Production equipment and process for roughening the surface of capacitor electrode aluminum foil

By using arc ion targets to deposit large-particle aluminum and ion bombardment cleaning in the vacuum cavity, the impact of the existing capacitor aluminum foil surface roughening process on the environment and electrical performance is solved, and the efficient and environmentally friendly aluminum foil surface roughening is achieved, reducing the Production cost.

CN111524710BActive Publication Date: 2024-12-03KUNSHAN PUYUAN VACUUM TECH ENG CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202010408357.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-05-14
Publication Date
2024-12-03
Estimated Expiration
2040-05-14

AI Technical Summary

Technical Problem

The surface roughening process of existing capacitor aluminum foil relies on chemical corrosion, affects the environment and electrical performance, and is complex in the process and high in cost.

Method used

The physical vapor deposition process in the vacuum cavity is adopted to deposit large-particle aluminum on the surface of the aluminum foil through a rectangular arc ion target, increasing the surface roughness, and ion bombardment cleaning is used for ionic bombardment to ensure oxidation-free and environmental protection.

Benefits of technology

It realizes efficient coarseness of the aluminum foil surface, increases the surface area, simplifies the process, reduces production costs, and has small equipment investment and no pollution in the environment. It is suitable for double-sided single-use treatment of rolled aluminum foil.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111524710B_ABST
    Figure CN111524710B_ABST
Patent Text Reader

Abstract

The invention discloses a production equipment and process for roughening the surface of capacitor electrode aluminum foil. The production equipment comprises first and second rectangular arc ion targets for aluminum plating on both sides of the aluminum foil respectively wound around first and second cooling main rollers in a vacuum chamber, an argon gas supply device, a discharging device and a collecting device for discharging and collecting the aluminum foil, a cooling system and a control system for cooling a vacuum pump group, the first and second cooling main rollers and the first and second rectangular arc ion targets. The production process steps are as follows: firstly installing the aluminum foil, then starting the vacuum pump group to evacuate the air, and cooling the first and second cooling main rollers to -20°C; filling the vacuum chamber with argon gas, opening each component to start aluminum plating, closing each component after aluminum plating is completed, raising the temperature of the first and second cooling main rollers to 35°C, stopping the vacuum pump group, breaking the vacuum, and removing the aluminum foil roll on the winding roller. The invention has no pollution to the environment, no oxidation on the aluminum foil surface, and high production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an aluminum foil processing technology, in particular to a production device and a process for roughening the surface of capacitor electrode aluminum foil. Background Art

[0002] The existing capacitor aluminum foil is divided into high-voltage anode foil, low-voltage anode foil and cathode foil. The surface area of ​​the anode foil and the cathode foil has a great relationship with the electrostatic capacity of the capacitor. The larger the surface area of ​​the aluminum foil, the better the performance of the capacitor.

[0003] At present, the surface of aluminum foil is basically roughened by chemical corrosion to increase the surface area, and chemical solution (NaOH) is used for corrosion, and then HNO3 is used to remove the aluminum oxide generated on the surface, and then rinsed with clean water. This process affects both the environment and the electrical properties of the aluminum foil, the production process is cumbersome, the equipment investment is high, and the production cost cannot be reduced. Summary of the invention

[0004] In order to overcome the above-mentioned defects, the present invention provides a production equipment and process for roughening the surface of capacitor electrode aluminum foil. The production equipment and process for roughening the surface of capacitor electrode aluminum foil have high efficiency in roughening the surface of the aluminum foil, are environmentally friendly, will not cause oxidation of the aluminum foil surface, have a simple process and low production cost.

[0005] The technical solution adopted by the present invention to solve its technical problems is: a production equipment for roughening the surface of capacitor electrode aluminum foil, including a vacuum chamber, a vacuum pump group, a first-side rectangular arc ion target, a second-side rectangular arc ion target, an argon gas supply device, a discharge device, a collection device, a first-side cooling main roller, a second-side cooling main roller, a cooling system and a control system, wherein the vacuum pump group can evacuate the vacuum chamber, the first-side cooling main roller and the second-side cooling main roller can be installed in the vacuum chamber so as to rotate synchronously, cooling channels are formed in the first-side cooling main roller and the second-side cooling main roller, the discharge device and the collection device are respectively installed in the vacuum chamber, and the aluminum foil drawn from the discharge device is sequentially wound around the surfaces of the first-side cooling main roller and the second-side cooling main roller and then collected by the collection device, and One side surface of the aluminum foil contacts with the first cooling main roller, and the other side surface of the aluminum foil contacts with the second cooling main roller. The first arc ion target faces the aluminum foil on the surface of the first cooling main roller, and the second arc ion target faces the aluminum foil on the surface of the second cooling main roller. The first arc ion target and the second arc ion target can deposit large-particle aluminum on the surface of the aluminum foil respectively. The cooling system can provide cooling liquid to the first cooling main roller, the second cooling main roller, the first arc ion target, the second arc ion target and the vacuum pump group. The argon supply device can provide argon to the vacuum chamber. The control system controls the operation of the vacuum pump group, the first arc ion target, the second arc ion target, the argon supply device, the discharge device, the collection device, the first cooling main roller, the second cooling main roller and the cooling system.

[0006] As a further improvement of the present invention, a first surface ion source and a second surface ion source are provided, the first surface ion source is directly opposite to the aluminum foil on the surface of the first surface cooling main roller, and the first surface ion source and the first surface arc ion target are arranged sequentially along the conveying direction of the aluminum foil, the second surface ion source is directly opposite to the aluminum foil on the surface of the second surface cooling main roller, and the second surface ion source and the second surface arc ion target are arranged sequentially along the conveying direction of the aluminum foil, the first surface ion source and the second surface ion source can respectively perform ion bombardment cleaning on the surface of the aluminum foil, and the cooling system can provide cooling liquid to the first surface ion source and the second surface ion source.

[0007] As a further improvement of the present invention, a water-cooling partition is further provided, wherein the water-cooling partition is fixedly installed in the vacuum chamber, and the inner side walls opposite to the water-cooling partition and the vacuum chamber respectively enclose a first arc ion target installation chamber and a second arc ion target installation chamber, and the first surface arc ion target and the second surface arc ion target are respectively fixedly installed in the first arc ion target installation chamber and the second arc ion target installation chamber, and the outer side surfaces of the parts of the circumference of the first surface cooling main roller and the second surface cooling main roller covered with aluminum foil respectively extend into the first arc ion target installation chamber and the second arc ion target installation chamber through the notch on the water-cooling partition, and the first surface ion source and the second surface ion source are respectively located on the outer sides of the first arc ion target installation chamber and the second arc ion target installation chamber, and two argon gas supply devices respectively provide argon gas to the first arc ion target installation chamber and the second arc ion target installation chamber.

[0008] As a further improvement of the present invention, a cooling channel of a sandwich structure is formed inside the first-side cooling main roller and the second-side cooling main roller, and the cooling channel is connected to the cooling system through a hot and cold exchanger.

[0009] As a further improvement of the present invention, a cooling main roller driving device is further provided, and the cooling main roller driving device drives the first cooling main roller and the second cooling main roller to rotate synchronously respectively.

[0010] As a further improvement of the present invention, the unwinding device includes an unwinding roller and an unwinding drive device, and the receiving device includes a winding roller and a winding drive device. The unwinding drive device and the winding drive device respectively drive the unwinding roller and the winding roller to rotate. An aluminum foil tension sensor is also provided. The aluminum foil tension sensor can sense the aluminum foil tension and transmit a signal to the control system. The control system controls the action of the unwinding drive device and the winding drive device.

[0011] As a further improvement of the present invention, both the unwinding roller and the winding roller are provided with a detachable air expansion shaft.

[0012] As a further improvement of the present invention, a plurality of auxiliary rollers are provided, at least one auxiliary roller is provided on both sides of the first cooling main roller and the second cooling main roller, and the aluminum foil entering and leaving the first cooling main roller and the second cooling main roller is redirected and transported via the auxiliary rollers.

[0013] As a further improvement of the present invention, a base and a sliding door are provided. The vacuum chamber is fixedly mounted on the base. An inlet is provided at one end of the vacuum chamber. The sliding door can be slidably mounted on the base. The sliding door can seal and close or open the inlet of the vacuum chamber.

[0014] As a further improvement of the present invention, the control system includes a PLC and a touch screen, the touch screen can edit and input data into the editing module of the PLC, and the vacuum chamber is also provided with a vacuum gauge, a gas flow meter, a vacuum valve, a temperature sensor and an alarm, the vacuum gauge can sense the vacuum degree in the vacuum chamber and transmit a signal to the PLC, the gas flow meter can detect the flow rate of argon gas sent into the vacuum chamber by the argon gas supply device and transmit a signal to the PLC, the temperature sensor can detect the surface temperature of the first-side cooling main roller and the second-side cooling main roller and transmit a signal to the PLC, the vacuum valve can connect the vacuum chamber with the outside world, and the PLC controls the alarm to sound an alarm.

[0015] A production process for roughening the surface of capacitor electrode aluminum foil, the steps of which are as follows:

[0016] Step 1: Load the rolled aluminum foil onto the unwinding roller, and lead one end of the aluminum foil out of the unwinding roller and pass through the first cooling main roller and the second cooling main roller in sequence, and finally pass through and wrap around the winding roller;

[0017] Step 2: Close the vacuum chamber, start the vacuum pump group, and evacuate the vacuum chamber;

[0018] Step 3: When the vacuum pressure in the vacuum chamber reaches 5*10-1Pa, the hot and cold exchanger starts to cool the first cooling main roller and the second cooling main roller, and the cooling temperature is set to -20℃;

[0019] Step 4: When the vacuum pressure in the vacuum chamber reaches 5*10-3Pa, the argon gas supply device is turned on to fill the vacuum chamber with argon gas, and the vacuum pressure in the vacuum chamber is stabilized at 6*10-1Pa;

[0020] Step 5: Turn on the unwinding drive device, the winding drive device and the cooling main roller drive device, set the aluminum foil linear speed to 2m / min, and the tension to 150N;

[0021] Step 6: Turn on the first surface ion source and the second surface ion source, and set the first surface ion source and the second surface ion source to a current of 0.5A and a voltage of 1500V;

[0022] Step 7: Turn on the first arc ion target and the second arc ion target, and set the current of the first arc ion target and the second arc ion target to 450A;

[0023] Step 8: High-purity large-particle aluminum is deposited on both sides of the aluminum foil at the same time. After the rolled aluminum foil is rolled onto the winding roller, the control system prompts that the work is completed, and the first and second arc ion targets, the first and second ion sources, the argon gas supply device, the unwinding drive device, the winding drive device and the cooling main roller drive device are turned off;

[0024] Step 9: The hot and cold switches start heating up, and the heating temperature is set to 35°C;

[0025] Step 10: Close the vacuum valve of the exhaust pipeline, stop the vacuum pump group, and open the vacuum valve on the vacuum chamber to break the vacuum;

[0026] Step 11: Open the door of the vacuum chamber and remove the aluminum foil roll from the winding roller. The surface roughening treatment of the aluminum foil is completed.

[0027] The beneficial effects of the present invention are as follows: the present invention adopts a physical vapor deposition process to place an aluminum foil in a vacuum chamber and uses an arc ion target to quickly deposit high-purity aluminum on the surface of the aluminum foil. During the deposition process, the parameters of the arc target are adjusted to make the deposited aluminum particles larger, thereby achieving the effect of depositing a layer of rough aluminum film on the surface of the aluminum foil. After the aluminum film is deposited, the roughness of the aluminum foil surface increases, and the surface area also increases accordingly. The entire production process of the present invention is completed in a vacuum chamber, there will be no environmental pollution, and the aluminum foil surface will not be oxidized. The process is simple, the equipment investment is small, and the equipment of the present invention can perform a one-time roughening treatment on both sides of the rolled aluminum foil, the production efficiency is high, and the production cost is greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the structural principle of the present invention. DETAILED DESCRIPTION

[0029] Embodiment: A production equipment for roughening the surface of capacitor electrode aluminum foil, comprising a vacuum chamber 1, a vacuum pump group 2, a first-side rectangular arc ion target 3, a second-side rectangular arc ion target 4, an argon gas supply device 5, a discharge device, a collection device, a first-side cooling main roller 6, a second-side cooling main roller 7, a cooling system and a control system, wherein the vacuum pump group 2 can evacuate the vacuum chamber 1, the first-side cooling main roller 6 and the second-side cooling main roller 7 can be installed in the vacuum chamber 1 so as to rotate synchronously, a cooling channel is formed in the first-side cooling main roller 6 and the second-side cooling main roller 7, the discharge device and the collection device are respectively installed in the vacuum chamber 1, and the aluminum foil 8 drawn from the discharge device is sequentially wound around the surfaces of the first-side cooling main roller 6 and the second-side cooling main roller 7 and then collected by the collection device, and the surface of one side of the aluminum foil 8 is connected to the surface of the first-side cooling main roller 6 and the second-side cooling main roller 7. The first side is in contact with the cooling main roller 6, and the other side surface of the aluminum foil 8 is in contact with the second side cooling main roller 7. The first side arc ion target is opposite to the aluminum foil on the surface of the first side cooling main roller 6, and the second side arc ion target is opposite to the aluminum foil on the surface of the second side cooling main roller 7. The first side arc ion target and the second side arc ion target can deposit large-particle aluminum on the surface of the aluminum foil 8 respectively. The cooling system can provide cooling liquid to the first side cooling main roller 6, the second side cooling main roller 7, the first side arc ion target, the second side arc ion target and the vacuum pump group 2. The argon gas supply device 5 can provide argon gas into the vacuum chamber 1. The control system controls the operation of the vacuum pump group 2, the first side arc ion target, the second side arc ion target, the argon gas supply device 5, the discharge device, the collection device, the first side cooling main roller 6, the second side cooling main roller 7 and the cooling system.

[0030] The production equipment adopts the physical vapor deposition process to place the aluminum foil 8 in the vacuum chamber 1, and uses the first arc ion target and the second arc ion target to quickly deposit high-purity aluminum on the surfaces of both sides of the aluminum foil 8. In the process, the parameters of the arc target are adjusted to make the deposited aluminum particles larger, so as to deposit a rough aluminum film on the surface of the aluminum foil 8. In this way, the surface roughness of the aluminum foil 8 will be larger, and the surface area will also be larger. The vacuum pump group 2 is composed of 6 molecular pumps, 2 Roots pumps, 2 two-stage rotary vane pumps, and a number of vacuum valves and vacuum pipelines. The first and second arc ion targets have two groups respectively, and each group of arc ion targets is equipped with a 500A arc power supply, and the output current is adjustable from 100A to 500A; the arc ion target is a rectangular target with a specification of 600*120mm, equipped with a 600*120*20mm high-purity (99.99%) aluminum target; the aluminum target is directly water-cooled to ensure long-term stable operation.

[0031] A first surface ion source 9 and a second surface ion source 10 are also provided. The first surface ion source 9 is directly opposite to the aluminum foil on the surface of the first surface cooling main roller 6, and the first surface ion source 9 and the first surface arc ion target are arranged in sequence along the aluminum foil conveying direction. The second surface ion source 10 is directly opposite to the aluminum foil on the surface of the second surface cooling main roller 7, and the second surface ion source 10 and the second surface arc ion target are arranged in sequence along the aluminum foil conveying direction. The first surface ion source 9 and the second surface ion source 10 can respectively perform ion bombardment cleaning on the surface of the aluminum foil, and the cooling system can provide cooling liquid to the first surface ion source 9 and the second surface ion source 10. The first surface ion source 9 and the second surface ion source 10 are respectively equipped with 10KW / 2000V ion source power supplies. The ion sources are arranged in front of the arc ion target. High-energy electric ion bombardment cleaning is performed on the surface of the aluminum foil to remove the oxide layer and other organic pollutants on the surface of the aluminum foil and improve the bonding force between the aluminum foil and the deposited aluminum. The cooling system is equipped with a 30KW industrial chiller to perform circulating water cooling on the arc target, ion source, vacuum pump, etc.

[0032] A water-cooled partition 16 is also provided, and the water-cooled partition 16 is fixedly installed in the vacuum chamber 1. The inner side walls of the water-cooled partition 16 and the vacuum chamber 1 respectively enclose the first arc ion target installation chamber 11 and the second arc ion target installation chamber 12. The first surface arc ion target and the second surface arc ion target are fixedly installed in the first arc ion target installation chamber 11 and the second arc ion target installation chamber 12 respectively. The outer surfaces of the first surface cooling main roller 6 and the second surface cooling main roller 7 covered with aluminum foil extend into the first arc ion target installation chamber 11 and the second arc ion target installation chamber 12 through the notch on the water-cooled partition. The first surface ion source 9 and the second surface ion source 10 are respectively located outside the first arc ion target installation chamber 11 and the second arc ion target installation chamber 12. Two argon gas supply devices 5 respectively provide argon gas to the first arc ion target installation chamber 11 and the second arc ion target installation chamber 12. The first and second surface arc ion targets are placed in the first and second arc ion target installation chambers to prevent aluminum particles from reaching other parts.

[0033] The first cooling main roller 6 and the second cooling main roller 7 form a cooling channel of a sandwich structure on the inner side, and the cooling channel is connected to the cooling system through a hot and cold exchanger. The first and second cooling main rollers adopt a double-layer structure to achieve interlayer refrigeration, and are equipped with a 20KW hot and cold exchanger. When the first and second arc targets are working, the interlayer of the first and second cooling main rollers is cooled to -20°C by liquid to protect the aluminum foil from deformation due to high temperature during surface roughening. When the vacuum chamber 1 is broken, the liquid in the interlayer of the first and second cooling main rollers needs to be heated to 35°C to avoid condensation on the surface of the aluminum foil due to too low temperature.

[0034] A cooling main roller driving device is also provided, and the cooling main roller driving device drives the first cooling main roller 6 and the second cooling main roller 7 to rotate synchronously. The cooling main roller driving device includes a variable frequency motor and a synchronous belt. One variable frequency motor drives the first cooling main roller 6 and the second cooling main roller 7 through the synchronous belt to realize synchronous transmission. The transmission shaft of the variable frequency motor uses a magnetic fluid seal.

[0035] The unwinding device includes an unwinding roller 14 and an unwinding drive device, and the rewinding device includes a rewinding roller 15 and a rewinding drive device. The unwinding drive device and the rewinding drive device drive the unwinding roller 14 and the rewinding roller 15 to rotate respectively, and are also provided with an aluminum foil tension sensor, which can sense the aluminum foil tension and transmit a signal to the control system, and the control system controls the unwinding drive device and the rewinding drive device to operate. The unwinding drive device and the rewinding drive device are both servo motors, which provide the winding tension of the aluminum foil, and the motor drive shaft is sealed with a magnetic fluid.

[0036] The unwinding roller 14 and the winding roller 15 are both detachably provided with an air-expanding shaft. The unwinding roller 14 and the winding roller 15 use a detachable air-expanding shaft, which is convenient for hoisting the aluminum foil roll.

[0037] A plurality of auxiliary rollers 13 are also provided. At least one auxiliary roller 13 is provided on both sides of the first cooling main roller 6 and the second cooling main roller 7. The aluminum foil entering and leaving the first cooling main roller 6 and the second cooling main roller 7 is redirected and transported through the auxiliary rollers 13. The auxiliary rollers 13 are used to guide the transmission direction of the aluminum foil and maintain the tension. By providing the auxiliary rollers 13 on both sides of the first cooling main roller 6 and the second cooling main roller 7, the length of the aluminum foil coated on the surface of the first cooling main roller 6 and the second cooling main roller 7 is increased, which is beneficial to cleaning and aluminum plating the surface of the aluminum foil.

[0038] A base and a sliding door are also provided, the vacuum chamber 1 is fixedly mounted on the base, one end of the vacuum chamber 1 is provided with an inlet, the sliding door can be slidably mounted on the base, and the sliding door can seal or open the inlet of the vacuum chamber 1. The vacuum chamber 1 is welded and processed using 304 stainless steel, the vacuum chamber 1 can be square or round, the vacuum chamber 1 and the door are both mounted on a large base, the lower part of the door is preferably equipped with rollers, and a mounting track is provided on the base, and the opening and closing of the door is preferably achieved by a motor driving the roller to roll on the track.

[0039] The control system includes a PLC and a touch screen, the touch screen can edit and input data into the editing module of the PLC, the vacuum chamber 1 is also provided with a vacuum gauge, a gas flow meter, a vacuum valve, a temperature sensor and an alarm, the vacuum gauge can sense the vacuum degree in the vacuum chamber and transmit a signal to the PLC, the gas flow meter can detect the argon flow rate sent into the vacuum chamber 1 by the argon supply device 5 and transmit a signal to the PLC, the temperature sensor can detect the surface temperature of the first cooling main roller 6 and the second cooling main roller 7 and transmit a signal to the PLC, the vacuum valve can connect the vacuum chamber with the outside world, and the PLC controls the alarm to sound an alarm. Through automated sensing and control, it is beneficial to improve the precise control of the thickness and roughness of the aluminum film on the surface of the aluminum foil.

[0040] A production process for roughening the surface of capacitor electrode aluminum foil, the steps of which are as follows:

[0041] Step 1: Load the rolled aluminum foil onto the unwinding roller 14, and lead one end of the aluminum foil out from the unwinding roller 14 and sequentially pass through the first cooling main roller 6 and the second cooling main roller 7 and finally pass through and around the winding roller 15;

[0042] Step 2: close the vacuum chamber 1, start the vacuum pump set 2, and evacuate the vacuum chamber 1;

[0043] Step 3: When the vacuum pressure in the vacuum chamber 1 reaches 5*10-1Pa, the hot and cold exchanger starts to cool the first cooling main roller 6 and the second cooling main roller 7, and the cooling temperature is set to -20°C;

[0044] Step 4: When the vacuum pressure in the vacuum chamber 1 reaches 5*10-3Pa, the argon gas supply device 5 is turned on to fill the vacuum chamber 1 with argon gas, and the vacuum pressure in the vacuum chamber 1 is stabilized at 6*10-1Pa;

[0045] Step 5: Turn on the unwinding drive device, the winding drive device and the cooling main roller drive device, set the aluminum foil linear speed to 2m / min, and the tension to 150N;

[0046] Step 6: Turn on the first surface ion source 9 and the second surface ion source 10, and set the first surface ion source 9 and the second surface ion source 10 to a current of 0.5A and a voltage of 1500V;

[0047] Step 7: Turn on the first arc ion target and the second arc ion target, and set the current of the first arc ion target and the second arc ion target to 450A;

[0048] Step 8: High-purity large-particle aluminum is deposited on both sides of the aluminum foil at the same time. After the rolled aluminum foil is rolled onto the winding roller 15, the control system prompts that the work is completed, and the first and second arc ion targets, the first and second ion sources, the argon gas supply device, the unwinding drive device, the winding drive device and the cooling main roller drive device are turned off;

[0049] Step 9: The hot and cold switches start heating up, and the heating temperature is set to 35°C;

[0050] Step 10: Close the vacuum valve of the exhaust pipeline, stop the vacuum pump group 2, and open the vacuum valve on the vacuum chamber 1 to break the vacuum;

[0051] Step 11: Open the door of the vacuum chamber 1, remove the aluminum foil roll on the winding roller 15, and the surface roughening treatment of the aluminum foil is completed.

Claims

1. A production equipment for roughening the surface of capacitor electrode aluminum foil, characterized by: The invention comprises a vacuum chamber (1), a vacuum pump group (2), a first rectangular arc ion target (3), a second rectangular arc ion target (4), an argon gas supply device (5), a discharge device, a collection device, a first cooling main roller (6), a second cooling main roller (7), a cooling system and a control system. The vacuum pump group can evacuate the vacuum chamber. The first cooling main roller and the second cooling main roller can be installed in the vacuum chamber so as to rotate synchronously. The first cooling main roller and the second cooling main roller are provided with cooling channels. The discharge device and the collection device are respectively installed in the vacuum chamber. The aluminum foil (8) drawn from the discharge device is sequentially wound around the surfaces of the first cooling main roller and the second cooling main roller and then collected by the collection device. The surface of one side of the aluminum foil is connected to the first cooling main roller. The first side arc ion target is opposite to the aluminum foil on the surface of the first cooling main roller, and the second side arc ion target is opposite to the aluminum foil on the surface of the second cooling main roller. The first side arc ion target and the second side arc ion target can deposit large particles of aluminum on the surface of the aluminum foil respectively. The cooling system can provide cooling liquid to the first side cooling main roller, the second side cooling main roller, the first side arc ion target, the second side arc ion target and the vacuum pump group. The argon gas supply device can provide argon gas to the vacuum chamber. The control system controls the operation of the vacuum pump group, the first side arc ion target, the second side arc ion target, the argon gas supply device, the material discharge device, the material collection device, the first side cooling main roller, the second side cooling main roller and the cooling system. A surface ion source (9) and a second surface ion source (10), wherein the first surface ion source is directly opposite to the aluminum foil on the surface of the first cooling main roller, and the first surface ion source and the first surface arc ion target are arranged in sequence along the aluminum foil conveying direction, the second surface ion source is directly opposite to the aluminum foil on the surface of the second cooling main roller, and the second surface ion source and the second surface arc ion target are arranged in sequence along the aluminum foil conveying direction, the first surface ion source and the second surface ion source can respectively perform electric ion bombardment cleaning on the surface of the aluminum foil, the cooling system can provide cooling liquid to the first surface ion source and the second surface ion source, and a water cooling partition (16) is also provided, wherein the water cooling partition is fixedly installed in a vacuum chamber, and the inner side wall opposite to the water cooling partition and the vacuum chamber respectively encloses a first arc ion target installation chamber (11) and a second arc ion target installation chamber (12). The first surface arc ion target and the second surface arc ion target are respectively fixedly installed in the first arc ion target installation chamber and the second arc ion target installation chamber, the first surface cooling main roller and the second surface cooling main roller are respectively covered with aluminum foil and the outer surface surface of the first arc ion target installation chamber and the second arc ion target installation chamber respectively extend into the first arc ion target installation chamber and the second arc ion target installation chamber through the notch portion of the water cooling partition plate, the first surface ion source and the second surface ion source are respectively located outside the first arc ion target installation chamber and the second arc ion target installation chamber, two argon gas supply devices respectively provide argon gas to the first arc ion target installation chamber and the second arc ion target installation chamber, the first surface cooling main roller and the second surface cooling main roller form a cooling channel with a sandwich structure inside, and the cooling channel is connected to the cooling system through a cold and hot exchanger,A cooling main roller drive device is also provided, and the cooling main roller drive device drives the first cooling main roller and the second cooling main roller to rotate synchronously respectively. The unwinding device includes an unwinding roller (14) and an unwinding drive device, and the rewinding device includes a rewinding roller (15) and a rewinding drive device. The unwinding drive device and the rewinding drive device drive the unwinding roller and the rewinding roller to rotate respectively. An aluminum foil tension sensor is also provided, and the aluminum foil tension sensor can sense the aluminum foil tension and transmit a signal to the control system, and the control system controls the actions of the unwinding drive device and the rewinding drive device.

2. The production equipment for roughening the surface of capacitor electrode aluminum foil according to claim 1, characterized in that: A plurality of auxiliary rollers (13) are also provided. At least one auxiliary roller is provided on both sides of the first cooling main roller and the second cooling main roller. The aluminum foil entering and leaving the first cooling main roller and the second cooling main roller is redirected and transported via the auxiliary rollers.

3. The production equipment for roughening the surface of capacitor electrode aluminum foil according to claim 1, characterized in that: A base and a sliding door are also provided. The vacuum cavity is fixedly installed on the base. An inlet is provided at one end of the vacuum cavity. The sliding door can be slidably installed on the base. The sliding door can seal and close or open the inlet of the vacuum cavity.

4. The production equipment for roughening the surface of capacitor electrode aluminum foil according to claim 1, characterized in that: The control system includes a PLC and a touch screen. The touch screen can edit and input data into the editing module of the PLC. The vacuum chamber is also provided with a vacuum gauge, a gas flow meter, a vacuum valve, a temperature sensor and an alarm. The vacuum gauge can sense the vacuum degree in the vacuum chamber and transmit a signal to the PLC. The gas flow meter can detect the flow rate of argon gas sent into the vacuum chamber by the argon gas supply device and transmit a signal to the PLC. The temperature sensor can detect the surface temperature of the first-side cooling main roller and the second-side cooling main roller and transmit a signal to the PLC. The vacuum valve can connect the vacuum chamber with the outside world. The PLC controls the alarm to sound an alarm.

5. A production process for roughening the surface of capacitor electrode aluminum foil using the production equipment for roughening the surface of capacitor electrode aluminum foil according to claim 1, characterized in that: The steps are as follows: Step 1: Load the rolled aluminum foil onto the unwinding roller, and lead one end of the aluminum foil out of the unwinding roller and pass through the first cooling main roller and the second cooling main roller in sequence, and finally pass through and wrap around the winding roller; Step 2: Close the vacuum chamber, start the vacuum pump group, and evacuate the vacuum chamber; Step 3: When the vacuum pressure in the vacuum chamber reaches 5*10-1Pa, the hot and cold exchanger starts to cool the first cooling main roller and the second cooling main roller, and the cooling temperature is set to -20℃; Step 4: When the vacuum pressure in the vacuum chamber reaches 5*10-3Pa, the argon gas supply device is turned on to fill the vacuum chamber with argon gas, and the vacuum pressure in the vacuum chamber is stabilized at 6*10-1Pa; Step 5: Turn on the unwinding drive device, the winding drive device and the cooling main roller drive device, set the aluminum foil linear speed to 2m / min, and the tension to 150N; Step 6: Turn on the first surface ion source and the second surface ion source, and set the first surface ion source and the second surface ion source to a current of 0.5A and a voltage of 1500V; Step 7: Turn on the first arc ion target and the second arc ion target, and set the current of the first arc ion target and the second arc ion target to 450A; Step 8: High-purity large-particle aluminum is deposited on both sides of the aluminum foil at the same time. After the rolled aluminum foil is rolled onto the winding roller, the control system prompts that the work is completed, and the first and second arc ion targets, the first and second ion sources, the argon gas supply device, the unwinding drive device, the winding drive device and the cooling main roller drive device are turned off; Step 9: The hot and cold switches start heating up, and the heating temperature is set to 35°C; Step 10: Close the vacuum valve of the exhaust pipeline, stop the vacuum pump group, and open the vacuum valve on the vacuum chamber to break the vacuum; Step 11: Open the door of the vacuum chamber and remove the aluminum foil roll from the winding roller. The surface roughening treatment of the aluminum foil is completed.

Citation Information

Patent Citations

  • Production equipment for roughening surface of capacitor electrode aluminum foil

    CN212365759U