ceramic substrate is ground and polished;

[0017] A metal thin film wiring layer is produced by sputtering from the inside to the outside on the surface of the processed thick film ceramic substrate by magnetron sputtering, and a required metallization pattern is prepared on the metal thin film wiring layer to obtain a thick-film hybrid multilayer ceramic substrate;

[0018] A nickel layer and a gold layer are plated on the surface of the metal frame from the inside to the outside in sequence;

[0019] Placing a gold-tin solder sheet and a metal frame in sequence on the metal film wiring layer of the thick-film hybrid multilayer ceramic substrate to form an integrated package shell pre-assembly;

[0020] The integrated packaging shell pre-assembly is sent into a brazing furnace and brazed into a whole under a protective atmosphere.

[0021] Furthermore, the brazing process includes a preheating process, a heat preservation process and a cooling process in sequence.

[0022] Preferably, the specific process of brazing is: first, heat up from room temperature to 250-270°C at a heating rate of 20-30°C / min, and keep warm for 5-10min; then heat up to 300-330°C at a heating rate of 20-30°C / min, and keep warm for 2-10min; finally, cool down at a cooling rate of 10-20°C / min, and the ceramic integrated packaging shell is obtained when it is taken out of the furnace.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] A six-layer film system is used between the thick film ceramic substrate and the metal frame. A metal with a soft material and easy plastic deformation is added to the film system as a stress release layer, so that the welding stress is transferred to the stress release layer. Since the material in this layer is soft and easy to plastic deformation, the welding stress can be effectively released, avoiding the damage to the adhesion and bonding between the ceramic and the bottom film Ti layer. In this way, the sealing reliability of the thick film ceramic substrate and the metal frame gold-tin brazing in the mass production of the thick film hybrid multilayer ceramic integrated packaging shell is improved. The shell is based on the test requirements of GJB2440A-2006 <General Specification for Hybrid Integrated Circuit Shell>, and the airtightness is better than 1.0×10 -9 Pa.m 3 .s -1 At the same time, it also broadens the production process window of thick-film hybrid multi-layer ceramic integrated packaging shells and improves the production qualification rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic structural diagram of a thick-thin-film hybrid multi-layer ceramic integrated packaging shell in a preferred embodiment of the present invention;

[0026] Figure 2 for Figure 1 A partial enlarged schematic diagram of the metal film wiring layer 20;

[0027] Figure 3 The figure is a flowchart of a manufacturing process of a thick-thin-film hybrid multilayer ceramic integrated packaging shell in a preferred embodiment of the present invention.

[0028] In the figure: 10 - thick film ceramic substrate, 20 - metal thin film wiring layer, 30 - gold-tin solder layer, 40 - metal frame, 201 - Ti layer, 202 - M layer, 203 - N layer, 204 - K layer, 205 - Au layer. DETAILED DESCRIPTION

[0029] For ease of understanding of the present invention, the present invention will be described more fully below in conjunction with specific embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0031] The first aspect of the present invention discloses a thick-film hybrid multilayer ceramic integrated packaging shell, which includes a thick-film multilayer ceramic substrate, which is composed of a thick-film ceramic substrate and a metal film wiring layer arranged on the thick-film ceramic substrate, and the metal film wiring layer is a six-layer thin film system of Ti / M / N / Ti / K / Au from the inside to the outside, wherein the M layer and the K layer are independently selected from Pt or Ni, and the N layer is a metal with a soft material and easy plastic deformation.

[0032] When the existing traditional ceramic surface Ti / Pt / Au or Ti / Ni / Au three-layer film is brazed with the metal frame by gold-tin eutectic brazing, the thin film Au layer will dissolve into the gold-tin solder, and the Ni or Pt thin film layer as a diffusion barrier layer will undergo metallurgical reaction with the Sn element in the gold-tin solder to form a brittle intermediate phase. Although the existence of the intermediate phase ensures that the connection between the metal frame and the ceramic has a certain mechanical strength, the brittle intermediate phase cannot release the welding stress, which will further affect the bonding of the thin film Ti layer as the adhesion layer with the ceramic. This makes the process window for gold-tin brazing of the ceramic and the metal frame relatively narrow, and there is a risk of cracking in the welding area and sealing failure in the ceramic integrated packaging shell, and the sealing reliability is poor.

[0033] In view of the above problems, the present invention adopts a six-layer thin film system of Ti / M / N / Ti / K / Au low stress on the surface of the thick-film hybrid multilayer ceramic substrate, wherein the N layer is a metal with a soft material and easy plastic deformation, and the plasticity of the metal in the N layer is fully utilized to use the N layer as a stress release layer. Under the same conditions, although the welding stress still exists when the metal frame is connected to the ceramic by gold-tin brazing, when the welding stress is transmitted to the middle N layer in the present invention, the welding stress can be effectively released due to the soft material and easy plastic deformation, thereby avoiding the damage to the adhesion and bonding between the ceramic and the bottom thin film Ti layer. It can be understood that the stress release layer here is a specific example that can be mentioned, including Au or Cu.

[0034] The ceramic integrated package shell of the present invention improves the sealing reliability of the gold-tin brazing of the ceramic substrate and the metal frame in mass production. The shell is tested according to the test requirements of GJB2440A-2006 <General Specification for Hybrid Integrated Circuit Shell> and has an airtightness better than 1.0×10 -9 Pa.m 3 .s -1 At the same time, it broadens the production process window of thick-film hybrid multi-layer ceramic integrated packaging shells and improves the production qualification rate.

[0035] Furthermore, the thick film ceramic substrate may be a common choice in the field of electronic housing packaging, and specific examples include but are not limited to one of an alumina ceramic substrate, an aluminum nitride ceramic substrate, and a LTCC substrate.

[0036] Furthermore, the ceramic integrated packaging shell in the present invention further comprises a metal frame, which is arranged on the surface of the thick-film multilayer ceramic substrate, and a gold-tin soldering layer is arranged between the metal frame and the thick-film multilayer ceramic substrate.

[0037] Further, the material of the metal frame is selected from one of 4J42, 4J33, and 4J29 constant expansion alloys, and the surface of the metal frame is provided with a nickel layer and a gold layer in sequence from the inside to the outside. Here, the material of the metal frame can be a conventional choice in the art, preferably a frame material with a thermal expansion coefficient close to that of the ceramic substrate material, so as to reduce the gold-tin welding stress. In some specific embodiments of the present invention, it can be selected from one of 4J42, 4J33, and 4J29 constant expansion alloys.

[0038] Furthermore, on the surface of the metal frame, the thickness of the nickel layer is 1.27-8.9 μm, and the thickness of the gold layer is 0.75-5.7 μm.

[0039] Furthermore, the stress release layer is Au.

[0040] Furthermore, in the metal thin film wiring layer, the thickness of the Ti layer is 0.1-0.6 μm, the thickness of the M layer is 1-3 μm, and the thickness of the N layer is 0.75-3 μm.

[0041] Another aspect of the present invention discloses a process for manufacturing the thick-thin film hybrid multilayer ceramic integrated package shell as described in the first aspect of the present invention, comprising the following steps:

[0042] Green porcelain is obtained by pressing and casting, and the green porcelain is sintered or printed with patterns to prepare a thick-film ceramic substrate with built-in passive components, and the surface of the thick-film ceramic substrate is ground and polished; it can be understood that pressing and casting to obtain green porcelain, sintering and printing patterns, and grinding and polishing the surface of the thick-film ceramic substrate are conventional means in the field. The specific process varies depending on the material of the substrate. These are all conventional means possessed by technical personnel in this field, and therefore, they are no longer specifically limited here.

[0043] A metal thin film wiring layer is produced by sputtering from the inside to the outside on the surface of the processed thick film ceramic substrate by magnetron sputtering, and a required metallization pattern is prepared on the metal thin film wiring layer to obtain a thick-film hybrid multilayer ceramic substrate; it can be understood that the magnetron sputtering and the preparation of the metallization pattern here belong to the existing technology in this field, and can be adjusted according to the different metals to be sputtered, so no specific limitation is given here.

[0044] A nickel layer and a gold layer are plated on the surface of the metal frame from the inside to the outside in sequence;

[0045] Placing a gold-tin solder sheet and a metal frame in sequence on the metal film wiring layer of the thick-film hybrid multilayer ceramic substrate to form an integrated package shell pre-assembly;

[0046] The integrated package shell pre-assembly is sent into a brazing furnace and brazed into a whole under a protective atmosphere. The protective atmosphere here mainly provides an oxygen-free environment during the brazing process, so the protective atmosphere here can be selected from one of nitrogen and inert gas.

[0047] Furthermore, the brazing process includes a preheating process, a heat preservation process and a cooling process in sequence. It is understandable that the temperature and time of the preheating, heat preservation and cooling process can be adjusted according to the substrate material, etc., and therefore, no specific limitation is made here.

[0048] Preferably, in some specific embodiments of the present invention, the specific process of brazing is: first, the temperature is raised from room temperature to 250-270°C at a heating rate of 20-30°C / min, and then kept warm for 5-10 minutes; then the temperature is raised to 300-330°C at a heating rate of 20-30°C / min, and kept warm for 2-10 minutes; finally, the temperature is lowered at a cooling rate of 10-20°C / min, and the ceramic integrated packaging shell is obtained when it is taken out of the furnace. The brazing process of the present invention first preheats and then keeps warm, so as to ensure that the shell preassembly is heated evenly before the solder melts. When cooling, since the stress release layer is a metal that is soft and easy to plastically deform, in order to avoid failure caused by welding stress, the temperature is directly lowered from a high temperature, thereby shortening the overall process production time and improving production efficiency.

[0049] The technical solution of the present invention is described more clearly and completely below in conjunction with specific embodiments.

[0050] like Figure 1 As shown in the figure, a ceramic integrated package shell includes a thick-film hybrid multilayer ceramic substrate, which is composed of a thick-film ceramic substrate 10 and a metal film wiring layer 20. The metal film wiring layer 20 is arranged on the surface of the thick-film ceramic substrate 10. In this embodiment, magnetron sputtering is used. It can be understood that as long as the technical solution of the present invention can be realized, other methods of making the metal film wiring layer 20 in the field can also be used in the present invention. Please continue to refer to Figure 1 A metal frame 40 is provided on the metal film wiring layer 20, and a gold-tin solder layer 30 is provided between the metal frame 40 and the metal film wiring layer 20, so as to ensure the sealing reliability and airtightness of the ceramic integrated packaging shell.

[0051] Furthermore, the thick film ceramic substrate 10 is selected from one of an alumina ceramic substrate, an aluminum nitride ceramic substrate, and a LTCC substrate.

[0052] Furthermore, the material of the metal frame 40 is selected from one of 4J42, 4J33, and 4J29 fixed expansion alloys, and the surface of the metal frame is provided with a nickel layer and a gold layer from the inside to the outside. Specifically, in this embodiment, the thickness of the nickel layer is 1.27-8.9μm, and the thickness of the gold layer is 0.75-5.7μm.

[0053] For details, please combine Figure 1 and Figure 2In this embodiment, the metal thin film wiring layer 20 is a six-layer thin film system, which includes Ti layer 201, M layer 202, N layer 203, Ti layer 201, K layer 204, and Au layer 205 from the inside to the outside, wherein M layer 202 and K layer 204 are independently selected from Pt or Ni, and N layer 203 is selected from metals with soft materials and easy plastic deformation, which can be Au or Cu, and is preferably Au in this embodiment. Preferably, in the metal thin film wiring layer 20, the thickness of each metal layer is different. In some specific embodiments of the present invention, preferably, in the metal thin film wiring layer 20, the film thickness of Ti layer 201 is 0.1-0.6μm, the film thickness of M layer 202 and K layer 204 is 1-3μm, and the film thickness of N layer 203 and Au layer 205 is 0.75-3μm.

[0054] like Figure 3 As shown in the flow chart, the manufacturing process of the integrated packaging shell in the present invention mainly includes three steps: first, a thick film ceramic substrate is manufactured, and then a metal film wiring layer is manufactured on the thick film ceramic substrate to obtain a thick film hybrid multilayer ceramic substrate, and then the thick film hybrid multilayer ceramic substrate and the metal surrounding frame are brazed to obtain a thick film hybrid multilayer integrated packaging shell.

[0055] The manufacturing process of the integrated packaging shell in the present invention is described in detail below in conjunction with specific embodiments.

[0056] Example 1

[0057] S1. In this embodiment, alumina green porcelain is prepared by pressing and casting, and then the alumina green porcelain is sintered or patterned to prepare a thick film ceramic substrate with built-in passive components, and the surface of the thick film ceramic substrate is ground and polished;

[0058] S2. After cleaning the thick film ceramic substrate in S1, a metal thin film wiring layer is prepared on the surface of the thick film ceramic substrate by a magnetron sputtering method, and Ti / Pt / Au / Ti / Pt / Au thin film wiring layers are sputtered from the inside to the outside, wherein the Ti layer in the Ti / Pt / Au / Ti / Pt / Au thin film wiring layer has a thickness of 0.3 μm, the Pt layer has a thickness of 1 μm, and the Au layer has a thickness of 0.75 μm, and then the required metallization pattern is prepared on the metal thin film wiring layer by photolithography;

[0059] S3, plating nickel and gold on the surface of the metal frame, wherein the material of the metal frame is 4J42 constant expansion alloy, the thickness of the nickel plating layer is 1.27 μm, and the thickness of the gold plating layer is 0.75 μm;

[0060] S4, placing preformed gold-tin solder sheets and metal frames in sequence around the metal film wiring layer to form an integrated package shell pre-assembly;

[0061] S5. Send the integrated packaging shell preassembly into the brazing furnace and braze it into a whole under the protection of pure nitrogen atmosphere. The temperature setting curve of the whole brazing process is as follows: the first step is to heat up from room temperature to 250℃ at a heating rate of 20℃ / min, and then keep warm for 5 minutes to ensure that the assembled ceramic and metal frame are heated evenly; the second step is to preheat at 250℃, further heat up to 300℃ at a heating rate of 20℃ / min, and keep warm at this temperature for 2 minutes; the third step is to cool down at a cooling rate of 10℃ / min, and the ceramic integrated packaging shell is obtained when it is taken out of the furnace.

[0062] The ceramic integrated package shell in this embodiment is tested for air tightness according to the test requirements of GJB2440A-2006 <General Specification for Hybrid Integrated Circuit Shell> after passing the environmental test of -65℃~+175℃ temperature cycle 100 times and -65℃~+150℃ heat shock 15 times. The results are shown in Table 1.

[0063] Table 1 The air tightness test results of the ceramic integrated packaging shell in Example 1

[0064]

[0065] It can be seen from the test results in Table 1 that the airtightness of the ceramic integrated package shell in Example 1 is better than 1.0×10 - 9 Pa.m 3 .s -1 Meet the requirements.

[0066] Example 2

[0067] S1. In this embodiment, aluminum nitride green ceramic is prepared by pressing and casting, and then the aluminum nitride green ceramic is sintered or patterned to prepare a thick film ceramic substrate with built-in passive components, and the surface of the thick film ceramic substrate is ground and polished;

[0068] S2. After cleaning the thick film ceramic substrate in S1, a metal thin film wiring layer is manufactured on the surface of the thick film ceramic substrate by a magnetron sputtering method, and Ti / Ni / Au / Ti / Ni / Au thin film wiring layers are sputtered in sequence from the inside to the outside, wherein the Ti layer in the Ti / Ni / Au / Ti / Ni / Au thin film wiring layer has a thickness of 0.3 μm, the Ni layer has a thickness of 2 μm, and the Au layer has a thickness of 2 μm, and then the required metallization pattern is prepared on the metal thin film wiring layer by photolithography;

[0069] S3, plating nickel and gold on the surface of the metal frame, wherein the material of the metal frame is 4J29 fixed expansion alloy, the thickness of the nickel plating layer is 2 μm, and the thickness of the gold plating layer is 2 μm;

[0070] S4, placing preformed gold-tin solder sheets and metal frames in sequence around the metal film wiring layer to form an integrated package shell pre-assembly;

[0071] S5. Send the integrated packaging shell preassembly into the brazing furnace and braze it into a whole under the protection of pure nitrogen atmosphere. The temperature setting curve of the whole brazing process is as follows: the first step is to heat up from room temperature to 260℃ at a heating rate of 25℃ / min, and then keep it warm for 8 minutes to ensure that the assembled ceramic and metal frame are heated evenly; the second step is to preheat at 260℃, further heat up to 315℃ at a heating rate of 25℃ / min, and keep it warm at this temperature for 5 minutes; the third step is to cool down at a cooling rate of 15℃ / min, and the ceramic integrated packaging shell is obtained when it is taken out of the furnace.

[0072] The ceramic integrated package shell in this embodiment is tested for air tightness according to the test requirements of GJB2440A-2006 <General Specification for Hybrid Integrated Circuit Shell> after passing the environmental test of -65℃~+175℃ temperature cycle 100 times and -65℃~+150℃ heat shock 15 times. The results are shown in Table 2.

[0073] Table 2 Test results of air tightness of ceramic integrated package in Example 2

[0074]

[0075] It can be seen from the test results in Table 2 that the airtightness of the ceramic integrated package shell in Example 2 is better than 1.0×10 - 9 Pa.m 3 .s -1 Meet the requirements.

[0076] Example 3

[0077] S1. In this embodiment, LTCC green ceramics are prepared by pressing and casting, and then the LTCC green ceramics are sintered or patterned to prepare a thick film ceramic substrate with built-in passive components, and the surface of the thick film ceramic substrate is ground and polished;

[0078] S2. After cleaning the thick film ceramic substrate in S1, a metal thin film wiring layer is manufactured on the surface of the thick film ceramic substrate by a magnetron sputtering method, and Ti / Pt / Au / Ti / Pt / Au thin film wiring layers are sputtered from the inside to the outside, wherein the Ti layer in the Ti / Pt / Au / Ti / Pt / Au thin film wiring layer has a thickness of 0.6 μm, the Pt layer has a thickness of 3 μm, and the Au layer has a thickness of 3 μm, and then the required metallization pattern is prepared on the metal thin film wiring layer by photolithography;

[0079] S3, plating nickel and gold on the surface of the metal frame, wherein the material of the metal frame is 4J29 fixed expansion alloy, the thickness of the nickel plating layer is 2 μm, and the thickness of the gold plating layer is 2 μm;

[0080] S4, placing preformed gold-tin solder sheets and metal frames in sequence around the metal film wiring layer to form an integrated package shell pre-assembly;

[0081] S5. Send the integrated packaging shell preassembly into the brazing furnace and braze it into a whole under the protection of pure nitrogen atmosphere. The temperature setting curve of the whole brazing process is as follows: the first step is to heat up from room temperature to 270℃ at a heating rate of 30℃ / min, and then keep it warm for 10 minutes to ensure that the assembled ceramic and metal frame are heated evenly; the second step is to preheat at 270℃, and then further heat up to 330℃ at a heating rate of 25℃ / min, and keep it warm at this temperature for 10 minutes; the third step is to cool down at a cooling rate of 20℃ / min, and a thick-thin film hybrid multilayer ceramic integrated packaging shell is obtained when it is taken out of the furnace.

[0082] The ceramic integrated package shell in this embodiment was tested for air tightness according to the test requirements of GJB2440A-2006 <General Specification for Hybrid Integrated Circuit Shell>, after passing the environmental test of -65℃~+175℃ temperature cycle 100 times and -65℃~+150℃ heat shock 15 times. The results are shown in Table 3.

[0083] Table 3 Air tightness test results of ceramic integrated packaging shell in Example 3

[0084]

[0085] It can be seen from the test results in Table 3 that the airtightness of the ceramic integrated package shell in Example 3 is better than 1.0×10 - 9 Pa.m 3 .s -1 Meet the requirements.

[0086] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0087] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A ceramic integrated packaging shell, comprising a thick-film multilayer ceramic substrate and a metal frame, wherein the thick-film multilayer ceramic substrate is composed of a thick-film ceramic substrate and a metal film wiring layer arranged on the surface of the thick-film ceramic substrate, the metal frame is arranged on the thick-film multilayer ceramic substrate, and a gold-tin solder layer is arranged between the metal frame and the thick-film multilayer ceramic substrate, characterized in that: The metal film wiring layer is a six-layer thin film system of Ti / M / N / Ti / K / Au from the inside to the outside, wherein the M layer and the K layer are independently selected from Pt or Ni, the N layer is a stress release layer, and the stress release layer is Au or Cu; the film thickness of the Ti layer is 0.1-0.6μm, the film thickness of the M layer and the K layer is 1-3μm, and the film thickness of the N layer is 0.75-3μm.

2. The ceramic integrated package as claimed in claim 1, characterized in that: The material of the metal frame is selected from one of 4J42, 4J33, and 4J29 fixed expansion alloys, and the surface of the metal frame is provided with a nickel layer and a gold layer in sequence from the inside to the outside.

3. The ceramic integrated package as claimed in claim 2, characterized in that: On the surface of the metal frame, the thickness of the nickel layer is 1.27-8.9 μm, and the thickness of the gold layer is 0.75-5.7 μm.

4. The ceramic integrated package as claimed in claim 1, characterized in that: The thick film ceramic substrate is selected from one of an alumina ceramic substrate, an aluminum nitride ceramic substrate and a LTCC substrate.

5. The ceramic integrated package as claimed in claim 1, characterized in that: The stress release layer is Au.

6. A process for manufacturing a ceramic integrated packaging shell according to any one of claims 1 to 5, characterized in that: The following steps are involved: Green porcelain is obtained by pressing and casting, the green porcelain is sintered or patterned to prepare a thick film ceramic substrate with built-in passive components, and the surface of the thick film ceramic substrate is ground and polished; A metal thin film wiring layer is produced by sputtering from the inside to the outside on the surface of the processed thick film ceramic substrate by magnetron sputtering, and a required metallization pattern is prepared on the metal thin film wiring layer to obtain a thick-film hybrid multilayer ceramic substrate; A nickel layer and a gold layer are plated on the surface of the metal frame from the inside to the outside in sequence; Placing a gold-tin solder sheet and a metal frame in sequence on the metal film wiring layer of the thick-film hybrid multilayer ceramic substrate to form an integrated package shell pre-assembly; The integrated packaging shell pre-assembly is sent into a brazing furnace and brazed into a whole under a protective atmosphere.

7. The manufacturing process according to claim 6, characterized in that: The brazing process includes a preheating process, a heat preservation process and a cooling process in sequence.

8. The manufacturing process according to claim 7, characterized in that: The specific process of brazing is: first, heating from room temperature to 250-270°C at a heating rate of 20-30°C / min, and keeping warm for 5-10min; then heating to 300-330°C at a heating rate of 20-30°C / min, and keeping warm for 2-10min; finally, cooling at a cooling rate of 10-20°C / min, and the ceramic integrated packaging shell is obtained when it is taken out of the furnace.

Citation Information

Patent Citations

  • Hermetically sealed package having stress reducing layer

    CN106414309A

  • Integrated ceramic packaging shell

    CN211788969U

  • Joint form made up of ceramic and metal

    JP1993139857A

  • Metallic thin-film laminated ceramic board

    JP1994177494A

  • Semiconductor element mounting substrate or heat sink and its manufacture and jointed body of the substrate or the heat sink with semiconductor element

    JP2000138320A