Silicon Etching Method

By using O2 to react with Si to generate SiO, the problem of toxicity and environmental impact of reaction products in XeF2 is solved, efficient and environmentally friendly silicon etching is achieved, and the etching selection ratio of Si/Si3N4 and Si/SiO2 is improved. Reduced process costs.

CN111916349BActive Publication Date: 2024-11-26BEIJING NAURA MICROELECTRONICS EQUIP CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN201910379737.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-05-08
Publication Date
2024-11-26
Estimated Expiration
2039-05-08

AI Technical Summary

Technical Problem

In the existing silicon etching methods, XeF2 as an etching gas has toxicity problems, the reaction products are harmful to the environment, and the etching choices of Si/Si3N4 and Si/SiO2 are relatively low, which easily leads to the barrier layer being etched away.

Method used

O2 is used as the etching gas to react with Si to generate volatile SiO. Etching is achieved by adjusting the chamber temperature and oxygen partial pressure to avoid the introduction of toxic gases and improve the etching selection ratio.

Benefits of technology

Non-toxic and low-cost silicon etching is achieved, reducing process costs, improving the etch selection ratio of Si/Si3N4 and Si/SiO2, improving product yield, and simplifying the process flow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111916349B_ABST
    Figure CN111916349B_ABST
Patent Text Reader

Abstract

The present invention provides a silicon etching method, which comprises: introducing O2 into a reaction chamber to achieve etching of Si by reacting with Si; wherein the chamber temperature and oxygen partial pressure are set to allow O2 to react with Si to generate volatile SiO. The silicon etching method provided by the present invention can avoid the introduction of toxic gases, and the reaction products will not have adverse effects on the environment, and can improve the etching selectivity of Si / Si3N4 and Si / SiO2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of etching, and in particular to a silicon etching method. Background Art

[0002] Sacrificial layer etching is a very important process in integrated circuits. However, with the update of technology, the original etching methods have encountered more and more bottlenecks. There are two types of etching for sacrificial layer materials: wet and dry. Among them, wet etching uses corrosive liquid to corrode the sacrificial layer, and the film is very easy to adhere and crack. Moreover, wet etching is difficult to achieve small hole pattern cleaning due to surface tension. In addition, wet etching often has a poor selectivity.

[0003] Dry etching mainly includes plasma dry etching and non-plasma dry etching. Since plasma dry etching uses plasma etching, it is inevitable that there will be a certain amount of ion implantation on the surface, which will cause electrical damage to nano devices. Non-plasma dry etching uses etching gas to react with sacrificial layer materials to generate waste gas and then discharge it. This method can remove the sacrificial layer without damaging the structure, and has good consistency and uniformity.

[0004] However, when performing silicon etching methods, existing non-plasma dry etching methods generally use XeF 2 As etching gas, XeF 2 It is a type of fluorine-based etchant. Gaseous XeF 2 It will spontaneously react with Si at room temperature to generate gaseous SiF 4 and Xe. However, XeF 2 The toxicity is relatively high, and the reaction products will have adverse effects on the environment. 3 N 4 and Si / SiO 2 The etching selectivity is relatively low, which can easily lead to the barrier layer SiO 2 Or Si 3 N 4 Be etched away. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art, and proposes a silicon etching method, which can avoid the introduction of toxic gases, and the reaction products will not have adverse effects on the environment, and can improve Si / Si 3 N 4 and Si / SiO 2 The etching selectivity ratio.

[0006] To achieve the above object, the present invention provides a silicon etching method, comprising:

[0007] O was introduced into the reaction chamber 2 , so as to achieve etching of Si by reacting with Si;

[0008] The chamber temperature and oxygen partial pressure are set to satisfy the conditions that the O 2 Reacts with Si to form volatile SiO.

[0009] Optionally, the chamber temperature ranges from 800°C to 1800°C.

[0010] Optionally, the oxygen partial pressure is in the range of 0.2×10 -5 -1×10 -2 Torr.

[0011] Optionally, the flow rate of the oxygen gas ranges from 5 to 200 sccm.

[0012] Optionally, anisotropic etching or isotropic etching is achieved by adjusting the flow rate of the oxygen.

[0013] Optionally, the flow rate of the oxygen gas is adjusted so that the flow rate of the oxygen gas is less than or equal to 30 sccm to achieve anisotropic etching; or, the flow rate of the oxygen gas is adjusted so that the flow rate of the oxygen gas is greater than 30 sccm to achieve isotropic etching.

[0014] Optionally, O is introduced into the reaction chamber. 2 At the same time, a dilution gas is introduced into the reaction chamber.

[0015] Optionally, the flow rate of the dilution gas ranges from 1 to 1000 sccm.

[0016] Optionally, the dilution gas includes nitrogen or an inert gas.

[0017] Optionally, the chamber pressure can be in the range of 10 -5 -10 -2 Torr.

[0018] Optionally, the reaction chamber is introduced with O 2 , so as to realize the step of etching Si by reacting with Si, and perform the step once or multiple times to complete the preset etching depth.

[0019] Beneficial effects of the present invention:

[0020] The silicon etching method provided by the present invention adopts O 2 As an etching gas, it reacts with Si to etch Si. At the same time, the chamber temperature and oxygen partial pressure are set to make O 2 Reacts with Si to form volatile SiO. 2It is non-toxic, low-cost, and the generated SiO will not have adverse effects on the environment, so there is no need for complex tail gas treatment, which can greatly reduce the process cost and improve Si / Si 3 N 4 and Si / SiO 2 The etching selectivity ratio can be improved, thereby improving the product yield. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a flow chart of the silicon etching method provided by the present invention.

[0022] Figure 2 A schematic structural diagram of process equipment used in the silicon etching method provided by the present invention. DETAILED DESCRIPTION

[0023] In order to enable those skilled in the art to better understand the technical solution of the present invention, the silicon etching method provided by the present invention is described in detail below with reference to the accompanying drawings.

[0024] See also Figure 1 The present invention provides a silicon etching method, which comprises:

[0025] Step S1, introducing O into the reaction chamber 2 , so as to achieve etching of Si by reacting with Si. The chamber temperature and oxygen partial pressure are set to make O 2 Reacts with Si to form volatile SiO.

[0026] The silicon etching method provided by the present invention is a non-plasma dry etching method. 2 It reacts with Si to generate volatile SiO and then is discharged. This method not only does not damage the substrate surface during the etching process, but also has good consistency and uniformity when using this method to etch silicon.

[0027] The silicon etching method provided by the present invention adopts O 2 As etching gas, O 2 It is non-toxic, low-cost, and the generation of SiO will not have adverse effects on the environment, so there is no need for complex tail gas treatment, which can greatly reduce the process cost. At the same time, by setting the appropriate chamber temperature and oxygen partial pressure, O 2 Reacting with Si to generate volatile SiO, that is, by controlling the chamber temperature and the oxygen partial pressure, the reaction product is made gaseous, which can make the silicon etching method provided by the present invention applicable to the pattern cleaning of small holes with high cleaning efficiency. 2 As an etching gas, it can improve Si / Si 3 N 4and Si / SiO 2 The etching selectivity ratio can be improved, thereby improving the product yield.

[0028] Through experiments, it was found that the use of O 2 As etching gas, Si / Si 3 N 4 and Si / SiO 2 The etching selectivity ratio can reach 1000:1.

[0029] Optionally, the chamber temperature ranges from 800°C to 1800°C. By controlling the chamber temperature within this range, it can be ensured that O 2 Reacts with Si to form volatile SiO.

[0030] Optionally, the oxygen partial pressure range is 0.2×10 -5 -1×10 -2 Torr. The so-called oxygen partial pressure refers to the product of the flow ratio and the chamber pressure, wherein the flow ratio is the ratio of the flow rate of oxygen to the total flow rate of all gases introduced into the reaction chamber. For example, if the gas introduced into the reaction chamber is only oxygen, the oxygen partial pressure is the product of the flow rate of oxygen and the chamber pressure. By controlling the oxygen partial pressure within the above range, it can be ensured that O 2 Reacts with Si to form volatile SiO.

[0031] Optionally, the oxygen flow rate is in the range of 5-200 sccm. By controlling the oxygen flow rate within this range, both the etching rate and the O 2 Reacts with Si to form volatile SiO.

[0032] Optionally, anisotropic etching or isotropic etching can be achieved by adjusting the flow rate of oxygen. In this way, the flow rate of oxygen can be adjusted according to different needs to obtain different etching patterns, so that the silicon etching method provided by the present invention can be applied to different processes, such as silicon sacrificial layer etching process, deep silicon etching process, silicon hard mask etching process, silicon mandrel etching process, etc. Specifically, anisotropic etching can be achieved by making the flow rate of oxygen less than or equal to 30sccm; or, isotropic etching can be achieved by making the flow rate of oxygen greater than 30sccm.

[0033] Optionally, the chamber pressure can be in the range of 10 -5 -10 -2 By controlling the chamber pressure within this range, both the etching uniformity and the O 2 Reacts with Si to form volatile SiO.

[0034] From the above, it can be seen that the silicon etching method provided by the present invention has a higher chamber temperature and a lower chamber pressure, which means that the substrate no longer needs to undergo a degassing process before entering the reaction chamber to remove water vapor on the surface of the substrate, thereby simplifying the process steps, improving production capacity, and reducing process costs.

[0035] Preferably, when O is introduced into the reaction chamber 2 At the same time, a dilution gas is introduced into the reaction chamber. With the help of the dilution gas, not only can the oxygen partial pressure be adjusted, but it also helps the flow of etching gas and the discharge of exhaust gas, thereby not only improving the consistency and uniformity of the process, but also improving the process efficiency. Optionally, the dilution gas includes nitrogen or an inert gas, etc. Optionally, the flow rate of the dilution gas ranges from 1 to 1000 sccm. By controlling the flow rate of the dilution gas within this range, it can be ensured that the oxygen partial pressure satisfies the requirement of O 2 It reacts with Si to generate volatile SiO, and also helps the flow of etching gas and the discharge of exhaust gas.

[0036] See also Figure 2 , which is a schematic diagram of the structure of the process equipment used in the silicon etching method provided by the present invention. The process equipment includes a reaction chamber 3, a first air inlet pipeline 5 and a second air inlet pipeline 6 for respectively introducing nitrogen and oxygen into the reaction chamber 3, and an exhaust device 4. Among them, a first flow controller 1 and a second flow controller 2 are respectively provided on the first air inlet pipeline 5 and the second air inlet pipeline 6, for respectively adjusting the flow rate of nitrogen and the flow rate of oxygen. The exhaust device 4 generally includes an exhaust pump and a flow regulating valve. By controlling the flow regulating valve to adjust the exhaust gas flow rate, the chamber pressure can be adjusted.

[0037] Optionally, the above step S1 can be performed once or multiple times to achieve the preset etching depth. It is easy to understand that when the above step S1 is performed multiple times to achieve the preset etching depth, the sum of the etching depths of multiple steps S1 is equal to the preset etching depth.

[0038] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.

Claims

1. A silicon etching method, characterized in that: include: Introducing O2 into the reaction chamber to etch Si by reacting with Si; The chamber temperature and oxygen partial pressure are set to allow the O2 to react with Si to generate volatile SiO; Anisotropic etching or isotropic etching is achieved by adjusting the flow rate of the oxygen; The flow rate of the oxygen gas is adjusted so that the flow rate of the oxygen gas is less than or equal to 30 sccm to achieve anisotropic etching; the flow rate of the oxygen gas is adjusted so that the flow rate of the oxygen gas is greater than 30 sccm to achieve isotropic etching.

2. The silicon etching method according to claim 1, characterized in that: The chamber temperature ranges from 800°C to 1800°C.

3. The silicon etching method according to claim 1, characterized in that: The oxygen partial pressure ranges from 0.2×10 -5 -1×10 -2 Torr.

4. The silicon etching method according to any one of claims 1 to 3, characterized in that: The flow rate of the oxygen gas ranges from 5 to 200 sccm.

5. The silicon etching method according to any one of claims 1 to 3, characterized in that: While O2 is introduced into the reaction chamber, a dilution gas is introduced into the reaction chamber.

6. The silicon etching method according to claim 5, characterized in that: The flow rate of the dilution gas ranges from 1 to 1000 sccm.

7. The silicon etching method according to claim 5, characterized in that: The diluent gas includes nitrogen or an inert gas.

8. The silicon etching method according to any one of claims 1 to 3, characterized in that: The chamber pressure range is 10 -5 -10 -2 Torr.

9. The silicon etching method according to claim 1, characterized in that: The step of introducing O2 into the reaction chamber to etch Si by reacting with Si is performed once or multiple times to complete a preset etching depth.

Citation Information

Patent Citations

  • Method for etching deep through silicon via (TSV)

    CN102031525A

  • Method for controlling size of germanium nanometer microstructure

    CN102569027A

  • Germanium nanowire structure manufacturing method

    CN103693615A