Photosensitive body for electrophotography, method for producing the same, and electrophotographic device
By using high-concentration dispersed inorganic oxides and lubricating resins in the photoreceptor, combined with the surface treatment of silane coupling agent, the friction and film formation problems during long-term use of the photoreceptor are solved, and stable images and high-quality Photoreceptor.
Patent Information
- Application Number
- CN202010077715.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-18
- Filing Date
- 2020-01-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-01-31
AI Technical Summary
The prior art is difficult to achieve low friction and stable image on the surface of the photoreceptor during long-term use, and there is a film formation problem, which affects the electrical characteristics and cleanliness of the photoreceptor.
A photosensitive layer containing inorganic oxides and lubricating resin is used to disperse the inorganic oxides at a high concentration and perform surface treatment with a silane coupling agent to form a negative charged laminated type, a positive charged single layer type or a positive charged laminated type photosensitive body. Improve mechanical strength and friction resistance while reducing friction to prevent film formation.
It is achieved to reduce the friction consumption of the photoreceptor surface during long-term use, avoid film formation, maintain image stability and improve cleanliness, and ensure high quality and durability of the photoreceptor.
Smart Images

Figure CN111708261B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electrophotographic photoreceptor (hereinafter also referred to as a "photoreceptor"), a method for producing the same, and an electrophotographic apparatus. Specifically, the present invention relates to an electrophotographic photoreceptor mainly composed of a photosensitive layer containing a conductive substrate and an organic material and used in an electrophotographic printer, a copier, a facsimile machine, etc., a method for producing the same, and an electrophotographic apparatus. Background Art
[0002] Electrophotographic photoreceptors have a basic structure in which a photosensitive layer having a photoconductive function is provided on a conductive substrate. In recent years, research and development of organic electrophotographic photoreceptors using organic compounds as functional components responsible for charge generation and transport has been actively carried out due to the diversity of materials, high productivity, safety and other advantages, and their application in copiers and printers is also progressing.
[0003] Generally speaking, a photoreceptor must have the function of maintaining surface charges in the dark, the function of receiving light and generating charges, and the function of transporting the generated charges. The photosensitive layer plays these roles. Photoreceptors are classified into so-called single-layer photoreceptors and laminated (functionally separated) photoreceptors according to the morphology of the photosensitive layer. A single-layer photoreceptor has a single-layer photosensitive layer that has both a charge generating function and a charge transporting function. A laminated photoreceptor has a photosensitive layer formed by laminating a charge generating layer and a charge transporting layer. The charge generating layer mainly plays the function of generating charges when receiving light. The charge transporting layer plays the function of maintaining surface charges in the dark and the function of transporting charges generated in the charge generating layer when receiving light.
[0004] The photosensitive layer is usually formed by applying a coating solution in which a charge generating material, a charge transporting material and a resin binder are dissolved or dispersed in an organic solvent onto a conductive substrate. In many of these organic electrophotographic photoreceptors, especially the outermost surface layer, polycarbonate is used as a resin binder because of its strong friction with paper or with a scraper for removing toner, excellent flexibility and good transmittance for exposure.
[0005] On the other hand, as an electronic photographic device in recent years, the so-called digital machine has become the mainstream. It uses monochromatic light such as argon, helium-neon, semiconductor laser or light-emitting diode as the exposure light source, digitizes information such as images and text and converts them into light signals. The light is irradiated on the charged photoreceptor to form an electrostatic latent image on the surface of the photoreceptor, which is visualized by toner.
[0006] As a method for charging a photoreceptor, there are non-contact charging methods in which a charging member such as a scorotron does not contact the photoreceptor, and contact charging methods in which a charging member such as a semi-conductive rubber roller or brush contacts the photoreceptor. Among them, the contact charging method has the following advantages compared to the non-contact charging method: because corona discharge occurs very close to the photoreceptor, less ozone is generated and the applied voltage can be lower. Therefore, since it can realize a smaller, lower-cost, and less environmentally friendly electronic photographic device, it has become the mainstream in medium-sized to small devices.
[0007] As a method for cleaning the surface of the photoreceptor, the process of scraping with a scraper and the process of cleaning during development are mainly used. In the cleaning with a scraper, the untransferred residual toner on the surface of the organic photoreceptor is sometimes scraped off with the scraper, and the scraped toner is recovered into a waste toner box or returned to the developer again. Such a cleaner using a scraper requires a space for a toner recovery box or toner recycling, and it is also necessary to monitor whether the toner recovery box is full. In addition, when paper powder or external additives remain on the scraper, it may sometimes cause damage to the surface of the organic photoreceptor and shorten the life of the photoreceptor. Therefore, sometimes a process is set up to recover the toner in the development process, or to magnetically or electrically attract the residual toner attached to the surface of the photoreceptor just before the development process.
[0008] Furthermore, when using a cleaning scraper, the rubber hardness and contact pressure of the scraper need to be increased to improve the cleaning performance, which may cause the photosensitive body to wear more, potential fluctuation or sensitivity fluctuation to occur, image anomalies to occur, and poor color balance or reproducibility in a color machine.
[0009] On the other hand, when a contact charging mechanism is used and a cleaning-free mechanism is used in which a developing device is used for developing and cleaning, toner with a changed charge amount is generated in the contact charging mechanism portion. In addition, if there is reverse polarity toner that may be mixed in a very small amount, there is a problem that such toner cannot be fully removed from the photosensitive body and the charging device is contaminated.
[0010] In addition, sometimes the surface of the photoreceptor is contaminated by ozone or nitrogen oxides generated when the photoreceptor is charged. In this case, in addition to the problem of image flow caused by the pollutants themselves, there are also the following problems: the attached substances reduce the lubricity of the photoreceptor surface; paper dust or toner is easily attached; the scraper is prone to squeaking or flipping up, and the surface is easily scratched.
[0011] In addition, in order to improve the toner transfer efficiency in the transfer process, the transfer current is optimized by matching the temperature and humidity environment and the characteristics of the paper, and attempts are made to reduce the residual toner by improving the transfer efficiency. In addition, as an organic photoreceptor suitable for such a treatment and contact charging method, an organic photoreceptor with improved toner release properties and an organic photoreceptor with less transfer influence are required.
[0012] In order to solve these technical problems, a method for improving the outermost surface layer of the photoreceptor has been proposed. For example, in Patent Documents 1 and 2, a method of adding fillers to the surface layer of the photosensitive layer is proposed to improve the durability of the photoreceptor surface. However, it is difficult to evenly disperse the filler by dispersing the filler in the film. In addition, due to the presence of filler agglomerates, or the reduction in the transmittance of the film, or the filler scattering the exposure light, the charge transport and charge generation will become uneven, and the image characteristics will sometimes decrease. In addition, there is a method of adding a dispersing material to improve the dispersibility of the filler, but in this case, the dispersing material itself will affect the photoreceptor characteristics, so it is difficult to achieve the dispersibility of the filler and the photoreceptor characteristics at the same time. In addition, although the wear resistance can be improved by adding fillers, filming (Japanese: フィィルミング) is likely to occur on the surface of the photoreceptor, and the treatment of image defects is not considered.
[0013] In addition, in order to improve wear resistance, patent documents 3, 4, 5, and 6 propose a scheme of making the photosensitive layer contain filler particles, but the influence of the agglomeration of particles on the photosensitive body characteristics when preparing the photosensitive layer coating liquid, the method of preparing the particles, and the influence related to impurity control and surface treatment have not been fully verified.
[0014] In addition, in Patent Document 7, in order to obtain a photoreceptor that has little wear even during long-term use and can achieve stable images, a scheme is proposed to form a photosensitive layer using an inorganic oxide that meets specific conditions, but the problem of film formation on the surface of the photoreceptor is not studied.
[0015] On the other hand, in order to protect the photosensitive layer and improve the mechanical strength, improve the surface lubricity, etc., a method of forming a surface protection layer on the photosensitive layer has been proposed. However, in these methods of forming the surface protection layer, there are technical problems such as difficulty in film formation on the charge transport layer and difficulty in fully realizing the charge transport performance and the charge retention function at the same time.
[0016] Prior art literature
[0017] Patent Literature
[0018] Patent Document 1: Japanese Patent Application Laid-Open No. 1-205171
[0019] Patent Document 2: Japanese Patent Laid-Open No. 7-333881
[0020] Patent Document 3: Japanese Patent Application Publication No. 2008-176054
[0021] Patent Document 4: Japanese Patent Application Publication No. 2002-91021
[0022] Patent Document 5: Japanese Patent Application Publication No. 2002-229239
[0023] Patent Document 6: Japanese Patent Application Publication No. 2015-169858
[0024] Patent Document 7: International Publication No. 2017 / 110300 Summary of the invention
[0025] Technical problem to be solved by the invention
[0026] As mentioned above, various technical solutions have been proposed for improving the outermost surface layer of the photoreceptor. However, the technologies disclosed in these patent documents cannot simultaneously achieve low wear and stable images during long-term use, and are insufficient to maintain good electrical properties.
[0027] Therefore, an object of the present invention is to provide an electrophotographic photosensitive body, a method for producing the same, and an electrophotographic apparatus that can reduce the amount of wear on the photosensitive body surface even during long-term use, and can obtain stable images without causing filming on the photosensitive body surface.
[0028] Technical solutions adopted to solve technical problems
[0029] In order to solve the above technical problems, the inventors have conducted careful research on the material of the outermost surface layer of a photoreceptor, and as a result, provided a photoreceptor having excellent wear resistance of the film, few image defects, and stable image quality during repeated use. Specifically, the inventors found that a good electrophotographic photoreceptor can be obtained by adopting the following structure, and finally completed the present invention.
[0030] That is, the first form of the electronic photographic photosensitive body of the present invention comprises: a conductive substrate; and a negatively charged stacked photosensitive layer composed of a charge generating layer and a charge transporting layer sequentially formed on the conductive substrate, wherein the charge transporting layer comprises an inorganic oxide and a lubricating resin, and when a 20 mass % inorganic oxide slurry obtained by dispersing the inorganic oxide at a concentration of 20 mass % relative to a solvent is irradiated with light of a wavelength of 780 nm, the transmittance of the light is above 40%.
[0031] In addition, the second form of the electronic photographic photosensitive body of the present invention comprises: a conductive substrate; and a single-layer photosensitive layer formed on the above-mentioned conductive substrate and comprising an inorganic oxide and a lubricating resin, wherein the transmittance of a 20 mass % inorganic oxide slurry obtained by dispersing the above-mentioned inorganic oxide at a concentration of 20 mass % relative to a solvent when irradiated with light of a wavelength of 780 nm is 40% or more.
[0032] In addition, the third form of the electronic photographic photosensitive body of the present invention comprises: a conductive substrate; and a positively charged stacked photosensitive layer composed of a charge transport layer and a charge generating layer formed in sequence on the above-mentioned conductive substrate, wherein the above-mentioned charge generating layer contains an inorganic oxide and a lubricating resin, and when a 20 mass% inorganic oxide slurry obtained by dispersing the above-mentioned inorganic oxide at a concentration of 20 mass% relative to a solvent is irradiated with light of a wavelength of 780nm, the transmittance of the above-mentioned light is above 40%.
[0033] The present invention also found that by making the photosensitive layer contain inorganic oxides, the mechanical strength of the photosensitive layer can be improved. In addition, by using inorganic oxides that show very high light transmittance when dispersed in a solvent at a high concentration, a high-quality photoreceptor can be provided. In this case, the viscosity of the above-mentioned 20 mass% inorganic oxide slurry is preferably below 50mPa·s. In addition, the primary particle size of the above-mentioned inorganic oxide is preferably 1 to 500nm as long as the inorganic oxide can maintain high transmittance after being dispersed in the solvent.
[0034] The lubricating resin preferably includes a polycarbonate resin containing a siloxane structure, and more preferably includes a polyarylate resin containing a siloxane structure. In addition, the photosensitive layer may be the outermost layer.
[0035] In addition, the inorganic oxide preferably has silicon dioxide as the main component, more preferably has silicon dioxide as the main component and contains aluminum element of more than 1ppm and less than 1000ppm. It is also preferred that the inorganic oxide is surface treated with a silane coupling agent. As the silane coupling agent, a silane coupling agent having a structure shown in the following general formula (1) is preferably used.
[0036] (R1) n -Si-(OR2) 4-n (1)
[0037] (In the formula, Si represents a silicon atom, R1 represents an organic group in which carbon is directly bonded to the silicon atom, R2 represents an organic group, and n represents an integer of 0 to 3.)
[0038] The fourth form of the method for manufacturing an electronic photographic photosensitive body of the present invention is a method for manufacturing the above-mentioned electronic photographic photosensitive body by using a photosensitive layer coating liquid to form the above-mentioned photosensitive layer containing an inorganic oxide and a lubricating resin, which includes: an inorganic oxide slurry preparation step of dispersing the above-mentioned inorganic oxide in the solvent for the above-mentioned photosensitive layer coating liquid once to obtain an inorganic oxide slurry; a photosensitive layer forming liquid preparation step of dissolving a charge transport material and a lubricating resin in the solvent for the above-mentioned photosensitive layer coating liquid to obtain a photosensitive layer forming liquid; and a photosensitive layer coating liquid preparation step of mixing the obtained inorganic oxide slurry and the above-mentioned photosensitive layer forming liquid to obtain the above-mentioned photosensitive layer coating liquid.
[0039] Furthermore, an electrophotographic apparatus according to a fifth aspect of the present invention is formed by mounting the above-mentioned electrophotographic photoreceptor.
[0040] Effects of the Invention
[0041] According to the present invention, by using a photosensitive layer having the above conditions, it is possible to obtain an electrophotographic photoreceptor that can reduce the amount of wear on the photoreceptor surface even during long-term use, prevent filming on the photoreceptor surface, and obtain stable images.
[0042] This is considered to be due to the following reasons.
[0043] In the present invention, the mechanical strength of the photosensitive layer can be improved by making the photosensitive layer contain inorganic oxides, but in the prior art, there is the following defect: when the inorganic oxide is dispersed alone in a solvent, an agglomerated part is generated, and then in the dispersion when mixed with a charge transport material or a resin component, the viscosity increases due to the addition of the resin component, so that it cannot be fully dispersed, resulting in a photosensitive body with tiny defects on the image. In contrast, in the present invention, because the inorganic oxide exhibits very high light transmittance after being dispersed in a solvent at a high concentration, it is believed that the inorganic oxide is in a uniform dispersion state and maintains a solvated state in a state close to that of primary particles. That is, in the present invention, even if the inorganic oxide is dispersed in a solvent at a high concentration, the viscosity of the slurry (dispersion liquid) is low, and as a result, it is easy to mix with a coating liquid in which other constituent components of the photosensitive layer are dissolved, so the agglomeration during mixing is also reduced, and thus a higher quality photosensitive body can be provided.
[0044] On the other hand, when only inorganic oxides are contained, although the amount of wear on the surface of the photoreceptor can be reduced, the friction between the cleaning blade and the surface of the photoreceptor increases. In particular, when the particle size of the inorganic oxide is 200 to 500 nm, the surface temperature of the photoreceptor is easily increased by the inorganic oxide. The silica component as an external additive contained in the toner becomes soft due to the surface temperature of the photoreceptor and easily adheres to the inorganic oxide, making it impossible to cleanly remove it with the cleaning blade, and film formation is easily generated on the surface of the photoreceptor. In the present invention, by using inorganic oxides and lubricating resins, the friction between the cleaning blade and the surface of the photoreceptor can be greatly reduced, the rise in the surface temperature of the photoreceptor can be suppressed, the cleanliness is improved, and the problem of film formation can be eliminated. By combining such a specific inorganic oxide and lubricating resin, wear resistance and film formation resistance can be achieved at the same time, which is the first result obtained through the research of the inventors. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] FIG. 1 is a schematic cross-sectional view showing a negatively charged laminated electrophotographic photoreceptor of the present invention.
[0046] Figure 1B It is a schematic cross-sectional view showing a positively charged single-layer electrophotographic photoreceptor of the present invention.
[0047] Figure 1C It is a schematic cross-sectional view showing a positively charged laminated electrophotographic photoreceptor of the present invention.
[0048] Figure 2 This is a flow chart showing an example of a method for producing an electrophotographic photoreceptor of the present invention.
[0049] Figure 3 This is a simplified structural diagram showing an example of the structure of the electronic photographic apparatus of the present invention.
[0050] Explanation of symbols
[0051] 1 Conductive substrate
[0052] 2 Basal layer
[0053] 3 Single-layer photosensitive layer
[0054] 4 Charge generation layer
[0055] 5 Charge transport layer
[0056] 6,7 Laminated photosensitive layer
[0057] 8 Photoreceptor
[0058] 21 Live components
[0059] 22 High voltage power supply
[0060] 23 Image Exposure Component
[0061] 24 Developer
[0062] 241 Development Roller
[0063] 25 Paper feeding member
[0064] 251 Feed roller
[0065] 252 Paper guide
[0066] 26 Transfer charger (direct charging type)
[0067] 27 Cleaning device
[0068] 271 Cleaning scraper
[0069] 28. Anti-static components
[0070] 60 Electronic photography device
[0071] 300 Photosensitive layer. DETAILED DESCRIPTION
[0072] The embodiments of the present invention are described in detail below with reference to the accompanying drawings. The present invention is not limited to the following description.
[0073] As described above, electrophotographic photoreceptors are roughly classified into so-called negatively charged laminated photoreceptors and positively charged laminated photoreceptors, which are laminated (functionally separated) photoreceptors, and single-layer photoreceptors mainly used as positively charged ones. Figure 1A to Figure 1C This is a schematic cross-sectional view showing an electrophotographic photoreceptor according to one embodiment of the present invention. Figure 1A It represents a negatively charged laminated electrophotographic photoreceptor, Figure 1B It refers to a positively charged single-layer electrophotographic photoreceptor, Figure 1C It indicates a positively charged laminated electrophotographic photoreceptor.
[0074] As shown in the figure, in the negatively charged laminated photoreceptor, a base layer 2 and a photosensitive layer 6 having a charge generating layer 4 and a charge transporting layer 5 are sequentially laminated on a conductive substrate 1, wherein the charge generating layer 4 has a charge generating function and the charge transporting layer 5 has a charge transporting function. On the other hand, in the positively charged single-layer photoreceptor, a base layer 2 and a single-layer photosensitive layer 3 having both charge generating and charge transporting functions are sequentially laminated on a conductive substrate 1. In addition, in the positively charged laminated photoreceptor, a base layer 2 and a photosensitive layer 7 having a charge transporting layer 5 and a charge generating layer 4 are sequentially laminated on a conductive substrate 1, wherein the charge transporting layer 5 has a charge transporting function and the charge generating layer 4 has both charge generating and charge transporting functions. In addition, in any type of photoreceptor, it is sufficient to provide a base layer 2 as needed. In addition, the "photosensitive layer" of the present invention includes both a laminated photosensitive layer obtained by laminating a charge generating layer and a charge transporting layer, and a single-layer photosensitive layer.
[0075] The photoreceptor according to the embodiment of the present invention has at least a photosensitive layer on a conductive substrate, the photosensitive layer comprising an inorganic oxide and a lubricating resin, and as the inorganic oxide, an inorganic oxide having a light transmittance of 40% or more when a 20% by mass inorganic oxide slurry obtained by dispersing the inorganic oxide at a concentration of 20% by mass relative to a solvent is irradiated with light of a wavelength of 780 nm is used. The transmittance is preferably 80% or more.
[0076] In the case where the photoreceptor according to an embodiment of the present invention is a single-layer type, the single-layer photosensitive layer is the above-mentioned photosensitive layer containing an inorganic oxide and a lubricating resin. In addition, in the case where the photoreceptor according to an embodiment of the present invention is a negatively charged stacked type having a negatively charged stacked type photosensitive layer composed of a charge generating layer and a charge transport layer formed in sequence on a conductive substrate, the charge transport layer is a photosensitive layer containing an inorganic oxide and a lubricating resin. In addition, in the case where the photoreceptor according to an embodiment of the present invention is a positively charged stacked type having a positively charged stacked type photosensitive layer composed of a charge transport layer and a charge generating layer formed in sequence on a conductive substrate, the charge generating layer is a photosensitive layer containing an inorganic oxide and a lubricating resin. In particular, in the case where the above-mentioned photosensitive layer containing an inorganic oxide and a lubricating resin is the outermost surface layer, the effect of improving wear resistance can be well obtained, which is preferred.
[0077] The inorganic oxide may be any inorganic oxide having a transmittance within the above range after being dispersed in a solvent, and examples thereof include aluminum oxide, zirconium oxide, titanium oxide, tin oxide, zinc oxide, and the like in addition to silicon dioxide as a main component.
[0078] Among them, inorganic oxides having silicon dioxide as a main component are preferred. The following methods are known as methods for producing silicon dioxide particles having a particle size of about several nanometers to several tens of nanometers: a method called a wet method using water glass as a raw material; a method called a dry method using chlorosilane or the like in a gas phase; a method using an alkoxide as a silicon dioxide precursor as a raw material, etc.
[0079] Here, when silicon dioxide is surface treated, if a large amount of heterogeneous metal exists as an impurity, defects are generated due to the metal different from the usual oxide site, the charge distribution on the surface changes, and the cohesion of the oxide particles increases starting from the site, resulting in an increase in the cohesion in the coating liquid or the photosensitive layer, so the purity of silicon dioxide is preferably high. Therefore, the content of metals other than the metal elements constituting the inorganic oxide is preferably controlled to be less than 1000ppm for each metal element.
[0080] On the other hand, in order to make the surface treatment agent fully react and improve the activity of the silica surface, it is preferred to add a very small amount of other types of metals in advance. The surface treatment agent reacts with the hydroxyl groups present on the surface of silica, but if silica contains a trace of other metal elements, the reactivity of the silanol groups (hydroxyl groups) adjacent to other metal elements present on the silica surface will be improved due to the influence of the difference in electronegativity between the metals. The hydroxyl group has high reactivity with the surface treatment agent, so it reacts with the surface treatment agent more strongly than other hydroxyl groups, and if it remains, it will cause cohesion. And after the reaction of these surface treatment agents, by the surface treatment agent and other hydroxyl reactions, due to the effect of the surface treatment agent and the reduction effect of the surface charge bias caused by the heterogeneous metal on the surface, the cohesion of silica between each other is greatly improved. Therefore, in the case where the inorganic oxide contains a trace of other metals, the reactivity of the surface treatment agent becomes better, and the result is that the dispersibility produced by the surface treatment is improved, so it is preferred.
[0081] Regarding silicon dioxide, if aluminum is added in a range below 1000ppm, it is suitable for surface treatment. The adjustment of the amount of aluminum in silicon dioxide can be carried out using the methods described in Japanese Patent Laid-Open No. 2004-143028, Japanese Patent Laid-Open No. 2013-224225, Japanese Patent Laid-Open No. 2015-117138, etc., but as long as it can be controlled within the desired range, the adjustment method is not particularly limited. Specifically, as a method for better controlling the amount of aluminum on the surface of silicon dioxide, for example, there is the following method. First, when manufacturing silicon dioxide particles, after the silicon dioxide particles are grown to a shape smaller than the target silicon dioxide particle size, an aluminum alkoxide that becomes an aluminum source is added to control the amount of aluminum on the surface of silicon dioxide. In addition, there is also a method of adding silicon dioxide particles to a solution containing aluminum chloride, applying an aluminum chloride solution on the surface of the silicon dioxide particles, and firing it after drying; and a method of reacting a mixed gas of an aluminum halide compound and a silicon halide compound, etc.
[0082] In addition, it is known that the structure of silica adopts a network-like bonding structure in which multiple silicon atoms and oxygen atoms are connected in a ring shape. When aluminum is contained, the number of atoms constituting the ring structure of silica becomes larger than that of ordinary silica due to the effect of mixing aluminum. Due to this effect, the steric hindrance when the surface treatment agent reacts with the hydroxyl group on the surface of silica containing aluminum is more moderate than that of ordinary silica surface, and the reactivity of the surface treatment agent is improved, resulting in a surface-treated silica with further improved dispersibility than when the same surface treatment agent is reacted with ordinary silica.
[0083] Here, in order to control the amount of aluminum element, silicon dioxide produced by a wet process is more preferred. In addition, considering the reactivity of the surface treatment agent, the content of aluminum element relative to silicon dioxide is preferably 1 ppm or more.
[0084] The form of the inorganic oxide is not particularly limited, but the sphericity of the inorganic oxide is preferably 0.8 or more, more preferably 0.9 or more, in order to reduce cohesion and obtain a uniform dispersion state.
[0085] In addition, the viscosity when the inorganic oxide is dispersed (primary dispersion) in the solvent is measured by the viscosity of a 20 mass% inorganic oxide slurry when dispersed at a concentration of 20 mass% relative to the solvent. From the perspective of promoting ideal mixing, it is preferably set to 50 mPa·s or less, and more preferably set to 10 mPa·s or less.
[0086] In addition, the primary particle size of the inorganic oxide is preferably 1 to 500 nm, more preferably 5 to 400 nm, and further preferably 10 to 300 nm, as long as the inorganic oxide can maintain high transmittance after being dispersed in the solvent. In addition, the particles in the dispersion may be in the shape of primary particles or may form a plurality of clusters, as long as the transmittance is within the range satisfying the above range.
[0087] In addition, the average distance between the particles of the inorganic oxide in the photosensitive layer is not particularly limited as long as the above-mentioned transmittance can be obtained. As a result, when the primary particle size is close, the binding force on the film components can be improved due to the interaction between the particles, which is related to the improvement of the abrasiveness of the film. Specifically, it is preferably below 200nm, and more preferably below 70nm.
[0088] In addition, when an inorganic oxide is used in the charge transport layer of a photoreceptor that is expected to have high resolution, it is better to consider the influence of α rays and the like from the material added to the charge transport layer. For example, if a semiconductor storage element is taken as an example, the storage element maintains the type of stored data according to whether or not charge is accumulated, but the size of the accumulated charge is also reduced by miniaturization, and the type of data changes due to the change in the degree of charge caused by the α rays irradiated from the outside, resulting in an unexpected data change. In addition, since the size of the current flowing in the semiconductor element is also reduced, the current (noise) generated by the α rays will also be relatively large compared to the size of the signal, which may cause malfunction. Similar to this phenomenon, if the influence of the charge transport layer of the photoreceptor on the movement of charge is considered, it is more preferable to use a material that generates less α rays as a film constituent material. Specifically, it is effective to reduce the concentration of uranium and thorium in the inorganic oxide, preferably thorium is below 30 ppb and uranium is below 1 ppb. As a method for reducing the amount of uranium and thorium in the inorganic oxide, for example, there is a description in Japanese Patent Application Laid-Open No. 2013-224225, etc. However, the method is not limited to this method as long as the concentration of these elements can be reduced.
[0089] In order to maintain the transmittance conditions of the present invention for the inorganic oxide, it is preferred that the surface of the inorganic oxide be subjected to a surface treatment.
[0090] As a surface treatment agent, as long as the above-mentioned transmittance can be obtained, a commercially available surface treatment agent can be used. It is more preferred to use a silane coupling agent. As a silane coupling agent, phenyl trimethoxysilane, vinyl trimethoxysilane, epoxy trimethoxysilane, methacrylic trimethoxysilane, amino trimethoxysilane, urea trimethoxysilane, mercaptopropyl trimethoxysilane, isocyanatopropyl trimethoxysilane, phenyl amino trimethoxysilane, acrylic trimethoxysilane, p-phenyl trimethoxysilane, 3-acryloxypropyl trimethoxysilane, 3-methacryloxypropyl trimethoxysilane, 3-isocyanatopropyl trimethoxysilane, 3-aminopropyl trimethoxysilane and N-phenyl-3-aminopropyl trimethoxysilane, etc., can be cited, and a silane coupling agent containing at least one of them can be used. In addition, the alkyl group of the alkoxy group is preferably a methyl group, but in addition, ethyl, propyl, and butyl are also preferred. The treatment amount of the surface treatment agent to the inorganic oxide is 0.01 to 10.0% by mass, preferably 0.05 to 5.0% by mass, relative to the mass of the inorganic oxide after treatment.
[0091] More specifically, the silane coupling agent may be a compound having a structure represented by the following general formula (1), but the silane coupling agent is not limited to the following compounds as long as it is a compound that undergoes a condensation reaction with a reactive group such as a hydroxyl group on the surface of the inorganic oxide.
[0092] (R1) n -Si-(OR2) 4-n (1)
[0093] (In the formula, Si represents a silicon atom, R1 represents an organic group in which carbon is directly bonded to the silicon atom, R2 represents an organic group, and n represents an integer of 0 to 3.)
[0094] In the organosilicon compound represented by the general formula (1), R1 may be alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl, and dodecyl; aryl groups such as phenyl, tolyl, naphthyl, and biphenyl; epoxy-containing groups such as γ-glycidoxypropyl and β-(3,4-epoxycyclohexyl)ethyl; methacryloyl-containing groups such as γ-acryloxypropyl and γ-methacryloxypropyl; γ-hydroxypropyl, 2,3-dihydroxypropyl; Hydroxyl-containing groups such as oxypropyl; vinyl-containing groups such as vinyl and propenyl; mercapto-containing groups such as γ-mercaptopropyl; amino-containing groups such as p-aminophenyl, γ-aminopropyl, N-β(aminoethyl)-γ-aminopropyl, N-phenyl-3-aminopropyl; halogen-containing groups such as m-aminophenyl, o-aminophenyl, γ-chloropropyl, 1,1,1-trifluoropropyl, nonafluorohexyl, perfluorooctylethyl; other nitro and cyano-substituted alkyl groups. In addition, as the hydrolyzable group of OR2, alkoxy groups such as methoxy and ethoxy, halogen groups, and acyloxy groups can be mentioned.
[0095] The silane coupling agent represented by the general formula (1) may be used alone or in combination of two or more. When multiple silane coupling agents are used in combination, two silane coupling agents may be reacted with the inorganic oxide simultaneously, or multiple silane coupling agents may be reacted sequentially.
[0096] In addition, in the silane coupling agent represented by the general formula (1), when n is 2 or more, multiple R1s may be the same or different. Similarly, when n is 2 or less, multiple R2s may be the same or different. In addition, when two or more organosilicon compounds represented by the general formula (1) are used, R1 and R2 may be the same or different in each coupling agent.
[0097] As the compound in which n is 0, for example, the following compounds may be mentioned. That is, tetramethoxysilane, tetraacetoxysilane, tetraethoxysilane, tetraallyloxysilane, tetrapropoxysilane, tetraisopropoxysilane, tetra(2-methoxyethoxy)silane, tetrabutoxysilane, tetraphenoxysilane, tetra(2-ethylbutoxy)silane, tetra(2-ethylhexyloxy)silane and the like may be mentioned.
[0098] As the compound in which n is 1, for example, the following compounds may be mentioned. That is, methyltrimethoxysilane, mercaptomethyltrimethoxysilane, trimethoxyvinylsilane, ethyltrimethoxysilane, 3,3,3-trifluoropropyltrimethoxysilane, 3-chloropropyltrimethoxysilane, triethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 2-aminoethylaminomethyltrimethoxysilane, methyltriacetoxysilane, chloromethyltriethoxysilane, ethyltriacetoxysilane, phenyltrimethoxysilane, 3-allylsulfuryltrimethoxysilane, 2-aminoethylaminomethyltrimethoxysilane, methyltriacetoxysilane, chloromethyltriethoxysilane, ethyltriacetoxysilane, phenyltrimethoxysilane, 3-allylsulfuryltrimethoxysilane, 2-aminoethylaminomethyltrimethoxysilane, methyltriacetoxysilane, methyltrimeth ... trimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-bromopropyltriethoxysilane, 3-allylaminopropyltrimethoxysilane, propyltriethoxysilane, hexyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, bis(ethylmethylketoxime)methoxymethylsilane, amyltriethoxysilane, octyltriethoxysilane, dodecyltriethoxysilane, etc.
[0099] Examples of the compound wherein n is 2 include the following compounds. Specifically, examples include dimethoxymethylsilane, dimethoxydimethylsilane, diethoxysilane, diethoxymethylsilane, dimethoxymethyl-3,3,3-trifluoropropylsilane, 3-chloropropyldimethoxymethylsilane, chloromethyldiethoxysilane, diethoxydimethylsilane, dimethoxy-3-mercaptopropylmethylsilane, diacetoxymethylvinylsilane, diethoxymethylvinylsilane, 3-aminopropyldiethoxymethylsilane, 3-(2-aminoethylaminopropyl)dimethoxymethylsilane, 3-methacryloxypropyldimethoxymethylsilane, Methoxymethylsilane, 3-(3-cyanopropylthiopropyl)dimethoxymethylsilane, 3-(2-acetoxyethylthiopropyl)dimethoxymethylsilane, dimethoxymethyl-2-piperidinoethylsilane, dibutoxydimethylsilane, 3-dimethylaminopropyldiethoxymethylsilane, diethoxymethylphenylsilane, diethoxy-3-glycidoxypropylmethylsilane, 3-(3-acetoxypropylthio)propyldimethoxymethylsilane, dimethoxymethyl-3-piperidinopropylsilane, diethoxymethyloctadecylsilane, and the like.
[0100] Examples of the compound wherein n is 3 include the following compounds: methoxytrimethylsilane, ethoxytrimethylsilane, methoxydimethyl-3,3,3-trifluoropropylsilane, 3-chloropropylmethoxydimethylsilane, methoxy-3-mercaptopropylmethylmethylsilane, and the like.
[0101] The photosensitive layer coating liquid of the present invention may further contain a trace amount of a hydrolyzate of a silane coupling agent, specifically, a compound having a structure represented by the following general formula (2) in an amount of 2% by mass or less.
[0102] Si(OH) m (R1) n (OR2) 4-(n+m) (2)
[0103] (In the formula, Si represents a silicon atom, R1 represents an organic group in which carbon is directly bonded to the silicon atom, R2 represents an organic group, m represents an integer of 1 to 4, n represents an integer of 0 to 3, and m+n is 4 or less.)
[0104] When the inorganic oxide is surface treated with multiple surface treatment agents, the surface treatment can be performed in any order in the surface treatment process. However, for example, when the inorganic oxide is surface treated with multiple silane coupling agents, it is preferred that the silane coupling agent having the structure shown in the above general formula (1) is used first in the surface treatment. In addition, in the surface treatment process, the silicon dioxide can be surface treated with a silane coupling agent and an organosilazane at the same time, or the silicon dioxide can be surface treated with a silane coupling agent first, and then with an organosilazane. In addition, the silicon dioxide can be surface treated with an organosilazane first, then with a silane coupling agent, and then with an organosilazane.
[0105] Here, the wavelength for measuring the transmittance of 20 mass % inorganic oxide slurry (inorganic oxide slurry) can be arbitrarily selected from the range from the visible light region to the laser wavelength region used for exposure in the electrophotographic device, but can be confirmed by the transmittance at a wavelength of 780nm used in the electrophotographic device.
[0106] The solvent used for the slurry of the inorganic oxide can be used as long as the inorganic oxide satisfies the above transmittance, and a solvent for the photosensitive layer coating liquid can be used. Preferred examples include tetrahydrofuran (THF), 1,3-dioxolane, tetrahydropyran, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, toluene, dichloromethane, 1,2-dichloroethane, chlorobenzene, ethylene glycol, ethylene glycol monomethyl ether, 1,2-dimethoxyethane, etc. These solvents can be used alone or in combination, but are not limited to these solvents. It is preferred to use tetrahydrofuran or a mixed solvent containing tetrahydrofuran.
[0107] The inorganic oxide slurry may be obtained by any method as long as the inorganic oxide and the solvent are mixed by stirring to form a slurry. Examples of the disperser used for dispersion during the slurry formation include a paint stirrer, a ball mill, and a sand mill.
[0108] As the lubricating resin, specifically, for example, a polycarbonate resin including a siloxane structure or a polyarylate resin including a siloxane structure is preferably used.
[0109] As the polycarbonate resin containing a siloxane structure, for example, there may be mentioned a polycarbonate resin having a repeating structure represented by the following general formula (3).
[0110]
[0111] In the above general formula (3), R7 to R 10 may be the same or different, and represent a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a fluoroalkyl group having 1 to 10 carbon atoms; h1, h2, h3, and h4 are integers from 0 to 4; V1 represents a divalent aliphatic group or a divalent cyclic aliphatic group; V2 represents a single bond, a linear, branched, or cyclic alkylene group having 1 to 12 carbon atoms, -O-, -S-, -SO-, -SO2-, or -CO-; and U represents a structural unit represented by the following structural formula (4), (5), or (6).
[0112]
[0113]
[0114] In the above structural formulae (4) to (6), n, m1, and m2 are integers of 1 to 400, preferably integers of 8 to 250.
[0115] In the above general formula (3), r3 and r4 satisfy 0.2≤r4 / (r3+r4)≤0.8, and r3, r4, k1, k2, and k3 satisfy 0.001≤k1 / (r3+r4+k1)≤0.005, 0.001≤k2 / (r3+r4+k2)≤0.005, and 0.001≤k3 / (r3+r4+k3)≤0.005. The chain end group is a monovalent aromatic group or a monovalent fluorinated aliphatic group.
[0116] Examples of the polyarylate resin containing a siloxane structure include copolymerized polyarylate resins having a structural unit represented by the following structural formula (7).
[0117] (Structural formula (7))
[0118]
[0119]
[0120] In the above structural formula (7), some structural formulas (A1), (A2), (B1), (B2), (C), (D), (E) and (F) represent structural units constituting the resin. a1, a2, b1, b2, c, d, e and f represent the mol% of each structural unit (A1), (A2), (B1), (B2), (C), (D), (E) and (F), respectively, a1+a2+b1+b2+c+d+e+f is 100 mol%, c+d+e+f is 0.001 to 10 mol%. In addition, W1 and W2 are selected from a single bond, -O-, -S-, -SO-, -CO-, -SO2-, -CR 41 R 42 -(R 41 and R 42 may be the same or different and represent two different types of a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, a halogenated alkyl group, or a substituted or unsubstituted aryl group having 6 to 12 carbon atoms), a substituted or unsubstituted cycloalkylene group having 5 to 12 carbon atoms, a substituted or unsubstituted α,ω alkylene group having 2 to 12 carbon atoms, a -9,9-fluorenyl group, a substituted or unsubstituted arylene group having 6 to 12 carbon atoms, and an aryl group having 6 to 12 carbon atoms or a divalent group containing an arylene group. R 11 ~R 30 R may be the same or different and represent a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, a fluorine atom, a chlorine atom, or a bromine atom. 31 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group which may have a substituent, or a cycloalkyl group which may have a substituent, a fluorine atom, a chlorine atom, or a bromine atom. m3 and m4 represent an integer of 1 or more.
[0121] In the copolymerized polyarylate resin, when the total amount of the structural units represented by the structural formula (7) (a1+a2+b1+b2+c+d+e+f) is 100 mol%, the amount of the siloxane component (c+d+e+f) is 0.001 to 10 mol%, preferably 0.03 to 10 mol%. When (c+d+e+f) is less than 0.001 mol%, a sufficient friction coefficient that can be sustained may not be obtained. On the other hand, when (c+d+e+f) is greater than 10 mol%, sufficient film hardness cannot be obtained, and in addition, when it is made into a coating liquid, sufficient compatibility with a solvent or a functional material may not be obtained.
[0122] In the structural formula (7), m3 and m4 are integers of 1 to 400, preferably 8 to 250.
[0123] In addition, in order to obtain the desired effect of the present invention, in the above structural formula (7), W2 is preferably a single bond, -O- or -CR 41 R 42 -(R 41and R 42 may be the same or different, and represent a hydrogen atom, a methyl group or an ethyl group), and W1 is preferably -CR 41 R 42 -(R 41 and R 42 may be the same or different and represent a hydrogen atom, a methyl group or an ethyl group).
[0124] In addition, as the siloxane structure in the above structural formula (7), for example, the constituent monomers include the following molecular formula (8) (reactive silicone resin Silaplane FM4411 (weight average molecular weight 1000), FM4421 (weight average molecular weight 5000), FM4425 (weight average molecular weight 15000) manufactured by Chisso Corporation), the following molecular formula (9) (reactive silicone resin Silaplane FMDA11 (weight average molecular weight 1000), FMDA21 (weight average molecular weight 5000), FMDA26 (weight average molecular weight 15000) manufactured by Chisso Corporation), etc.
[0125] Molecular formula (8)
[0126]
[0127] Molecular formula (9)
[0128]
[0129] In the formula, R 31 It represents n-butyl.
[0130] Specific examples of the structural units of the polyarylate resin represented by the chemical structural formula 7, namely, structural formulas (A1), (A2), (B1), (B2), (C), (D), (E), and (F) are shown below. In addition, specific examples of copolymerized polyarylate resins having structural formulas (A1), (A2), (B1), (B2), (C), (D), (E), and (F) are shown in Table 1 below. However, the copolymerized polyarylate resins that can be used are not limited to the resins of these exemplified structures.
[0131] Specific example of structural formula (A1)
[0132]
[0133] Specific example of structural formula (A2)
[0134]
[0135] Specific example of structural formula (B1)
[0136]
[0137] Specific example of structural formula (B2)
[0138]
[0139] Specific example of structural formula (C)
[0140]
[0141] Specific example of structural formula (D)
[0142]
[0143] Specific example of structural formula (E)
[0144]
[0145] Specific example of structural formula (F)
[0146]
[0147] In the formula, R 31 It represents n-butyl.
[0148] [Table 1]
[0149]
[0150] The copolymerized polyarylate resin may have other structural units. When the copolymerized polyarylate resin as a whole is taken as 100 mol %, the blending ratio of the structural unit represented by the structural formula (7) is preferably 10 to 100 mol %, more preferably 50 to 100 mol %.
[0151] The polyarylate resin may be synthesized only by interfacial polymerization, but is more preferably synthesized by reacting a siloxane component by solution polymerization and then performing interfacial polymerization.
[0152] The mass average molecular weight of the polycarbonate resin and the polyarylate resin is preferably 5,000 to 250,000, more preferably 10,000 to 150,000.
[0153] The photoreceptor of the present invention may have any layer structure if it satisfies the conditions related to the above-mentioned inorganic oxide and lubricating resin. The photoreceptor of the present invention is classified into a negatively charged laminated photoreceptor, a positively charged single-layer photoreceptor, and a positively charged laminated photoreceptor according to the composition of the photosensitive layer. The negatively charged laminated photoreceptor comprises a photosensitive layer 6, which sequentially comprises a charge generating layer containing a charge generating material, and a charge transport layer containing a charge transport material and a resin binder containing at least a lubricating resin. The positively charged single-layer photoreceptor comprises a photosensitive layer 3, which comprises a charge transport material, a resin binder containing at least a lubricating resin, and a charge generating material. The positively charged laminated photoreceptor comprises a photosensitive layer 7, which sequentially comprises a charge transport layer containing a charge transport material, and a charge generating layer containing a charge transport material, a resin binder containing at least a lubricating resin, and a charge generating material.
[0154] The conductive substrate 1 has a function as an electrode of the photoreceptor and is also a support for each layer constituting the photoreceptor, and may be in any shape of a cylinder, a plate, a film, etc. As the material of the conductive substrate 1, metals such as aluminum, stainless steel, and nickel, or materials subjected to a conductive treatment on the surface of glass, resin, etc. may be used.
[0155] The base layer 2 is a layer with resin as the main component or a layer composed of metal oxide films such as acid-proof aluminum. The base layer 2 is provided as required for the purpose of controlling the injection of charge from the conductive substrate 1 to the photosensitive layer, or covering the surface defects of the conductive substrate 1, improving the adhesion between the photosensitive layer and the conductive substrate 1, etc. As the resin material used for the base layer 2, insulating polymers such as casein, polyvinyl alcohol, polyamide, melamine, cellulose, and conductive polymers such as polythiophene, polypyrrole, and polyaniline can be cited. These resins can be used alone or in combination. In addition, these resins can also be used by containing metal oxides such as titanium dioxide and zinc oxide.
[0156] (Negatively charged laminated photoreceptor)
[0157] In the negatively charged laminated photoreceptor, the photosensitive layer has a charge generating layer 4 and a charge transporting layer 5, and the charge transporting layer 5 is the outermost layer.
[0158] In the negatively charged laminated photoreceptor, the charge generating layer 4 is formed by applying a coating liquid in which particles of a charge generating material are dispersed in a resin binder, etc., and the charge generating layer 4 generates charges by receiving light. The charge generating layer 4 is important in that its charge generating efficiency is high and the generated charges are injected into the charge transport layer 5. It is desirable that its electric field dependence is small and that the injection is good even at a low electric field.
[0159] As the charge generating material, phthalocyanine compounds such as X-type metal-free phthalocyanine, τ-type metal-free phthalocyanine, α-type oxytitanium phthalocyanine, β-type oxytitanium phthalocyanine, Y-type oxytitanium phthalocyanine, γ-type oxytitanium phthalocyanine, amorphous oxytitanium phthalocyanine, and ε-type copper phthalocyanine, various azo pigments, anthraquinone pigments, thiopyrylium pigments, perylene pigments, perynone pigments, squarylium pigments, and quinacridone pigments can be used alone or in appropriate combination. Appropriate materials can be selected according to the light wavelength region of the exposure light source used for image formation. The charge generating layer 4 can also be used by using the charge generating material as the main body and adding a charge transport material thereto.
[0160] As the resin binder of the charge generating layer 4, polymers and copolymers of polycarbonate resin, polyester resin, polyamide resin, polyurethane resin, vinyl chloride resin, vinyl acetate resin, phenoxy resin, polyvinyl acetal resin, polyvinyl butyral resin, polystyrene resin, polysulfone resin, diallyl phthalate resin, and methacrylate resin can be used in appropriate combination.
[0161] The content of the charge generating material in the charge generating layer 4 is preferably 20 to 80% by mass, more preferably 30 to 70% by mass, relative to the solid content in the charge generating layer 4. In addition, the content of the resin binder in the charge generating layer 4 is preferably 20 to 80% by mass, more preferably 30 to 70% by mass, relative to the solid content in the charge generating layer 4. The charge generating layer 4 only needs to have a charge generating function, so its thickness depends on the light absorption coefficient of the charge generating material, and is generally 1 μm or less, preferably 0.5 μm or less.
[0162] In the case of a negatively charged laminated photoreceptor, the charge transport layer 5 is the above-mentioned photosensitive layer containing an inorganic oxide and a lubricating resin. In the negatively charged laminated photoreceptor, the charge transport layer 5 is mainly composed of the above-mentioned inorganic oxide, a charge transport material, and a resin binder containing at least a lubricating resin. Thereby, the desired effect of the present invention can be obtained.
[0163] As the resin binder of the charge transport layer 5, it is preferred to use other resins in addition to the above-mentioned lubricating resin. In particular, when the blending amount of the lubricating resin is recorded as A (parts by mass) and the blending amount of the other resin is recorded as B (parts by mass), it is preferred that the ratio A / (B+A) of the lubricating resin in the total amount of the resin binder satisfies 0.1≤A / (B+A)≤0.5, and more preferably satisfies 0.2≤A / (B+A)≤0.4. If the ratio A / (B+A) of the lubricating resin is less than 0.1, film formation is likely to occur, and if it exceeds 0.5, the printing resistance tends to deteriorate.
[0164] As such other resins, other polyarylate resins or polycarbonate resins can be used, for example, various polycarbonate resins such as bisphenol A type, bisphenol Z type, bisphenol A type-biphenyl copolymer, bisphenol Z type-biphenyl copolymer, polyphenylene resin, polyester resin, polyvinyl acetal resin, polyvinyl butyral resin, polyvinyl alcohol resin, vinyl chloride resin, vinyl acetate resin, polyethylene resin, polypropylene resin, acrylic resin, polyurethane resin, epoxy resin, melamine resin, silicone resin, polyamide resin, polystyrene resin, polyacetal resin, polysulfone resin, polymers of methacrylate and their copolymers, etc. In addition, the same resins with different molecular weights can also be used in combination. In particular, as other resins, copolymerized polycarbonate resins having a repeating structure shown in the following general formula (10) can be preferably used.
[0165]
[0166] In the above general formula (10), R3~R6 are the same or different, representing a hydrogen atom, an alkyl group with 1 to 10 carbon atoms or a fluorinated alkyl group with 1 to 10 carbon atoms, g1, g2, g3, g4 are integers from 0 to 4, r1 and r2 satisfy 0.3≤r2 / (r1+r2)≤0.7, and the chain end group is a monovalent aromatic group or a monovalent fluorinated aliphatic group.
[0167] As the charge transport material of the charge transport layer 5, various hydrazone compounds, styryl compounds, diamine compounds, butadiene compounds, indole compounds, etc. can be used alone or in combination. Examples of the charge transport material include compounds shown in (II-1) to (II-14) below, but are not limited thereto.
[0168]
[0169]
[0170] The content of the inorganic oxide in the charge transport layer 5 is preferably 1 to 40% by mass, more preferably 2 to 30% by mass, relative to the solid content of the charge transport layer 5. The content of the resin binder in the charge transport layer 5 is preferably 10 to 90% by mass, more preferably 20 to 80% by mass, relative to the solid content of the charge transport layer 5 excluding the inorganic oxide. The content of the charge transport material in the charge transport layer 5 is preferably 10 to 90% by mass, more preferably 20 to 80% by mass, relative to the solid content of the charge transport layer 5 excluding the inorganic oxide.
[0171] The film thickness of the charge transport layer 5 is preferably in the range of 3 to 50 μm, more preferably in the range of 15 to 40 μm, in order to maintain a practically effective surface potential.
[0172] The solvent used for slurrying the above-mentioned inorganic oxide is not particularly limited, as long as the above-mentioned inorganic oxide satisfies the above-mentioned transmittance, and a solvent for the photosensitive layer coating liquid can be used. Preferred examples include tetrahydrofuran (THF), 1,3-dioxolane, tetrahydropyran, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, toluene, dichloromethane, 1,2-dichloroethane, chlorobenzene, ethylene glycol, ethylene glycol monomethyl ether, 1,2-dimethoxyethane, etc. These solvents can be used alone or in combination, but are not limited to these solvents. It is preferred to use tetrahydrofuran or a mixed solvent containing tetrahydrofuran.
[0173] (Single-layer photoreceptor)
[0174] In the case of a single-layer photoreceptor, the photosensitive layer 3 is the outermost surface layer, and is the photosensitive layer containing the inorganic oxide and the lubricating resin. The single-layer photosensitive layer 3 is mainly composed of the inorganic oxide, the charge generating material, the hole transport material, the electron transport material (acceptor compound), and the resin binder containing at least the lubricating resin. Thereby, the desired effect of the present invention can be obtained.
[0175] As the charge generating material, for example, phthalocyanine pigments, azo pigments, anthraquinone pigments, perylene pigments, cyclic ketone pigments, polycyclic quinone pigments, squarylium pigments, thiopyranium pigments, quinacridone pigments, etc. can be used. In addition, these charge generating materials can be used alone or in combination of two or more. In particular, as azo pigments, disazo pigments and trisazo pigments are preferred, as perylene pigments, N, N'-di (3, 5-dimethylphenyl) -3, 4: 9, 10-perylene - di (carboximide) is preferred, and as phthalocyanine pigments, metal-free phthalocyanine, copper phthalocyanine, and oxytitanium phthalocyanine are preferred. In addition, when using X-type metal-free phthalocyanine, τ-type metal-free phthalocyanine, ε-type copper phthalocyanine, α-type oxytitanium phthalocyanine, β-type oxytitanium phthalocyanine, Y-type oxytitanium phthalocyanine, amorphous oxytitanium phthalocyanine, oxytitanium phthalocyanine with a Bragg angle 2θ of 9.6° as the maximum peak in the CuKα:X-ray diffraction pattern described in Japanese Patent Laid-Open No. 8-209023, U.S. Patent No. 5736282 and U.S. Patent No. 5874570, significant improvements are shown in sensitivity, durability and image quality.
[0176] As the hole transport material, for example, hydrazone compounds, pyrazoline compounds, pyrazolone compounds, Oxadiazole compounds, The hole transport material may be a 3-D-type hole transport material, such as a 3-D-type hole transport material, ...
[0177] As the electron transport material (acceptor compound), succinic anhydride, maleic anhydride, dibromosuccinic anhydride, phthalic anhydride, 3-nitrophthalic anhydride, 4-nitrophthalic anhydride, pyromellitic anhydride, pyromellitic acid, trimellitic acid, trimellitic anhydride, phthalimide, 4-nitrophthalimide, tetracyanoethylene, tetracyanoquinodimethane, chloranil, tetrabromobenzoquinone, o-nitrobenzoic acid, malononitrile, trinitrofluorenone, trinitrothioxanthone, dinitrobenzene, dinitroanthracene, dinitroacridine, nitroanthraquinone, dinitroanthraquinone, thiopyran compounds, quinone compounds, benzoquinone compounds, diphenoquinone compounds, naphthoquinone compounds, anthraquinone compounds, stilbenequinone compounds, azoquinone compounds, etc. can be mentioned. In addition, these electron transport materials can be used alone or in combination of two or more.
[0178] As the resin binder of the single-layer photosensitive layer 3, the above-mentioned lubricating resin and other resins are preferably used, similarly to the resin binder used in the charge transport layer 5 in the case of the negatively charged laminated photoreceptor. The preferred conditions for the ratio of the lubricating resin in this case can also be set to be the same as those for the charge transport layer 5 in the case of the negatively charged laminated photoreceptor. That is, in the single-layer photosensitive layer 3, when the blending amount of the lubricating resin is recorded as A (parts by mass) and the blending amount of other resins is recorded as B (parts by mass), it is preferred that the ratio A / (B+A) of the lubricating resin in the total amount of the resin binder satisfies 0.1≤A / (B+A)≤0.5, and more preferably satisfies 0.2≤A / (B+A)≤0.4.
[0179] As such other resins, other polyarylate resins or polycarbonate resins can be used, for example, various polycarbonate resins such as bisphenol A type, bisphenol Z type, bisphenol A type-biphenyl copolymer, bisphenol Z type-biphenyl copolymer, polyphenylene resin, polyester resin, polyvinyl acetal resin, polyvinyl butyral resin, polyvinyl alcohol resin, vinyl chloride resin, vinyl acetate resin, polyethylene resin, polypropylene resin, acrylic resin, polyurethane resin, epoxy resin, melamine resin, silicone resin, polyamide resin, polystyrene resin, polyacetal resin, other polyarylate resins, polysulfone resin, polymers of methacrylate and their copolymers, etc. In addition, the same resins with different molecular weights can also be used in combination. In particular, as other resins, copolymerized polycarbonate resins having a repeating structure shown in the above-mentioned general formula (10) can be preferably used.
[0180] The content of the inorganic oxide in the single-layer photosensitive layer 3 is preferably 1 to 40% by mass, more preferably 2 to 30% by mass, relative to the solid content of the single-layer photosensitive layer 3. The content of the charge generating material in the single-layer photosensitive layer 3 is preferably 0.1 to 20% by mass, more preferably 0.5 to 10% by mass, relative to the solid content of the single-layer photosensitive layer 3 excluding the inorganic oxide. The content of the positive hole transport material in the single-layer photosensitive layer 3 is preferably 3 to 80% by mass, more preferably 5 to 60% by mass, relative to the solid content of the single-layer photosensitive layer 3 excluding the inorganic oxide. The content of the electron transport material in the single-layer photosensitive layer 3 is preferably 1 to 50% by mass, more preferably 5 to 40% by mass, relative to the solid content of the single-layer photosensitive layer 3 excluding the inorganic oxide. The content of the resin binder in the single-layer photosensitive layer 3 is preferably 10 to 90% by mass, more preferably 20 to 80% by mass, relative to the solid content of the single-layer photosensitive layer 3 excluding the inorganic oxide.
[0181] The film thickness of the single-layer photosensitive layer 3 is preferably in the range of 3 to 100 μm, more preferably in the range of 5 to 40 μm, in order to maintain a practically effective surface potential.
[0182] (Positively charged laminated photoreceptor)
[0183] In the positively charged laminated photoreceptor, the photosensitive layer has a charge transport layer 5 and a charge generation layer 4, and the charge generation layer 4 is the outermost layer.
[0184] In the positively charged laminated photoreceptor, the charge transport layer 5 is mainly composed of a charge transport material and a resin binder. As the charge transport material used for the charge transport layer 5 in the positively charged laminated photoreceptor, the same materials as those exemplified in the embodiment of the charge transport layer 5 in the negatively charged laminated photoreceptor can be used. The content of each material and the film thickness of the charge transport layer 5 can also be the same as those of the negatively charged laminated photoreceptor. As the resin binder of the charge transport layer 5, in addition to the other resins exemplified in the embodiment of the charge transport layer 5 in the negatively charged laminated photoreceptor, a lubricating resin can also be used.
[0185] In the case of a positively charged laminated photoreceptor, the charge generating layer 4 is the above-mentioned photosensitive layer containing an inorganic oxide and a lubricating resin. In the positively charged laminated photoreceptor, the charge generating layer 4 is mainly composed of the above-mentioned inorganic oxide, a charge generating material, a hole transport material, an electron transport material (acceptor compound), and a resin binder containing at least a lubricating resin. Thereby, the desired effect of the present invention can be obtained.
[0186] As the charge generating material, hole transport material, and electron transport material used in the charge generating layer 4 in the positively charged laminated photoreceptor, the same materials as those exemplified as the embodiments of the single-layer photosensitive layer 3 in the single-layer photoreceptor can be used. The content of each material and the film thickness of the charge generating layer 4 can also be the same as those of the single-layer photosensitive layer 3 in the single-layer photoreceptor. In the positively charged laminated photoreceptor, as the resin binder of the charge generating layer 4, the lubricating resin and other resins are preferably used, similarly to the resin binder used for the single-layer photosensitive layer 3 in the single-layer photoreceptor. The preferred conditions for the ratio of the lubricating resin in this case and the specific examples of the other resins can be the same as those of the single-layer photosensitive layer 3 in the single-layer photoreceptor. That is, in the charge generating layer 4, when the blending amount of the lubricating resin is denoted as A (parts by mass) and the blending amount of other resins is denoted as B (parts by mass), the ratio A / (B+A) of the lubricating resin in the total amount of the resin binder preferably satisfies 0.1≤A / (B+A)≤0.5, and more preferably satisfies 0.2≤A / (B+A)≤0.4.
[0187] In any of the above-mentioned laminated or single-layer photosensitive layers, an antioxidant, a light stabilizer or other deterioration inhibitor may be contained for the purpose of improving environmental resistance and stability to harmful light. Examples of compounds used for this purpose include chromanol derivatives such as vitamin E and esterified compounds, polyarylalkyl compounds, hydroquinone derivatives, etherified compounds, dietherified compounds, benzophenone derivatives, benzotriazole derivatives, thioether compounds, phenylenediamine derivatives, phosphates, phosphites, phenol compounds, hindered phenol compounds, linear amine compounds, cyclic amine compounds, hindered amine compounds, and the like.
[0188] In addition, in order to improve the flatness of the formed film and impart lubricity, the photosensitive layer may contain a leveling agent such as silicone oil or fluorine oil. In order to adjust the film hardness, reduce the friction coefficient, impart lubricity, etc., the photosensitive layer may contain metal oxides such as silica, titanium oxide, zinc oxide, calcium oxide, aluminum oxide, zirconium oxide, metal sulfates such as barium sulfate and calcium sulfate, microparticles of metal nitrides such as silicon nitride and aluminum nitride, or fluorine resin particles such as tetrafluoroethylene resin, fluorine-based comb-shaped graft polymer resins, etc. In addition, other known additives may be contained as needed within a range that does not significantly damage the electronic photographic properties.
[0189] (Method for producing photoreceptor)
[0190] The manufacturing method according to an embodiment of the present invention comprises the following steps when manufacturing a photosensitive body by forming the photosensitive layer containing the inorganic oxide and the lubricating resin using a photosensitive layer coating liquid. Figure 2As shown, first, the inorganic oxide slurry is dispersed once in the solvent for the photosensitive layer coating liquid to obtain the inorganic oxide slurry (inorganic oxide slurry preparation step (S1)). Next, the charge transport material and the lubricating resin are dissolved in the solvent for the photosensitive layer coating liquid to obtain the photosensitive layer forming liquid (photosensitive layer forming liquid preparation step (S2)). Then, the obtained inorganic oxide slurry and the photosensitive layer forming liquid are mixed to obtain the photosensitive layer coating liquid (photosensitive layer coating liquid preparation step (S3)). In this way, a photoreceptor that has little wear and tear during long-term use, does not form a film, and can achieve stable images can be reliably manufactured.
[0191] Here, as the photosensitive layer forming liquid, at least a charge transport material and a lubricating resin are included. For example, when the photosensitive layer including the inorganic oxide and the lubricating resin is a negatively charged laminated type photosensitive layer, the photosensitive layer forming liquid can be prepared by dissolving the charge transport material and the resin binder including at least the lubricating resin in a solvent for the photosensitive layer coating liquid. In addition, when the photosensitive layer including the inorganic oxide and the lubricating resin is a single-layer type photosensitive layer and a positively charged laminated type photosensitive layer, the photosensitive layer forming liquid can be prepared by dissolving the hole transport material, the electron transport material and the resin binder including at least the lubricating resin in a solvent for the photosensitive layer coating liquid, and then dispersing (secondary dispersion) the charge generating material therein.
[0192] The solvent for the photosensitive layer coating solution preferably includes tetrahydrofuran (THF), 1,3-dioxolane, tetrahydropyran, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, toluene, dichloromethane, 1,2-dichloroethane, chlorobenzene, ethylene glycol, ethylene glycol monomethyl ether, 1,2-dimethoxyethane, etc. These solvents can be used alone or in combination. It is preferred to use tetrahydrofuran or a mixed solvent containing tetrahydrofuran. The solvent for the photosensitive layer coating solution can be the same as the solvent used in the slurry of the inorganic oxide.
[0193] When the inorganic oxide slurry and other constituent components of the photosensitive layer are mixed, dissolution and dispersion may be performed in any order. For example, after the photosensitive layer forming liquid is prepared, the liquid may be added to the inorganic oxide slurry.
[0194] The inorganic oxide slurry can be prepared by using the above-mentioned disperser according to a conventional method without particular limitation. The photosensitive layer forming liquid and the photosensitive layer coating liquid can also be prepared by conventional methods without particular limitation.
[0195] (Electronic Photographic Device)
[0196] The electronic photographic device of the embodiment of the present invention is formed by carrying the above-mentioned electronic photographic photosensitive body, and the desired effect can be obtained by applying it to various mechanical processing processes. Specifically, in charging processes such as contact charging methods using charging components such as rollers and brushes, non-contact charging methods using corotrons, grid electrode wires (scorotrons), etc., and contact development and non-contact development methods using non-magnetic single-component, magnetic single-component, two-component, etc. development methods, sufficient effects can be obtained. In particular, in the case of a charging process having a contact charging method in which the charging component is charged by contact with the photosensitive body, the present invention is useful in suppressing the wear caused by the contact of the charging component.
[0197] Figure 3 A simplified structural diagram showing an example of a structure of an electronic photographic device according to an embodiment of the present invention. The illustrated electronic photographic device 60 is equipped with a photoreceptor 8 according to an embodiment of the present invention, and the photoreceptor 8 includes a conductive substrate 1, a base layer 2 covering the outer peripheral surface of the conductive substrate 1, and a photosensitive layer 300. The electronic photographic device 60 is composed of a charging member 21 arranged at the outer peripheral edge of the photoreceptor 8, a high-voltage power supply 22 for supplying an applied voltage to the charging member 21, an image exposure member 23, a developer 24 having a developing roller 241, a paper feed member 25 having a paper feed roller 251 and a paper feed guide 252, and a transfer charger (direct charging type) 26. The electronic photographic device 60 may also include a cleaning device 27 having a cleaning blade 271, and a charge removing member 28. In addition, the electronic photographic device 60 may be a color printer.
[0198] Example
[0199] Hereinafter, specific embodiments of the present invention will be described in detail using examples. The present invention is not limited to the following examples within the scope of the inventive concept.
[0200] (Preparation of Inorganic Oxide Slurry)
[0201] (Production Examples 1 to 20)
[0202] Inorganic oxide slurries were prepared according to the manufacturing examples shown in Table 2 below. Specifically, silica (YA010C (aluminum content 500ppm), YA050C (aluminum content 900ppm), YA100C (aluminum content 900ppm), YA180C (aluminum content 900ppm), YA400C (aluminum content 900ppm)) manufactured by Yaduma Technologies was used as an inorganic oxide, and the treatment agent described in Table 2 was used as a surface treatment agent to prepare surface-treated silica, which was then dispersed (primary dispersion) in tetrahydrofuran (THF) for a photosensitive layer coating solution to obtain each inorganic oxide slurry. For the inorganic oxide after the surface treatment of Manufacturing Example 1, the amount of the surface treatment agent was quantified, and the result was 0.8% by mass relative to the inorganic oxide after the treatment.
[0203] [Table 2]
[0204]
[0205] *1) Silica A: Made by Yaduma Technology Co., Ltd., YA010C, primary particle size 10 nm
[0206] *2) Silica B: Made by Yaduma Technology Co., Ltd., YA050C, primary particle size 50 nm
[0207] *3) Silica C: Made by Yaduma Technology Co., Ltd., YA100C, primary particle size 100 nm
[0208] *4) Silica D: Made by Yaduma Technology Co., Ltd., YA180C, primary particle size 180nm
[0209] *5) Silica E: Made by Yaduma Technology Co., Ltd., YA400C, primary particle size 400 nm
[0210] *6) KBM573: Made by Shin-Etsu Chemical Co., Ltd., N-phenyl-3-aminopropyltrimethoxysilane
[0211] *7)KBM903: Made by Shin-Etsu Chemical Co., Ltd.
[0212] (Manufacturing of Negatively Charged Laminated Photoreceptor)
[0213] (Example 1)
[0214] 5 parts by mass of alcohol-soluble nylon (manufactured by Toray Industries, Ltd., trade name "CM8000") and 5 parts by mass of aminosilane-treated titanium oxide fine particles were dissolved and dispersed in 90 parts by mass of methanol to prepare a coating liquid 1. The coating liquid 1 was dip-coated on the outer circumference of an aluminum cylinder having an outer diameter of 30 mm as a conductive substrate, and dried at a temperature of 100° C. for 30 minutes to form a base layer with a film thickness of 3 μm.
[0215] 1 part by mass of Y-type oxytitanium phthalocyanine as a charge generating material and 1.5 parts by mass of polyvinyl butyral resin (manufactured by Sekisui Chemical Co., Ltd., trade name "S-LEC BM-2") as a resin binder were dissolved and dispersed in 60 parts by mass of dichloromethane to prepare a coating liquid 2. The coating liquid 2 was dip-coated on the above-mentioned base layer. The coating liquid was dried at a temperature of 80°C for 30 minutes to form a charge generating layer with a film thickness of 0.3 μm.
[0216] 9 parts by mass of the compound represented by the following structural formula as a charge transport material (CTM),
[0217]
[0218] 8 parts by mass of a polycarbonate resin having a repeating unit represented by the following structural formula as a resin binder 1, and
[0219]
[0220] 3 parts by mass of a polycarbonate resin having a repeating unit represented by the following structural formula as a resin binder 2,
[0221]
[0222] Dissolved in 80 parts by mass of THF. This liquid was added to 25 parts by mass of the inorganic oxide slurry prepared in Production Example 1 to prepare a coating liquid 3. This coating liquid 3 was dip-coated on the charge generating layer and dried at 120°C for 60 minutes to form a charge transport layer with a film thickness of 20 μm, thereby preparing a negatively charged laminated photoreceptor.
[0223] (Example 2)
[0224] A photoreceptor was prepared in the same manner as in Example 1 except that the resin binder 2 used in Example 1 was changed to a polycarbonate resin having a repeating unit represented by the following structural formula as the resin binder 3.
[0225]
[0226] (Example 3)
[0227] A photoreceptor was prepared in the same manner as in Example 1 except that the resin binder 2 used in Example 1 was replaced with a polyarylate resin having a repeating unit represented by the following structural formula as the resin binder 4.
[0228]
[0229] (Example 4)
[0230] A photoreceptor was prepared in the same manner as in Example 1 except that the resin binder 2 used in Example 1 was replaced with a polycarbonate resin having a repeating unit represented by the following structural formula as the resin binder 5 .
[0231]
[0232] (Examples 5 to 23)
[0233] A photoreceptor was prepared in the same manner as in Example 1 except that the type of the inorganic oxide slurry of Production Example 1 used in Example 1 was changed as described in Table 3 below.
[0234] (Comparative Example 1)
[0235] A photoreceptor was prepared in the same manner as in Example 1 except that the resin used in the coating liquid 3 in Example 1 was changed to only the resin binder 1 and the added amount was changed to 11 parts by mass.
[0236] (Example 24)
[0237] A photoreceptor was prepared in the same manner as in Example 1 except that the resin used in the coating liquid 3 in Example 1 was changed to 10 parts by mass of the resin binder 1 and 1 part by mass of the resin binder 2.
[0238] (Example 25)
[0239] A photoreceptor was prepared in the same manner as in Example 1 except that the resin used in the coating liquid 3 in Example 1 was changed to 10 parts by mass of the resin binder 1 and 1 part by mass of the resin binder 3.
[0240] (Example 26)
[0241] A photoreceptor was prepared in the same manner as in Example 1 except that the resin used in the coating liquid 3 in Example 1 was changed to 10 parts by mass of the resin binder 1 and 1 part by mass of the resin binder 4.
[0242] (Comparative Example 2)
[0243] A photoreceptor was prepared in the same manner as in Example 1 except that the resin used in the coating liquid 3 in Example 1 was changed to 5 parts by mass of the resin binder 1 and 6 parts by mass of the resin binder 2.
[0244] (Comparative Example 3)
[0245] A photoreceptor was prepared in the same manner as in Example 1 except that the resin used in the coating liquid 3 in Example 1 was changed to 11 parts by mass of a polycarbonate resin having a repeating unit represented by the following structural formula as the resin binder 6 .
[0246]
[0247] (Comparative Example 4)
[0248] A photoreceptor was prepared in the same manner as in Example 1 except that the inorganic oxide slurry of Preparation Example 1 used for coating liquid 3 in Example 1 was changed to the inorganic oxide slurry of Preparation Example 5, the resin used was changed to only polycarbonate resin binder 1, and the addition amount was changed to 11 parts by mass.
[0249] (Comparative Example 5)
[0250] A photoreceptor was prepared in the same manner as in Example 1 except that the inorganic oxide slurry of Preparation Example 1 used for coating liquid 3 in Example 1 was changed to the inorganic oxide slurry of Preparation Example 9, the resin used was changed to only polycarbonate resin binder 1, and the addition amount was changed to 11 parts by mass.
[0251] (Comparative Example 6)
[0252] A photoreceptor was prepared in the same manner as in Example 1 except that the inorganic oxide slurry of Preparation Example 1 used for coating liquid 3 in Example 1 was replaced by the inorganic oxide slurry of Preparation Example 13, the resin used was changed to only polycarbonate resin binder 1, and the addition amount was changed to 11 parts by mass.
[0253] (Manufacturing of Positively Charged Single-layer Photoreceptor)
[0254] (Example 27)
[0255] 0.2 parts by mass of vinyl chloride-vinyl acetate-vinyl alcohol copolymer (manufactured by Nissin Chemical Industry Co., Ltd., trade name "SOLBIN TA5R") was stirred and dissolved in 99 parts by mass of methyl ethyl ketone to prepare coating liquid 4. The coating liquid 4 was dip-coated on the outer circumference of an aluminum cylinder having an outer diameter of 24 mm as a conductive substrate, and dried at a temperature of 100°C for 30 minutes to form a base layer with a film thickness of 0.1 μm.
[0256] 0.1 parts by weight of X-type metal-free phthalocyanine as a charge generating material, 8 parts by weight of the charge transport material (CTM) used in Example 1 as a hole transport material, 4 parts by weight of a compound having a structure represented by the following structural formula as an electron transport material (ETM),
[0257]
[0258] 6 parts by mass of the polycarbonate resin used as the resin binder 1 in the charge transport layer of Example 1 and 2 parts by mass of the polycarbonate resin used as the resin binder 2 in the charge transport layer of Example 1 were dissolved and dispersed in 80 parts by mass of THF. This liquid was added to 25 parts by mass of the inorganic oxide slurry prepared in Production Example 1 to prepare a coating liquid 5.
[0259] The coating liquid 5 was dip-coated on the base layer and dried at 100° C. for 60 minutes to form a photosensitive layer with a film thickness of 25 μm, thereby producing a single-layer photoreceptor.
[0260] (Example 28)
[0261] A photoreceptor was prepared by the same method as in Example 27, except that the inorganic oxide slurry used in Example 27 was changed to the inorganic oxide slurry of Production Example 10.
[0262] (Comparative Example 7)
[0263] A photoreceptor was prepared in the same manner as in Example 27 except that the resin used in Example 27 was changed to only the resin binder 1 and the amount thereof added was changed to 8 parts by mass.
[0264] (Comparative Example 8)
[0265] A photoreceptor was prepared in the same manner as in Example 27 except that the resin used in Example 27 was changed to only the resin binder 1 and the amount thereof added was changed to 8 parts by mass, and the inorganic oxide slurry used was changed to the inorganic oxide slurry of Production Example 10.
[0266] (Manufacturing of Positively Charged Laminated Photoreceptor)
[0267] (Example 29)
[0268] 5 parts by mass of the polycarbonate resin used as the resin binder 1 in Example 27 and 5 parts by mass of the charge transport material used in Example 1 were dissolved in 80 parts by mass of THF to prepare a coating liquid 6. The coating liquid 6 was dip-coated on the outer circumference of an aluminum cylinder having an outer diameter of 24 mm as a conductive substrate, and dried at a temperature of 120° C. for 60 minutes to form a charge transport layer having a film thickness of 15 μm.
[0269] 0.1 parts by mass of Y-type oxytitanium phthalocyanine as a charge generating material, 2 parts by mass of the charge transport material (CTM) used in Example 1 as a hole transport material, 5 parts by mass of the compound used in Example 27 as an electron transport material (ETM), 10 parts by mass of the polycarbonate resin used in Example 1 as a resin binder 1, and 3 parts by mass of the polycarbonate resin used in Example 1 as a resin binder 2 were dissolved and dispersed in 120 parts by mass of 1,2-dichloroethane. This liquid was added to 25 parts by mass of the inorganic oxide slurry prepared in Production Example 1 to prepare a coating liquid 7. This coating liquid 7 was dip-coated on the charge transport layer and dried at a temperature of 100°C for 60 minutes to form a charge generating layer with a film thickness of 15 μm, thereby preparing a positively charged laminated photoreceptor.
[0270] (Example 30)
[0271] A photoreceptor was prepared by the same method as in Example 29, except that the inorganic oxide slurry used in Example 29 was changed to the inorganic oxide slurry of Production Example 10.
[0272] (Comparative Example 9)
[0273] A photoreceptor was prepared in the same manner as in Example 29, except that the resin used in Example 29 was changed to only the resin binder 1 and the amount thereof added was changed to 13 parts by mass.
[0274] (Comparative Example 10)
[0275] A photoreceptor was prepared in the same manner as in Example 29 except that the resin used in Example 29 was changed to only the resin binder 1 and the amount thereof added was changed to 13 parts by mass, and the inorganic oxide slurry used was changed to the inorganic oxide slurry of Production Example 10.
[0276] (Transmittance of Inorganic Oxide Slurry)
[0277] For the inorganic oxide slurry of each manufacturing example, the inorganic oxide was once dispersed at 20% by mass relative to THF, thereby preparing the slurry for evaluation. These samples are referred to as 20% by mass inorganic oxide slurry. The slurry for evaluation was added to a quartz cuvette with an optical path length of 10 mm, and the transmittance of light when irradiated with light of a wavelength of 780 nm was measured using a spectrophotometer (UV-3100 made by Shimadzu Corporation). The transmittance of these lights is also referred to as slurry transmittance. The measurement results are shown in Table 3 below.
[0278] (Viscosity of Inorganic Oxide Slurry)
[0279] For the inorganic oxide slurry of each manufacturing example, the inorganic oxide was dispersed in THF at 20 mass %, thereby preparing a 20 mass % inorganic oxide slurry for evaluation. The viscosity of these 20 mass % inorganic oxide slurries at 20° C. was measured using a vibration viscometer (VISCOMATEV-10A manufactured by SEKONIC). These viscosities are also referred to as slurry liquid viscosities. The measurement results are shown in Table 3 below.
[0280] (Evaluation of Photoreceptor)
[0281] The electrical properties, abrasion resistance (amount of abrasion), and film-forming resistance of the photoreceptors prepared in Examples 1 to 30 and Comparative Examples 1 to 10 were evaluated by the following methods. The evaluation results are shown in Table 4 below.
[0282] (Electrical Characteristics)
[0283] The electrical characteristics of the photoreceptors obtained in each of the Examples and Comparative Examples were evaluated by the following method using a process simulator (CYNTHIA91) manufactured by Genetech Co., Ltd.
[0284] For the photoreceptors of Examples 1 to 26 and Comparative Examples 1 to 6, the surface of the photoreceptors was charged to -650 V by corona discharge in a dark place at a temperature of 22° C. and a humidity of 50%, and the surface potential V0 immediately after charging was measured. Then, after leaving the photoreceptors in a dark place for 5 seconds, the surface potential V5 was measured, and the potential retention rate Vk5 (%) after charging for 5 seconds was calculated according to the following calculation formula (1).
[0285] Vk5=V5 / V0×100 (1)
[0286] Next, a halogen lamp was used as the light source, and a filter was used to separate the wavelength at 780 nm to obtain 1.0 μW / cm 2 The exposure light is irradiated to the photoreceptor for 5 seconds from the time when the surface potential reaches -600 V. The exposure amount required for the light to decay until the surface potential reaches -300 V is recorded as E1 / 2 (μJ / cm 2 ), and the residual potential on the surface of the photoreceptor after 5 seconds of exposure was recorded as Vr5 (V) for evaluation.
[0287] The photoreceptors of Examples 27 to 30 and Comparative Examples 7 to 10 were evaluated in the same manner as above with the charge potential set to +650 V and exposure light irradiated from the time the surface potential reached +600 V, with E1 / 2 being the exposure amount required until the surface potential reached +300 V.
[0288] (Evaluation of wear resistance)
[0289] The photoreceptors prepared in Examples 1 to 26 and Comparative Examples 1 to 6 were mounted on a HP printer LJ4250 and 10,000 sheets of A4 paper were printed. The film thickness of the photoreceptors before and after printing was measured, and the average abrasion amount (μm) after printing was evaluated.
[0290] In addition, the photosensitive bodies prepared in Examples 27 to 30 and Comparative Examples 7 to 10 were mounted on a printer HL-2040 manufactured by Brother Co., Ltd., and 10,000 sheets of A4 paper were printed. The film thickness of the photosensitive bodies before and after printing was measured, and the average abrasion (μm) after printing was evaluated.
[0291] (Evaluation of film formation)
[0292] Filming was evaluated based on the presence or absence of toner adhesion on the photoreceptor surface after repeated printing. No toner adhesion was evaluated as ○, slight toner adhesion was evaluated as △, and clear toner adhesion was evaluated as ×.
[0293] [Table 3]
[0294]
[0295] [Table 4]
[0296]
[0297] From the results of Tables 3 and 4 above, it can be seen that the photoreceptors of Examples 1 to 30 using inorganic oxides having high transmittance and low viscosity when made into inorganic oxide slurry and using lubricating resins have good wear resistance and good electrical properties, and no filming occurs at the initial stage and after printing 10,000 sheets. On the other hand, in Comparative Examples 1, 4 to 10, when no lubricating resin is added, it is confirmed that although the wear resistance is good, filming occurs after printing 10,000 sheets. In addition, in Comparative Example 3, when a soft resin is used, it is confirmed that although filming does not occur, the film wear amount increases.
[0298] From the above, it was confirmed that according to the present invention, the amount of wear on the surface of the photoreceptor can be reduced even in long-term use, and filming does not occur on the surface of the photoreceptor, so that a stable image can be obtained.
Claims
1. An electrophotographic photoreceptor comprising: a conductive substrate; and A negatively charged laminated photosensitive layer composed of a charge generating layer and a charge transporting layer sequentially formed on the conductive substrate, wherein the charge transporting layer comprises an inorganic oxide and a resin binder, The resin binder comprises a lubricating resin and other resins, and when the blending amount of the lubricating resin is recorded as A parts by mass and the blending amount of the other resin is recorded as B parts by mass, the ratio A / (B+A) of the lubricating resin in the total amount of the resin binder satisfies 0.1≤A / (B+A)≤0.5, The lubricating resin comprises a polycarbonate resin containing a siloxane structure or a polyarylate resin containing a siloxane structure, The other resin is a copolymerized polycarbonate resin having a repeating structure represented by the following general formula (10): In the general formula (10), R3 to R6 are the same or different and represent a hydrogen atom, an alkyl group having 1 to 10 carbon atoms or a fluoroalkyl group having 1 to 10 carbon atoms, g1, g2, g3, and g4 are integers of 0 to 4, r1 and r2 satisfy 0.3≤r2 / (r1+r2)≤0.7, and the chain end group is a monovalent aromatic group or a monovalent fluorinated aliphatic group, The polycarbonate resin containing a siloxane structure is a polycarbonate resin having a repeating structure represented by the following general formula (3): In the above general formula (3), R7 to R 10 may be the same or different, and represent a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a fluoroalkyl group having 1 to 10 carbon atoms, h1, h2, h3, and h4 are integers of 0 to 4, V1 represents an aliphatic divalent group or a cyclic aliphatic divalent group, V2 represents a single bond, a linear, branched, or cyclic alkylene group having 1 to 12 carbon atoms, -O-, -S-, -SO-, -SO2-, or -CO-, and U represents a structural unit represented by the following structural formula (5) or (6), In the above structural formulas (5) and (6), m1 and m2 are integers of 1 to 400. In the above general formula (3), r3 and r4 satisfy 0.2≤r4 / (r3+r4)≤0.8, r3, r4, k2, and k3 satisfy 0.001≤k2 / (r3+r4+k2)≤0.005 and 0.001≤k3 / (r3+r4+k3)≤0.005, and the chain terminal group is a monovalent aromatic group or a monovalent fluorinated aliphatic group, The polyarylate resin containing a siloxane structure is a copolymerized polyarylate resin having structural units represented by the following partial structural formulae (A1), (A2), (B1), (B2), (C) and (D), In the above structural formula, some structural formulas (A1), (A2), (B1), (B2), (C) and (D) represent structural units constituting the resin; a1, a2, b1, b2, c and d represent the mole % of each structural unit (A1), (A2), (B1), (B2), (C) and (D), respectively; a1+a2+b1+b2+c+d is 100 mole %, and c+d is 0.001 to 10 mole %; W1 and W2 are selected from single bonds, -O-, -S-, -SO-, -CO-, -SO2-, -CR 41 R 42 -, a substituted or unsubstituted cycloalkylene group having 5 to 12 carbon atoms, a substituted or unsubstituted α,ω alkylene group having 2 to 12 carbon atoms, -9,9-fluorenyl, a substituted or unsubstituted arylene group having 6 to 12 carbon atoms, and two different divalent groups of an aryl group or an arylene group-containing group having 6 to 12 carbon atoms, wherein R 41 and R 42 may be the same or different, and represent a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, a halogenated alkyl group, or a substituted or unsubstituted aryl group having 6 to 12 carbon atoms; R 11 ~R 30 may be the same or different, and represent a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, a fluorine atom, a chlorine atom, or a bromine atom; m3 represents an integer greater than 1, When a 20 mass % inorganic oxide slurry in which the inorganic oxide is dispersed at a concentration of 20 mass % relative to a solvent is irradiated with light having a wavelength of 780 nm, the transmittance of the light is 80% or more.
2. An electrophotographic photoreceptor comprising: a conductive substrate; and a single-layer photosensitive layer comprising an inorganic oxide and a resin binder formed on the conductive substrate; The resin binder comprises a lubricating resin and other resins, and when the blending amount of the lubricating resin is recorded as A parts by mass and the blending amount of the other resin is recorded as B parts by mass, the ratio A / (B+A) of the lubricating resin in the total amount of the resin binder satisfies 0.1≤A / (B+A)≤0.5, The lubricating resin comprises a polycarbonate resin containing a siloxane structure or a polyarylate resin containing a siloxane structure, The other resin is a copolymerized polycarbonate resin having a repeating structure represented by the following general formula (10): In the general formula (10), R3 to R6 are the same or different and represent a hydrogen atom, an alkyl group having 1 to 10 carbon atoms or a fluoroalkyl group having 1 to 10 carbon atoms, g1, g2, g3, and g4 are integers of 0 to 4, r1 and r2 satisfy 0.3≤r2 / (r1+r2)≤0.7, and the chain end group is a monovalent aromatic group or a monovalent fluorinated aliphatic group, The polycarbonate resin containing a siloxane structure is a polycarbonate resin having a repeating structure represented by the following general formula (3): In the above general formula (3), R7 to R 10 may be the same or different, and represent a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a fluoroalkyl group having 1 to 10 carbon atoms, h1, h2, h3, and h4 are integers of 0 to 4, V1 represents an aliphatic divalent group or a cyclic aliphatic divalent group, V2 represents a single bond, a linear, branched, or cyclic alkylene group having 1 to 12 carbon atoms, -O-, -S-, -SO-, -SO2-, or -CO-, and U represents a structural unit represented by the following structural formula (5) or (6), In the above structural formulas (5) and (6), m1 and m2 are integers of 1 to 400. In the above general formula (3), r3 and r4 satisfy 0.2≤r4 / (r3+r4)≤0.8, r3, r4, k2, and k3 satisfy 0.001≤k2 / (r3+r4+k2)≤0.005 and 0.001≤k3 / (r3+r4+k3)≤0.005, and the chain terminal group is a monovalent aromatic group or a monovalent fluorinated aliphatic group, The polyarylate resin containing a siloxane structure is a copolymerized polyarylate resin having structural units represented by the following partial structural formulae (A1), (A2), (B1), (B2), (C) and (D), In the above structural formula, some structural formulas (A1), (A2), (B1), (B2), (C) and (D) represent structural units constituting the resin; a1, a2, b1, b2, c and d represent the mole % of each structural unit (A1), (A2), (B1), (B2), (C) and (D), respectively; a1+a2+b1+b2+c+d is 100 mole %, and c+d is 0.001 to 10 mole %; W1 and W2 are selected from single bonds, -O-, -S-, -SO-, -CO-, -SO2-, -CR 41 R 42-, a substituted or unsubstituted cycloalkylene group having 5 to 12 carbon atoms, a substituted or unsubstituted α,ω alkylene group having 2 to 12 carbon atoms, -9,9-fluorenyl, a substituted or unsubstituted arylene group having 6 to 12 carbon atoms, and two different divalent groups of an aryl group or an arylene group-containing group having 6 to 12 carbon atoms, wherein R 41 and R 42 may be the same or different, and represent a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, a halogenated alkyl group, or a substituted or unsubstituted aryl group having 6 to 12 carbon atoms; R 11 ~R 30 may be the same or different, and represent a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, a fluorine atom, a chlorine atom, or a bromine atom; m3 represents an integer greater than 1, When a 20 mass % inorganic oxide slurry in which the inorganic oxide is dispersed at a concentration of 20 mass % relative to a solvent is irradiated with light having a wavelength of 780 nm, the transmittance of the light is 80% or more.
3. An electrophotographic photoreceptor comprising: a conductive substrate; and A positively charged laminated photosensitive layer composed of a charge transport layer and a charge generation layer sequentially formed on the conductive substrate, wherein the charge generation layer contains an inorganic oxide and a resin binder, The resin binder comprises a lubricating resin and other resins, and when the blending amount of the lubricating resin is recorded as A parts by mass and the blending amount of the other resin is recorded as B parts by mass, the ratio A / (B+A) of the lubricating resin in the total amount of the resin binder satisfies 0.1≤A / (B+A)≤0.5, The lubricating resin comprises a polycarbonate resin containing a siloxane structure or a polyarylate resin containing a siloxane structure, The other resin is a copolymerized polycarbonate resin having a repeating structure represented by the following general formula (10): In the general formula (10), R3 to R6 are the same or different and represent a hydrogen atom, an alkyl group having 1 to 10 carbon atoms or a fluoroalkyl group having 1 to 10 carbon atoms, g1, g2, g3, and g4 are integers of 0 to 4, r1 and r2 satisfy 0.3≤r2 / (r1+r2)≤0.7, and the chain end group is a monovalent aromatic group or a monovalent fluorinated aliphatic group, The polycarbonate resin containing a siloxane structure is a polycarbonate resin having a repeating structure represented by the following general formula (3): In the above general formula (3), R7 to R 10may be the same or different, and represent a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a fluoroalkyl group having 1 to 10 carbon atoms, h1, h2, h3, and h4 are integers of 0 to 4, V1 represents an aliphatic divalent group or a cyclic aliphatic divalent group, V2 represents a single bond, a linear, branched, or cyclic alkylene group having 1 to 12 carbon atoms, -O-, -S-, -SO-, -SO2-, or -CO-, and U represents a structural unit represented by the following structural formula (5) or (6), In the above structural formulas (5) and (6), m1 and m2 are integers of 1 to 400. In the above general formula (3), r3 and r4 satisfy 0.2≤r4 / (r3+r4)≤0.8, r3, r4, k2, and k3 satisfy 0.001≤k2 / (r3+r4+k2)≤0.005 and 0.001≤k3 / (r3+r4+k3)≤0.005, and the chain terminal group is a monovalent aromatic group or a monovalent fluorinated aliphatic group, The polyarylate resin containing a siloxane structure is a copolymerized polyarylate resin having structural units represented by the following partial structural formulae (A1), (A2), (B1), (B2), (C) and (D), In the above structural formula, some structural formulas (A1), (A2), (B1), (B2), (C) and (D) represent structural units constituting the resin; a1, a2, b1, b2, c and d represent the mole % of each structural unit (A1), (A2), (B1), (B2), (C) and (D), respectively; a1+a2+b1+b2+c+d is 100 mole %, and c+d is 0.001 to 10 mole %; W1 and W2 are selected from single bonds, -O-, -S-, -SO-, -CO-, -SO2-, -CR 41 R 42 -, a substituted or unsubstituted cycloalkylene group having 5 to 12 carbon atoms, a substituted or unsubstituted α,ω alkylene group having 2 to 12 carbon atoms, -9,9-fluorenyl, a substituted or unsubstituted arylene group having 6 to 12 carbon atoms, and two different divalent groups of an aryl group or an arylene group-containing group having 6 to 12 carbon atoms, wherein R 41 and R 42 may be the same or different, and represent a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, a halogenated alkyl group, or a substituted or unsubstituted aryl group having 6 to 12 carbon atoms; R 11 ~R 30 may be the same or different, and represent a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, a fluorine atom, a chlorine atom, or a bromine atom; m3 represents an integer greater than 1, When a 20 mass % inorganic oxide slurry in which the inorganic oxide is dispersed at a concentration of 20 mass % relative to a solvent is irradiated with light having a wavelength of 780 nm, the transmittance of the light is 80% or more.
4. The electrophotographic photoreceptor according to any one of claims 1 to 3, wherein The viscosity of the 20 mass % inorganic oxide slurry is below 50 mPa·s.
5. The electrophotographic photoreceptor according to any one of claims 1 to 3, wherein The primary particle size of the inorganic oxide is 1 to 500 nm.
6. The electrophotographic photoreceptor according to any one of claims 1 to 3, wherein The photosensitive layer is the outermost surface layer.
7. The electrophotographic photoreceptor according to any one of claims 1 to 3, wherein The inorganic oxide contains silicon dioxide as a main component.
8. The electrophotographic photoreceptor according to claim 7, wherein: The inorganic oxide contains silicon dioxide as a main component and contains aluminum element in an amount of 1 ppm to 1000 ppm both inclusive.
9. The electrophotographic photoreceptor according to claim 7, wherein: The inorganic oxide is surface treated with a silane coupling agent.
10. The electrophotographic photoreceptor according to claim 9, wherein The silane coupling agent has a structure represented by the following general formula (1): (R1) n -Si-(OR2) 4-n (1) In the formula, Si represents a silicon atom, R1 represents an organic group in a form in which carbon is directly bonded to the silicon atom, R2 represents an organic group, and n represents an integer of 0 to 3.
11. A method for producing an electrophotographic photoreceptor, comprising forming the photosensitive layer comprising an inorganic oxide and a resin binder using a photosensitive layer coating liquid, thereby producing the electrophotographic photoreceptor according to any one of claims 1 to 3, wherein: include: An inorganic oxide slurry preparation step of dispersing the inorganic oxide in the solvent for the photosensitive layer coating solution to obtain an inorganic oxide slurry; A photosensitive layer forming liquid preparation step of dissolving a charge transport material and a resin binder in the solvent for the photosensitive layer coating liquid to obtain a photosensitive layer forming liquid; and A photosensitive layer coating liquid preparation step is to mix the obtained inorganic oxide slurry and the photosensitive layer forming liquid to obtain the photosensitive layer coating liquid. 12 . An electrophotographic apparatus comprising the electrophotographic photoreceptor according to claim 1 mounted thereon.