A light gas tank and its preparation method

By using plastic bottle preforms and glass fiber wire tempered layer in the gas tank, combining epoxy resin protective layer and specific cover materials, the problems of large weight and single material of the existing gas tank are solved, and lightweight portability and versatility are achieved. Improves safety performance and application prospects.

CN111473242BActive Publication Date: 2024-11-08KUNSHAN POLYMRUIMER NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010473366.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-05-29
Publication Date
2024-11-08
Estimated Expiration
2040-05-29

AI Technical Summary

Technical Problem

The existing gas tanks are made of steel and have a large weight, which limits their portability and versatility. The material is single, so the range of use is limited.

Method used

A plastic bottle is used to form a tempered layer by wrapping glass fiber wires, and an epoxy resin protective layer is coated on the outside. Combined with a specific outer cover material, the pressure, aging and high temperature resistance of the gas tank is improved while reducing weight.

Benefits of technology

It realizes the lightness and portability of the gas tank, improves safety performance and versatility, enhances impact, fire and wear resistance, and expands application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111473242B_ABST
    Figure CN111473242B_ABST
Patent Text Reader

Abstract

The present invention discloses a light gas tank and a preparation method thereof, wherein the gas tank comprises a main body, the main body comprises a bottle embryo, a tempered layer and a protective layer, the bottle embryo is provided with a bottle mouth, and a connecting piece for connecting with a gas valve is provided in the bottle mouth; the tempered layer is composed of glass fiber filaments wound on the outer wall of the bottle embryo; the protective layer is composed of epoxy resin filled in the gap of the tempered layer. The diameter of the glass fiber filaments is 10-22μm, and the thickness of the tempered layer is 0.5cm-5cm; the molding thickness of the bottle embryo is 5mm-5cm; the thickness of the protective layer is 1-5mm. The present invention uses plastic as the bottle embryo and uses glass fiber filaments to wind to form a tempered layer. While ensuring the pressure in the bottle, the weight of the gas tank is reduced, making it portable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gas cylinders, in particular to a light gas cylinder and a preparation method thereof. Background Art

[0002] A gas tank (liquefied gas cylinder) is a container for storing gas. Due to the high pressure of gas, high requirements are placed on the material of the container. Gas tanks in the prior art generally use steel as raw material, which is stamped into shape and then the bottle mouth is processed accordingly to form a cylinder. Due to the material, the cylinder is heavy and inconvenient to carry. It can generally only be fixed in the kitchen and has a relatively single purpose. Summary of the invention

[0003] The purpose of the present invention is to provide a lightweight gas tank and a preparation method thereof, which uses plastic as a bottle embryo and forms a tempered layer by winding glass fiber filaments, thereby reducing the weight of the gas tank while ensuring the pressure inside the bottle, making it portable and having high safety performance.

[0004] To achieve the above object, the present invention provides the following technical solutions:

[0005] A light gas tank comprises a main body, wherein the main body comprises a bottle embryo, a tempered layer and a protective layer, the bottle embryo is provided with a bottle mouth, and a connecting piece for connecting with a gas valve is arranged in the bottle mouth; the tempered layer is composed of glass fiber filaments wound on the outer wall of the bottle embryo; the protective layer is composed of epoxy resin filled in the gap of the tempered layer.

[0006] Furthermore, the diameter of the glass fiber yarn is 10-22 μm, the thickness of the tempered layer is 0.5 cm to 5 cm; the molding thickness of the bottle embryo is 5 mm to 5 cm; and the thickness of the protective layer is 1-5 mm.

[0007] Furthermore, the diameter of the glass fiber filament is 10-22 μm; if the diameter of the glass fiber filament is less than 10 μm, the glass fiber filament is easily broken during the process of winding the glass fiber filament on the outer wall of the bottle embryo to form a tempered layer, affecting the efficiency of the glass fiber filament winding; if the diameter of the glass fiber filament is greater than 22 μm, there will be large gaps on the outer surface of the tempered layer, which will cause hidden dangers to the safety of the gas tank. Therefore, the diameter of the glass fiber filament of the present invention is controlled to be 10-22 μm.

[0008] Furthermore, the connecting piece is in the shape of a flat strip, extending from both sides of the bottle mouth, and connecting interfaces are arranged on both sides of the connecting piece; and scales and scale values ​​corresponding to the scales are arranged on the bottle embryo.

[0009] Furthermore, the light gas tank also includes an outer cover, the main body is arranged in the outer cover, and the outer cover is provided with a plurality of scale holes.

[0010] Preferably, a boss is provided at the bottom of the outer cover, a positioning groove matching the boss is provided at the bottom of the main body, and a support rod for fixing the main body is also provided in the outer cover.

[0011] Furthermore, the outer cover is composed of the following raw materials in parts by weight: 60-80 parts of polycarbonate, 10-20 parts of ABS resin, 10-15 parts of bisphenol A-bis(diphenyl phosphate), 10-15 parts of diatomaceous earth, 4-6 parts of phenyltriethoxysilane, 5-10 parts of isocyanatepropyltriethoxysilane, 3-5 parts of aluminum silicate fiber, 5-8 parts of nano titanium dioxide, 5-8 parts of nano silicon carbide, 5-8 parts of aluminum tripolyphosphate, 3-5 parts of isopropyl alcohol, and 2-5 parts of antioxidant.

[0012] Furthermore, the weight ratio of acrylonitrile:1,3-butadiene:styrene in the ABS resin is 1:1:2;

[0013] Polycarbonate is an almost colorless glassy amorphous polymer with good optical properties. It is resistant to weak acids, weak bases, and neutral oils, but not to ultraviolet light or strong bases. The main performance defects of polycarbonate are that it is not stable enough in hydrolysis resistance, is sensitive to notches, has poor resistance to organic chemicals and scratches, and will turn yellow when exposed to ultraviolet light for a long time. Like other resins, polycarbonate is easily corroded by certain organic solvents. However, polycarbonate has high toughness, and the resin can be processed into large rigid products. Polycarbonate is flame retardant, wear-resistant, and anti-oxidant. The invention adds ABS resin to the raw materials for preparing the outer cover. The invention uses polycarbonate and ABS as main raw materials to prepare the outer cover, and utilizes the complementary performance of the two resins. Among them, 1,3-butadiene provides low-temperature ductility and impact resistance for the ABS resin, but too much butadiene will reduce the hardness, gloss and fluidity of the resin, acrylonitrile provides hardness, heat resistance, acid, alkali, salt and other chemical corrosion resistance for the ABS resin, and styrene provides hardness, processing fluidity and product surface finish for the ABS resin. The outer cover prepared by setting the weight ratio of acrylonitrile:1,3-butadiene:styrene in the ABS resin to 1:1:2 has good impact resistance, wear resistance, heat resistance and chemical corrosion resistance.

[0014] In addition, diatomaceous earth and nano silicon carbide are added to the outer cover of the present invention, which greatly improves the wear resistance of polycarbonate. The density of the diatomaceous earth of the present invention is 2.0-2.2 g / cm 3 , Bulk density 0.45-0.55g / cm 3 , specific surface area 45-60㎡ / g, pore volume 0.45-0.98m 3 / g; The diatomaceous earth of the present invention has a large porosity, can provide excellent surface properties for the raw material components, increase volume, thicken and improve adhesion, and solve the problem of poor wear resistance of polycarbonate.

[0015] The aluminum silicate fiber has a diameter of ≤20 μm and an aspect ratio of 10:1. The aluminum silicate fiber of the present invention has good heat resistance, corrosion resistance, and mechanical strength. As the skeleton of the outer cover, the raw material components of the outer cover are tightly combined together, which plays a good role in the structural stability of the outer cover. The aluminum silicate fiber of the present invention has good high temperature resistance, thermal stability, good resistance to mechanical vibration, and small thermal expansion. It is used together with two halogen-free flame retardants, aluminum tripolyphosphate and bisphenol A-bis (diphenyl phosphate), which greatly enhances the fire resistance and heat insulation properties of the raw materials. The simultaneous use of the three flame retardants is particularly suitable for the flame retardancy of the PC / ABS system.

[0016] The present invention adopts isocyanate propyl triethoxysilane and phenyl triethoxysilane as coupling agents. The isocyanate propyl triethoxysilane molecule contains two different active groups, i.e., isocyanate and ethoxy, and the phenyl triethoxysilane contains ethoxy, which can be used to couple organic molecules and inorganic fillers, enhance their adhesion, and improve the mechanical, electrical, water-resistant, anti-aging and other properties of the product. If the amount of the coupling agent is too large, the adhesion of the raw material components will deteriorate, and if the amount of the coupling agent is too small, the raw materials will not be dispersed well. The present invention controls 4-6 parts of phenyl triethoxysilane and 5-10 parts of isocyanate propyl triethoxysilane, so that the prepared outer cover has the best performance.

[0017] The antioxidant used in the present invention is a conventional oxidant and is not particularly limited herein.

[0018] The particle size of the titanium dioxide of the present invention is 100-200nm;

[0019] The particle size of the nano silicon carbide of the present invention is 100-150nm; by adding nano silicon carbide and nano titanium dioxide, the surface properties of the raw material particles can be nano modified, so that the raw material particles are evenly dispersed, the fluidity of the raw material is increased, and the surface tension of the raw material surface is reduced; the fire resistance and wear resistance of the gas tank cover are improved.

[0020] Furthermore, the thickness of the outer cover is 1-5 cm.

[0021] Furthermore, the outer cover is prepared by blow molding, which is not particularly limited herein.

[0022] Another object of the present invention is to provide a method for preparing the above-mentioned gas cylinder, comprising the following steps:

[0023] S10, preparing a bottle-shaped mold;

[0024] S20, placing a connector for installing the air valve in the mold;

[0025] S30, squeezing plastic particles into the bottle-shaped mold, and blow-molding the bottle embryo through a blow molding process, at which time, the connector is fixedly connected to the bottle embryo as a whole;

[0026] S40, winding glass fiber filaments around the outer wall of the bottle blank to form a tempered layer;

[0027] S50, coating the bottle preform processed in S40 with epoxy resin to fill the gaps in the tempered layer and form a protective layer on the bottle preform;

[0028] S60, setting scales and scale values ​​corresponding to the scales on the bottle embryo processed in S50.

[0029] Furthermore, the plastic particles are PE resin, the molding thickness of the bottle embryo is 5mm to 5cm; and the thickness of the tempered layer is 0.5cm to 5cm.

[0030] Furthermore, in step S30, the temperature of the bottle-shaped mold is 50°C to 90°C, the inflation pressure in the bottle-shaped mold is 0.7MPa to 0.9MPa, and the extrusion temperature of the plastic particles is 180°C to 220°C.

[0031] Furthermore, in step S40, the glass fiber filament has a diameter of 10-22 μm.

[0032] Furthermore, in step S50, the epoxy resin completely covers the tempered layer to form a smooth protective layer on the tempered layer.

[0033] The light gas tank of the present invention uses plastic material as the bottle embryo to reduce the weight of the gas tank and make it portable; uses glass fiber filaments to form a tempered layer to ensure that the pressure in the bottle is sufficient for storing gas; uses epoxy resin to form a protective layer on the bottle embryo, which can fill the gap between adjacent glass fiber filaments, strengthen its pressure resistance, and make it resistant to aging and high temperature. At the same time, by setting an outer cover on the outside of the gas tank, and making the outer cover of plastic with specific components, the prepared gas tank is not only light in weight, but also has good impact resistance, fire resistance, and wear resistance, and high safety performance, which greatly improves the application prospects of the gas tank. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 is a flow chart of a method for preparing a light gas cylinder in one embodiment;

[0035] Figure 2 It is a structural schematic diagram of a light gas tank body in one embodiment;

[0036] Figure 3 is a cross-sectional view of a light gas tank body in one embodiment;

[0037] Figure 4 The figure is a schematic diagram of the main body and outer cover structure of a light gas tank in one embodiment.

[0038] Figure 5 It is a schematic diagram of another main body and outer cover structure of a light gas tank in one embodiment. DETAILED DESCRIPTION

[0039] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] Example 1

[0041] like Figure 2 and 3 As shown, a light gas tank includes a main body 100, wherein the main body 100 includes a bottle preform 110, a tempered layer 120, and a protective layer 130; the bottle preform 110 is provided with a bottle mouth 111, the tempered layer 120 is composed of glass fiber filaments wound on the outer wall of the bottle preform 110; the protective layer 130 is composed of epoxy resin filled in the gaps in the tempered layer 120. A connecting piece 112 for connecting with a gas valve is provided in the bottle mouth 111. In this embodiment, the connecting piece 112 is in the shape of a flat strip, extending from both sides of the bottle mouth 111, and a connecting interface 113 is provided on both sides thereof. Preferably, the interface is a nut, so that the gas valve can be directly connected to the gas tank through the connecting piece 112, so that the gas tank is easy to replace.

[0042] The diameter of the glass fiber yarn is 10-22 μm, the thickness of the tempered layer 120 is 0.5 cm to 5 cm; the molding thickness of the bottle embryo 110 is 5 mm to 5 cm; and the thickness of the protective layer 130 is 1-5 mm.

[0043] Specifically, the preform 110 is blow-molded by plastic particles. In this embodiment, the plastic particles are PE resin. The molding thickness of the preform 110 can be set according to actual needs. In this embodiment, the molding thickness of the preform 110 is 5 mm to 5 cm.

[0044] The tempered layer 120 completely covers the outer wall of the preform 110, and the glass fiber is tightly wound on the preform 110, and the thickness of the formed tempered layer is 0.5 cm to 5 cm. In order to ensure the pressure inside the bottle.

[0045] The protective layer 130 completely covers the tempered layer 120 and forms a smooth protective layer on the tempered layer 120. Since epoxy resin as an anti-corrosion material not only has the characteristics of being dense, water-resistant, leak-resistant, and high-strength, but also has good process properties such as strong adhesion, normal temperature operation, and simple construction, the protective layer 20 formed by coating with epoxy resin can effectively enhance the aging resistance and high temperature resistance of the gas tank.

[0046] In the present invention, the outer cover 200 and the main body 100 can be matched in various structures, such as Figure 4 It is a schematic diagram of another main body and outer cover structure of a light gas tank in one embodiment.

[0047] In one embodiment, continue to refer to Figure 5 The gas tank further comprises an outer cover 200, the main body 100 is arranged in the outer cover 200, a boss 210 is arranged at the bottom of the outer cover 200, a positioning groove 140 matching the boss 210 is arranged at the bottom of the main body 100, and a support rod 220 for fixing the main body 100 is also arranged in the outer cover 200. Specifically, one end of the support rod 220 is hinged at the top corner of the outer cover 200, and the other end is provided with a buffer anti-skid pad 221. After the main body 100 is placed, the support rod 220 is propped up so that the buffer anti-skid pad 221 presses the two sides of the bottle mouth of the main body 100, thereby realizing the fixing of the main body 100 in the outer cover 200.

[0048] Preferably, in order to facilitate observation of the remaining amount of gas, the bottle preform 110 is provided with scales and scale values ​​corresponding to the scales (not shown in the figure), and the outer cover 200 is provided with a plurality of scale holes corresponding to the scales and scale values ​​(not shown in the figure). In order to facilitate transportation, a carrying component or a shoulder strap may be provided on the outer wall or the top of the outer cover 200. In this embodiment, a carrying component 230 is provided on the top of the outer cover 200.

[0049] The light gas tank of the present invention uses plastic material as the bottle embryo 110, which reduces the weight of the gas tank and makes it portable; uses glass fiber filaments to form a tempered layer 120 to ensure that the pressure in the bottle is sufficient for storing gas; uses epoxy resin to form a protective layer 130 on the bottle embryo 110, which can fill the gaps between adjacent glass fiber filaments, enhance its pressure resistance, and at the same time make it resistant to aging and high temperature.

[0050] The outer cover 200 has a thickness of 3 cm and is composed of the following raw materials in parts by weight: 70 parts of polycarbonate, 15 parts of ABS resin, 12 parts of bisphenol A-bis(diphenyl phosphate), 12 parts of diatomaceous earth, 5 parts of phenyltriethoxysilane, 8 parts of isocyanatepropyltriethoxysilane, 4 parts of aluminum silicate fiber, 6 parts of nano titanium dioxide, 6 parts of nano silicon carbide, 6 parts of aluminum tripolyphosphate, 4 parts of isopropyl alcohol, and 3 parts of antioxidant.

[0051] like Figure 1 As shown, Figure 1 The flowchart of a method for preparing a light gas cylinder in one embodiment is shown. The method for preparing a light gas cylinder includes the following steps:

[0052] S10, preparing a bottle-shaped mold. Specifically, the bottle-shaped mold is provided with a bottle mouth and is mainly composed of two assembled axisymmetric components, so that the preform can be easily taken out after being formed;

[0053] S20, placing a connector for installing the gas valve in the mold, specifically, the connector is placed at the bottle mouth. In this embodiment, the connector is in the form of a flat strip, extending from both sides of the bottle mouth, and is provided with connection interfaces on both sides. Preferably, the interface is a nut, so that the gas valve can be directly connected to the gas tank through the connector, making it easy to replace the gas tank.

[0054] S30, squeeze the plastic particles into the bottling mold, and blow mold the preform through the blow molding process. At this time, the connector is fixedly connected to the preform. Specifically, the temperature of the bottle mold is 50℃~90℃, the blowing pressure in the bottle mold is 0.7MPa~0.9MPa, the extrusion temperature of the plastic particles is 180℃~220℃, and when the intermittent blow molding process is adopted, it can be divided into four stages of blow molding, each blowing time is 15s, the cooling time is 20s, and the four stages of blowing temperatures are: 155℃, 165℃, 165℃ and 170℃ respectively.

[0055] The plastic particles may be made of transparent material. In this embodiment, the plastic particles are PE resin. The molding thickness of the preform may be set according to actual needs. In this embodiment, the molding thickness of the preform is 5 mm to 5 cm.

[0056] S40, winding glass fiber filaments on the outer wall of the bottle preform to form a tempered layer, wherein the glass fiber filaments completely cover the outer wall of the bottle preform. In this embodiment, the thickness of the formed tempered layer is 0.5 cm to 5 cm.

[0057] S50, coating the bottle embryo processed by S40 with epoxy resin, filling the gaps in the tempered layer, and forming a protective layer on the bottle embryo. Specifically, the epoxy resin completely covers the tempered layer and forms a smooth protective layer on the tempered layer. The thickness of the protective layer is 1-5 mm. Since epoxy resin as an anti-corrosion material not only has the characteristics of being dense, water-resistant, good in leakage resistance, and high strength, but also has good process properties such as strong adhesion, normal temperature operation, and simple construction, the use of epoxy resin coating to form a protective layer can effectively enhance the aging resistance and high temperature resistance of the gas tank.

[0058] In one embodiment, the method for preparing a light gas tank further includes step S60, setting scales and scale values ​​corresponding to the scales on the bottle embryo for observing the remaining amount of gas.

[0059] Comparative Example 1

[0060] The difference between Comparative Example 1 and Example 1 is that the outer cover components use ordinary titanium dioxide and silicon carbide instead of nano titanium dioxide and nano silicon carbide;

[0061] Comparative Example 2

[0062] The difference between Comparative Example 2 and Example 1 is that the outer cover component uses ordinary silicon carbide instead of nano silicon carbide;

[0063] Comparative Example 3

[0064] The only difference between Comparative Example 3 and Example 1 is that the aspect ratio of the aluminum silicate fiber of the outer cover component is 9:1;

[0065] Comparative Example 4

[0066] The only difference between Comparative Example 4 and Example 1 is that the outer cover component uses aluminum silicate fiber with an aspect ratio of 11:1;

[0067] Comparative Example 5

[0068] The difference between Comparative Example 5 and Example 1 is that the outer cover component uses 7 parts of phenyltriethoxysilane and 11 parts of isocyanatepropyltriethoxysilane in equal amounts;

[0069] Comparative Example 6

[0070] The difference between Comparative Example 6 and Example 1 is that the outer cover component uses 3 parts of phenyltriethoxysilane and 4 parts of isocyanatepropyltriethoxysilane in equal amounts;

[0071] The following performance tests were performed on Example 1 and Comparative Examples 1-6 using ASTM (American Society for Testing and Materials) standards:

[0072] 1. Tensile strength and elongation at break: The tensile strength and elongation at break of the material are determined using the ASTM D638 method.

[0073] 2. Flexural strength and flexural modulus: The flexural strength and flexural modulus of the material are determined using the ASTM D790 method.

[0074] 3. Notched impact strength: The notched impact strength of the material is measured using the ASTM D256 method.

[0075] 4. Heat deformation temperature: The heat deformation temperature of the material is determined using the ASTM D648 method.

[0076] 5. Melt flow rate: The melt flow rate of the material is determined by ASTM D1238 method.

[0077] Various performance tests such as impact strength, tensile strength, high temperature resistance, and wear resistance were conducted on the outer cover products made from Example 1 of the present invention and Comparative Examples 1-6;

[0078]

[0079]

[0080] From the comparison in the above table, it can be seen that the outer cover product of the present invention has good performances such as impact strength, tensile strength, high temperature resistance, wear resistance, acid and alkali resistance, etc.

[0081] The light gas tank of the present invention uses plastic material as the bottle embryo to reduce the weight of the gas tank and make it portable; uses glass fiber filaments to form a tempered layer to ensure that the pressure in the bottle is sufficient for storing gas; uses epoxy resin to form a protective layer on the bottle embryo, which can fill the gap between adjacent glass fiber filaments, strengthen its pressure resistance, and make it resistant to aging and high temperature. At the same time, by setting an outer cover on the outside of the gas tank, and making the outer cover of plastic with specific components, the prepared gas tank is not only light in weight, but also has good impact resistance, fire resistance, and wear resistance, and high safety performance, which greatly improves the application prospects of the gas tank.

[0082] The above embodiments only express several preferred implementations of the present invention, and the description thereof is relatively specific and detailed. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the invention concept described herein through the above teachings or the technology or knowledge in the relevant field, and it cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several deformations and improvements can be made without departing from the concept of the present invention. The changes and modifications made by the personnel in this field do not depart from the spirit and scope of the present invention, and all of these belong to the protection scope of the claims attached to the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.

Claims

1. A light gas tank, characterized in that: The invention comprises a main body, wherein the main body comprises a bottle embryo, a tempered layer and a protective layer, wherein the bottle embryo is provided with a bottle mouth, wherein a connecting piece for connecting with a gas valve is provided in the bottle mouth; the tempered layer is composed of glass fiber filaments wound on the outer wall of the bottle embryo; and the protective layer is composed of epoxy resin filled in the gap of the tempered layer; The light gas tank further comprises an outer cover, the main body is arranged in the outer cover, and the outer cover is provided with a plurality of scale holes; The outer cover is composed of the following raw materials in parts by weight: 60-80 parts of polycarbonate, 10-20 parts of ABS resin, 10-15 parts of bisphenol A-bis(diphenyl phosphate), 10-15 parts of diatomaceous earth, 4-6 parts of phenyltriethoxysilane, 5-10 parts of isocyanatepropyltriethoxysilane, 3-5 parts of aluminum silicate fiber, 5-8 parts of nano titanium dioxide, 5-8 parts of nano silicon carbide, 5-8 parts of aluminum tripolyphosphate, 3-5 parts of isopropyl alcohol, and 2-5 parts of antioxidant; The weight ratio of acrylonitrile:1,3-butadiene:styrene in the ABS resin is 1:1:2; The diatomaceous earth has a density of 2.0-2.2 g / cm3, a bulk density of 0.45-0.55 g / cm3, a specific surface area of ​​45-60 m2 / g, and a pore volume of 0.45-0.98 m3 / g; The aluminum silicate fiber has a diameter of ≤20 μm and an aspect ratio of 10:1; The particle size of the nano titanium dioxide is 100-200nm; The particle size of the nano silicon carbide is 100-150nm; The thickness of the outer cover is 1-5 cm; The diameter of the glass fiber yarn is 10-22 μm, the thickness of the tempered layer is 0.5 cm to 5 cm; the molding thickness of the bottle embryo is 5 mm to 5 cm; the thickness of the protective layer is 1-5 mm; The connecting piece is in the shape of a flat strip, extending from both sides of the bottle mouth, and connecting interfaces are provided on both sides of the connecting piece; The bottle embryo is provided with scales and scale values ​​corresponding to the scales.

2. A method for preparing a light gas cylinder as claimed in claim 1, characterized in that: The following steps are involved: S10, preparing a bottle-shaped mold; S20, placing a connector for installing the air valve in the mold; S30, squeezing plastic particles into the bottle-shaped mold, blow-molding the bottle embryo through a blow molding process, and fixing the connector and the bottle embryo as a whole; S40, winding glass fiber filaments around the outer wall of the bottle blank to form a tempered layer; S50, coating the bottle preform processed in S40 with epoxy resin to fill the gaps in the tempered layer and form a protective layer on the bottle preform; S60, setting scales and scale values ​​corresponding to the scales on the bottle embryo processed in S50.

3. The method for preparing a light gas cylinder according to claim 2, characterized in that: The plastic particles are PE resin, the molding thickness of the bottle embryo is 5mm-5cm; the thickness of the tempered layer is 0.5cm-5cm.

4. The method for preparing a light gas cylinder according to claim 2, characterized in that: In step S30, the temperature of the bottle-shaped mold is 50°C to 90°C, the inflation pressure in the bottle-shaped mold is 0.7MPa to 0.9MPa, and the extrusion temperature of the plastic particles is 180°C to 220°C.

5. The method for preparing a light gas cylinder according to claim 2, characterized in that: In step S40, the diameter of the glass fiber filament is 10-22 μm; in step S50, the epoxy resin completely covers the tempered layer to form a smooth protective layer on the tempered layer.