Methods for recycling silicone

By heat-treating silicone rubber and silicone oil in a digestion system of acetic anhydride and Bronsted acid and converting them into acetoxysiloxane and silane, the problem of recycling silicone materials is solved, and material reuse and environmental protection are achieved.

CN112011085BActive Publication Date: 2024-10-01EVONIK OPERATIONS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010465608.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-05-28
Filing Date
2020-05-28
Publication Date
2024-10-01
Estimated Expiration
2040-05-28

AI Technical Summary

Technical Problem

Existing technology makes it difficult to effectively recycle silicone materials, resulting in the production of fine silica when landfilled and burned, causing environmental and economic problems.

Method used

Silicone recycling is achieved by thermally treating silicone rubber and silicone oil in a digestion system containing acetic anhydride and Bronsted acid to convert them into silicones and silanes with acetoxy groups.

Benefits of technology

This method allows silicone materials to be converted into reactive silicones and silanes at high thermal processing temperatures, enabling simple processing into valuable products, avoiding landfills, and is applicable to all types of silicone materials, including high molecular weight solids and Liquid silicone.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present application relates to a method for recycling silicones. A method for recycling silicones, in particular silicone rubbers and / or silicone oils, by chemically converting them into silanes and / or siloxanes having acetoxy groups is described, wherein the silicone rubbers and / or silicone oils are thermally treated in a digestion system comprising acetic anhydride and / or acetoxysiloxanes and at least one Bronsted acid, preferably with the addition of acetic acid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of silicone; more specifically, the present invention relates to a method for recycling silicone by chemically converting silicone (preferably silicone rubber and silicone oil) into silanes and / or siloxanes with acetoxy groups, as well as a method for converting them into silanes and / or siloxanes with alkoxy groups, and a method for converting silanes and / or siloxanes with acetoxy groups into silanes and / or siloxanes with hydroxyl groups. Background Art

[0002] Silicone components meet specific requirements from the medical, pharmaceutical and food technology point of view due to their specific material properties. If handled properly, they are physiologically completely inert. For example, products made of silicone are encountered in food applications, medicine and the pharmaceutical sector. Pacifiers for babies are made of silicone, as are diver's goggles. In technical industrial applications, silicone appears in many cases as a material for gaskets or for membranes in dynamic applications. It is used in the automotive sector for hoses, sheaths or as cable insulation.

[0003] Silicones have a key advantage over other rubber types in terms of their mechanical properties. In the case of silicones, they remain at a relatively stable level over a very wide temperature range, whereas the mechanical properties of many other materials degrade significantly under cold or hot conditions. For example, when looking at the technical data sheet for EPDM material, it is shown that it is superior to silicone blends in terms of mechanical properties, because the properties at room temperature are reported here, and the exact opposite image is found at high or low temperatures. The thermal stability of silicone in air is from about -80°C to about 250°C. Because of the very low compression set typical of silicones shown here, this property is widely used in gaskets.

[0004] Due to their excellent ozone, UV and weathering stability, silicone mixtures are also frequently used for outdoor applications. In addition, silicones have very low flammability and have good electrical insulation capabilities and good electrical conductivity. For example, silicones are chemically stable to vegetable and animal fats, hot water and alcohol. The stability is limited by acids, bases, fuels and ketones as well as water vapor. Silicones also have very high air permeability.

[0005] In addition to industrial applications, silicone has been used for decades as a preferred elastomer in the medical field. Silicone components are also used as short-term implants (less than 30 days in Class IIa medical products) or long-term implants (30 days or longer in Class IIb medical products), where they perform critical functions in devices such as cardiac catheters, pacemakers, ventilators, neurostimulators and defibrillators.

[0006] Silicone rubber for long-term implants is supplied worldwide by only a very few producers, such as NuSil Technology. These compounds are produced according to strict regulations issued by the US Food and Drug Administration (FDA). Even during processing, exceptional purity must be ensured and components must be produced in clean rooms.

[0007] An important advantage of silicone here is that it is biocompatible and therefore well tolerated by humans. The biocompatibility of silicone mixtures is usually shown by USP Class VI classification (USP stands for United States Pharmacopeia) or by testing according to the more stringent (DINEN) ISO 10993 standard. (DINEN) ISO 10993 is used in particular for testing medical products that are implanted in the human body for a long period of time or permanently. For shorter-term applications, a classification according to USP Class VI or possibly a lower classification is sufficient.

[0008] Furthermore, silicone offers the option of steam sterilization (heating in an autoclave) due to its ability to be used over a wide temperature range of about -80°C to about 250°C. Thus, silicone products can be free of living microorganisms, their dormant forms, viruses, etc. The good electrical insulation properties of silicone are also of particular interest in the medical field.

[0009] By varying the silicone rubber used and the crosslinking pattern, silicones can be given specific properties. For example, HTV silicone rubbers are flexible and stable over a wide temperature range from -50°C up to 200°C, in some cases up to 300°C. They can be found in gaskets in the automotive or food industries, in cable sheathing or as insulation material.

[0010] RTV silicone rubbers are particularly valuable due to their thermal conductivity and electrical insulation capabilities, so they are preferably used in the electrical and electronic fields.

[0011] Liquid silicones (also LSR, liquid silicone rubber) have a lower viscosity than HTV and RTV silicone rubbers. They can be converted into a variety of different forms and processed by injection molding, for example to give silicone hoses. Since LSR silicones are always produced with platinum crosslinking, products based on liquid silicones can be used in the medical technology sector.

[0012] Due to its high stability in the human body, silicone constitutes a very good protection for critical components and is additionally preferably used for functional components due to the properties mentioned.

[0013] In principle, silicone rubber differs from other organic elastomers in that its main chain with an inorganic structure is not composed of carbon compounds, but is formed by a combination of silicon atoms and oxygen atoms, especially using pyrogenic silica as a filler to form good properties.

[0014] According to the material state of silicone rubber and their vulcanization temperature, they can be divided into three groups:

[0015] Silicone rubbers known as HTV (high temperature vulcanized) or HCR (high consistency rubber) are those with solid raw materials. These silicone rubbers are usually vulcanized at high temperatures between 140° C. and 200° C. Crosslinking occurs by peroxide or by addition reaction using platinum compounds as catalysts.

[0016] Liquid silicone or LSR (liquid silicone rubber) as raw material is a (viscous) fluid and consists of two components which are mixed directly before processing. The crosslinking takes place by addition reaction at temperatures similar to those of HIV type, usually significantly faster crosslinking takes place.

[0017] Both silicone types can be coloured. Finished elastomeric articles made from HTV silicone and LSR silicone differ little in their properties.

[0018] The third group is the so-called RTV (room temperature vulcanizing) silicones. In these cases, crosslinking already occurs at room temperature. They are widely used as sealing compounds or for prototyping. They are available both as one-component systems and as two-component systems.

[0019] While the performance benefits of silicone due to its superior chemical stability contribute to the useful life of articles made from silicone, the stability of silicone is a problem when it comes to disposal at the end of its life cycle.

[0020] The extent to which silicone rubber materials can be utilized, for example by mechanically comminuting spent material consisting of silicone rubber and adding the comminuted material thus obtained as filler to new silicone rubber compounds that have not yet been cured, may be very limited. Transporting silicone waste to suitable landfills and burying them therein can incur considerable costs. In the ever-increasing environmental debate, their natural non-degradability or difficulty in degradation also puts silicones on the dark side from a sustainability point of view.

[0021] In the case of purely hydrocarbon-based polymers, such as polyethylene and polypropylene, energy utilization, which is an option of converting these polymers into heat energy and releasing carbon dioxide and water by combustion, is not a viable option for silicones, since their combustion produces large amounts of finely divided silica, which leads to even greater technical problems. On the other hand, according to information from ECO America, the recycling of 1 metric ton of silicone rubber saves 5774 kWh of energy, 16.3 barrels of oil and 98 million BTU of energy.

[0022] In addition to the material and energy utilization of silicone waste, the technical problem to be solved is therefore defined as providing an environmentally feasible and at the same time economically attractive physical recycling method for all kinds of silicones, which allows avoiding their landfilling and feeding the silicone materials back into value-generating, new silicone-based material flows. In addition, the method sought should also be applicable to silicone oils.

[0023] US 5110972 is devoted to the physical recycling of used silicone by dissolving the silicone waste in a suitable solvent and converting the silicone waste into dimethylsiloxane rings such as D3, D4, D5, etc. by using a two-stage acid / base catalytic cracking process. The silicone waste used therein consists of a high molecular weight liquid or elastomeric material, in particular a solid formed of silicone polymers, usually with short alkyl groups, especially methyl groups. Thus, the silicone rings are obtained in high yield by distillation.

[0024] Japanese publication Heisei 9-176364 proposes a method in which silicone resins are decomposed into recyclable siloxane monomers or oligomers under the action of orthocarboxylic acid esters and compounds with active hydrogen groups and catalysts. The disadvantage of this method is that it is carried out under the relatively mild and inexpensive conditions described therein and is inevitably affected by unwanted by-products from the hydrolysis of the orthocarboxylic acid esters, for example, if methyl orthoformate is used as the orthocarboxylic acid ester, it will be affected by methyl formate. Since it is not possible to directly use the monomers or oligomers containing orthocarboxylic acid esters, that is, obtained, it is necessary to further post-treat them, for example as described in Japanese publication Heisei 9-7779. In view of these difficulties and the complexity involved, this method has not yet become part of industrial practice.

[0025] In light of these Japanese publications, US Pat. No. 6,172,253 B1 likewise relates to the physical recycling of silicone-containing materials, i.e., those having Si-O-Si bonds, by decomposing these silicone-containing materials with alkyl carbonates and active hydrogen-containing compounds in the presence of a catalyst to form a large number of silicone monomers and / or silicone oligomers (more than 200 different examples in the product mixture).

[0026] According to this teaching, treatment of silicone rubber at 90° C. under reflux conditions for 4 hours in a mixture of dimethyl carbonate and methanol with addition of sulfuric acid leads to a highly variable substance mixture comprising more than 200 different compounds, including dimethoxydimethylsilane.

[0027] The non-selectivity of otherwise mild digestion processes makes them unattractive, since any reuse of the materials from the decomposition reaction first requires passing through complex thermal separation processes.

[0028] EP 1057855A1 teaches a method for the digestion of crosslinked silicone wastes, wherein they are hydrolyzed by reacting them with hydroxyl-containing solvents such as methanol, ethanol or isopropanol under supercritical conditions. Non-crosslinked, non-functionalized silicone compounds (=silicone oils) are obtained here, as shown by the infrared spectrum included therein. The necessity of observing supercritical pressure conditions requires the use of pressure-grade equipment, which makes this method expensive on an industrial scale.

[0029] Enthaler et al. focused on the iron-catalyzed depolymerization of polysiloxanes for the preparation of dichlorodimethylsilane, diacetoxydimethylsilane and dimethoxydimethylsilane (J. Appl. Polym. Sci. 2015, DOI: 10.1002 / APP.41287). In order to obtain dimethyldichlorosilane, the authors allowed aromatic and aliphatic acid chlorides and p-toluenesulfonyl chloride to act on α,ω-dihydroxypolydimethylsiloxane at a temperature of 170-190°C under the catalysis of iron salts. In most of the reaction systems provided, the yield of dimethyldichlorosilane is very low and ranges from <1% to 62% (Table I, supra); a reaction system consisting of α,ω-dihydroxypolydimethylsiloxane (chain length N=7), 7.5 mol% of iron(III) fluoride and 3 equivalents of benzoyl chloride alone, based on each dimethylsiloxy unit used, gives dimethyldichlorosilane in 86% yield after treatment at 190°C for five hours.

[0030] Apart from the fact that the depolymerization of silicones to give chlorosilane substances is undesirable from the perspective of the environment, disposal and waste avoidance, which is especially true for chemical companies that do not carry out the Müller-Rochow synthesis themselves, the use of phosgene makes the process expensive and uneconomical. Furthermore, the amount of iron(III) fluoride required is considerable and is already 41 g for every 550 g of α,ω-dihydroxypolydimethylsiloxane used.

[0031] The same reference (page 5) also describes the option of depolymerizing α,ω-dihydroxypolydimethylsiloxane (chain length N=7) with acetic anhydride in the temperature range of 140° C. to 180° C. with a reaction time of 16 hours under iron salt catalysis. A pressure tube is used here. Experiments at 160° C. with 2.5 mol % of iron(III) chloride, 2 equivalents of acetic anhydride (in each case based on each dimethylsiloxy unit used) give a yield of 51% of diacetoxydimethylsilane and also some polydimethylsiloxane rings, such as D4 and D6.

[0032] The yields are modest for industrial purposes and the use of relatively large quantities of highly corrosive iron halides is additionally unattractive since most chemical reactors are made of, for example, highly alloyed stainless steels rather than Hastelloy.

[0033] Apparently even further removed from industrial practice is the effort described in the same reference, which depolymerizes α,ω-dihydroxypolydimethylsiloxane (chain length N=7) in excess methanol with the aid of an autoclave, under ferric salt catalysis (Fe(III) fluoride), and adds 3.0 equivalents of poly(propylene carbonate) per dimethylsiloxy unit used, over the course of 24 hours at a reaction temperature of 180° C. to obtain the desired dimethoxydimethylsilane. Here only dimethoxydimethylsilane is formed in a yield of 18%, while 14% of propane-1,2-diol and 32% of propylene carbonate are formed.

[0034] Another route for the physical recycling of silicones, in particular silicone oils, is described by Enthaler et al. in ACS Sustainable Chemistry & Engineering 3(1), 2015, pp. 163-169. The authors use the reagent boron trifluoride etherate to obtain difluorodimethylsilane and 1,3-difluoro-1,1,3,3-tetramethyldisiloxane in moderate yields, for example, from α,ω-dihydroxypolydimethylsiloxane containing only 7D units, and then convert the product into α,ω-dihydroxypolydimethylsiloxane under the action of aqueous sodium hydroxide solution. Factors of doubt about this method in terms of industrial practice are especially the handling of expensive boron reagents and fluorides, which, as the authors assume, would be suitable for recycling boron trifluoride.

[0035] Enthaler et al. reported in Eur. J. Lipid Technol. 2015, 117, 778-785 the iron-catalyzed depolymerization of poly(dimethylsiloxane) with hexanoic anhydride at 200° C. for 24 hours. The authors observed that this method converted silicone oils into the corresponding short-chain silicone entities with hexoxy functional groups in good yields, but found that its limitation was the use of high molecular weight end-of-life silicones, such as those used in baking trays.

[0036] These academic contributions have enriched the understanding of the degradation mechanisms involved, arguably lacking an industrially feasible and attractive physical recycling route for silicone oils and solid silicones.

[0037] WO 2014 / 130948 A1 teaches a method for recycling silicone waste from a mixture with an organic polymer and a depolymerization catalyst, wherein the mixture is heated to at least such an extent that at least some of the siloxanes used are converted into cyclosiloxanes and residues, and the cyclosiloxanes are removed from the heated matrix in a degassing operation. The examples in this patent specification illustrate that the technical complexity involved in obtaining siloxane ring utilization is considerable, since the depolymerization is first carried out in a first step in an apparatus consisting of two connected screw extruders at high temperature and with the application of an auxiliary vacuum, and the residue from the first step is then further depolymerized in a second step in an apparatus comprising a stirrer at a temperature of up to 260° C. and with the application of an auxiliary vacuum. Summary of the invention

[0038] In view of this prior art, the problem to be solved was to find a simple method which enables the recycling of silicones. Surprisingly, the inventors have now been able to provide a method which enables this and which allows both silicone rubbers and silicones to be converted into reactive siloxanes and / or silanes and which allows easy processing thereof, for example to give silanes and / or siloxanes carrying alkoxy groups and / or silanes and / or siloxanes carrying hydroxyl groups. It has been found that, surprisingly, not only silicone oils but also solid silicone rubbers can be converted in a valuable manner into siloxanes and / or silanes carrying reactive acetoxy groups by thermally treating them in a digestion system, in each case with the addition of acetic acid.

[0039] Against this background, the present invention provides a method for recycling silicone by chemically converting silicone, in particular silicone rubber and / or silicone oil, into siloxanes and / or silanes having acetoxy groups, wherein the silicone to be recycled is prepared in a reaction mixture containing acetic anhydride and / or acetoxysiloxane and at least one Bronsted acid ( acid), preferably added to a digestion system of acetic acid for heat treatment.

[0040] In a particularly preferred embodiment, the process according to the invention is carried out with addition of acetic acid.

[0041] In a preferred embodiment of the present invention, the digestion system comprises:

[0042] a) acetic anhydride and Bronsted acids, b) acetic anhydride, siloxane rings and / or hydroxy-functional siloxanes and Bronsted acids, c) acetoxysiloxanes and Bronsted acids, or d) acetoxysiloxanes, siloxane rings and / or hydroxy-functional siloxanes, acetic anhydride and Bronsted acids, preference being given to adding acetic acid in each case.

[0043] Preferably, according to the invention, the Bronsted acid used is a protic acid with a pKa of less than -1.30, such as preferably nitric acid, methanesulfonic acid and p-toluenesulfonic acid, preferably a protic acid with a pKa of less than -2.90, such as preferably concentrated sulfuric acid,

[0044] More preferred are protic acids with a pKa less than -4.90, such as preferably perfluoroalkanesulfonic acids, such as heptafluoropropanesulfonic acid, pentafluoroethanesulfonic acid, trifluoromethanesulfonic acid, followed by perchloric acid and chlorosulfonic acid,

[0045] Among these, perfluoroalkanesulfonic acid is preferred in particular, and trifluoromethanesulfonic acid is very particularly preferred here,

[0046] And also preferably, for example, the commercially available product and and perfluoroalkylsulfonic acid resins such as Sulfonic acid or perfluoroalkylsulfonic acid ion exchange resins in the form of (eg NR 50 type).

[0047] Particularly preferred Bronsted acids for use according to the invention are perfluoroalkanesulfonic acids, most preferably trifluoromethanesulfonic acid.

[0048] In principle, all silicones, in particular silicone rubbers and / or silicone oils, can be recycled within the scope of the present invention. More particularly, this also applies to all silicones listed in the introductory part of the description. Reference is therefore made explicitly to them. In a preferred embodiment of the present invention, the process according to the present invention relates to a process for recycling silicones, in particular silicone rubbers and / or silicone oils, with the exception of hexamethyldisiloxane. In a preferred embodiment of the present invention, the silicone oil to be recycled consists of D and M units. In another preferred embodiment of the present invention, the silicone to be recycled has a molar mass of >236 g / mol.

[0049] The method according to the invention for recycling silicone can be demonstrated in particular by the digestion of high-quality silicone hose (Example 1).

[0050] The digestion of the high molecular weight solid silicone according to the invention is also applicable to silicone oils (eg, to polydimethylsiloxanes terminated with trimethylsilyl groups, Example 2).

[0051] Preferably, according to the present invention, the heat treatment of silicone oil or silicone rubber in the digestion system is preferably carried out between 50°C and 200°C, more preferably between 80°C and 160°C, especially between 120°C and 150°C.

[0052] The digestion process according to the invention can advantageously be carried out at standard pressure (1013 hPa), reduced pressure or other pressures in order to achieve high heat treatment temperatures of up to 200° C. at elevated pressure in pressure-rated equipment. Preferably, the digestion process according to the invention is carried out at standard pressure.

[0053] Preferably, according to the present invention, the amount of the Bronsted acid used in the digestion system is advantageously 0.1 to 1.5 mass %, preferably 0.15 to 1.0 mass %, more preferably 0.2 to 0.8 mass %, based on the total mass of the corresponding digestion system.

[0054] According to the present invention, it is preferred that the amount of acetic acid added to the digestion system is advantageously 0.5-4.0% by mass, preferably 1.5-3.5% by mass, based on the total mass of the corresponding digestion system.

[0055] If desired, the silanes and / or siloxanes with reactive acetoxy functions obtained by the process according to the invention can be used again as adhesives and sealants, for example in the form of polymeric active substances, optionally blended with other crosslinking silanes and / or siloxanes, filled and / or unfilled with fillers.

[0056] It is obvious to the person skilled in the art that the respective nature and chemical composition of the silicone used and intended for recycling shapes the composition of acetoxy-containing siloxanes obtained by the process according to the invention. For example, if trimethylsilyl units are present in the precursor material, their presence also leads to the formation of trimethylsilyl acetate (see Example 2, silicone oil).

[0057] The process according to the invention therefore even constitutes an attractive alternative route to the synthesis of trimethylsilyl acetates in its configuration involving the recycling of polydimethylsilicone. Trimethylsilyl acetates are silanizing agents which play a major role in protecting group chemistry, especially in the synthesis of natural products and pharmaceutically active molecules. The importance of the trimethylsilyl protecting group was shown, for example, by Oppolzer in US Pat. No. 4,328,353 in the synthesis of norpatchoulenol.

[0058] In a preferred embodiment of the invention, the digestion system contains acetic anhydride. The amount of acetic anhydride advantageously used here is guided by the amount of silicone rubber and / or silicone oil to be recycled and the desired target structure of the silanes / siloxanes carrying acetoxy groups (the desired average chain length is defined in each case by the amount of acetic anhydride used, based on the amount of silicone substrate to be recycled).

[0059] If the digestion method of the invention is carried out in a reactor with a simple stirring and / or mixing aggregate, the procedure when adding any other reaction components is guided only by observing how the reaction matrix (for example consisting of silicone rubber chips and liquid) can be mixed with the added corresponding reactants, which in some cases is very inhomogeneous at the beginning of the method. Such a procedure is shown in Example 5.

[0060] In the context of the present invention, the term "siloxanes containing acetoxy groups" also relates in particular to substances which contain varying amounts of silanes having acetoxy groups, for example trimethylsilyl acetate, diacetoxydimethylsilane and the like.

[0061] The polymerization behavior of the silanes and / or siloxanes having reactive acetoxy groups obtained according to the invention could already be demonstrated in a simple manual experiment by applying a small volume of about 0.5 to 2 ml to a black bakelite lid. In particular, the still Brønsted-acidic acetoxysilanes / siloxanes polymerize very quickly under the influence of air humidity and leave an opaque white silicone film.

[0062] Alternatively, the high reactivity of the acetoxysilanes and / or siloxanes obtained by the process according to the invention also allows their conversion, for example, into the corresponding alkoxysilanes / siloxanes.

[0063] The present invention therefore also relates to the preparation of alkoxy-substituted silanes and / or siloxanes from the Brønsted-acidic acetoxysilanes and / or siloxanes obtained according to the invention.

[0064] The inventors have established that the acetoxysilanes and / or siloxanes which are still Brønsted-acidic and which are obtained by the process according to the invention should first preferably be brought into contact with a sufficient amount of base to neutralize the Brønsted acid present therein, preferably trifluoromethanesulfonic acid. For example, the amount of potassium acetate required for neutralizing the trifluoromethanesulfonic acid present in the acetoxysiloxane in a trifluoromethanesulfonic acid solution (preferably an excess) is added thereto, salt precipitation is optionally removed, excess ethanol is added, and before the volatiles are removed, the mixture is heated to 80° C. under gentle reflux for 6 hours. The volatiles here consist in particular of the corresponding acetates of the alcohols used, which in the case of volatile alcohols can then be easily removed by distillation with excess alcohol. The residue consists of the corresponding siloxanes carrying alkoxy groups (in Example 3, siloxanes carrying ethoxy groups), such as the corresponding 29 Si NMR spectrum shown.

[0065] Thus, according to the invention, the corresponding alkoxysilanes and / or siloxanes are obtainable in a simple manner and can also be used as polymerization-active substances and, in this case, preferably with addition of suitable crosslinking catalysts, as sealants and adhesives, optionally blended with other crosslinking silanes and / or siloxanes, filled and / or unfilled with fillers and / or pigments.

[0066] In contrast, if the Bronsted acid is not neutralized, the reaction of the still Bronsted-acidic acetoxysiloxane with ethanol, for example under otherwise identical conditions, produces a mixture of chain-extended siloxanes bearing ethoxy and hydroxy groups in approximately equal proportions (see non-inventive comparative example 4).

[0067] Therefore, the present invention further provides a method for converting silanes and / or siloxanes having acetoxy groups obtained in the digestion system according to the invention into silanes and / or siloxanes having alkoxy groups, wherein:

[0068] a) the Bronsted-acidic acetoxysilane and / or acetoxysiloxane is first contacted with at least an amount of a base sufficient to neutralize the Bronsted acid,

[0069] b) optionally removing the resulting salt precipitate,

[0070] c) adding an excess of alcohol of 100% to 500%, preferably 150% to 350%, based on the acetoxy equivalents present in the acetoxysilane and / or acetoxysiloxane, and

[0071] d) exchanging the alkoxy groups with the silicon-bonded acetoxy functional groups at a temperature range of preferably 60° C. to 130° C., more preferably 70° C. to 120° C., for a period of preferably 1 to 10 hours, and

[0072] e) optionally removing the acetate obtained by distillation together with excess alcohol.

[0073] Preferably, according to the present invention, the alcohol used is preferably selected from C1-C 10 alkanols such as methanol, ethanol, 1-propanol, 2-propanol, isopropanol, 1-butanol, 2-butanol, isobutanol, tert-butanol, pentanol, hexanol, heptanol, octanol, nonanol, decanol, in each case including the isomers thereof,

[0074] and allyl alcohol, 1-hexenol, butynediol, dodecanol, stearyl alcohol, vinyloxybutanol. 2-ethylhexanol, cyclohexanol, benzyl alcohol, ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol and polyethylene glycols, 1,2-propylene glycol, dipropylene glycol and polypropylene glycols, 1,4-butanediol, 1,6-hexanediol, trimethylolpropane, glycerol, pentaerythritol, sorbitol and / or compounds with hydroxyl groups based on natural products,

[0075] More preferred are polyether alcohols or phenols, compounds having 1 to 8 phenolic OH functions, such as phenol, alkylphenols and arylphenols, bisphenol A and novolacs.

[0076] According to the invention, the alcohol is added in an excess of 100% to 500%, preferably 150% to 350%, based on the acetoxy equivalents present in the acetoxysiloxane.

[0077] The present invention further provides a method for converting siloxanes with acetoxy groups obtained in a digestion system into siloxanes with hydroxy groups, wherein these siloxanes are subjected to hydrolysis in an alkaline system. A particular embodiment of the present invention is to carry out the hydrolysis in an aqueous alkaline system, wherein the base used is an alkali metal hydroxide and / or an alkaline earth metal hydroxide and / or an alkali metal carbonate and / or a bicarbonate and / or an alkaline earth metal carbonate and / or a bicarbonate. Preferably, the aqueous alkaline system is an aqueous bicarbonate solution. The hydrolysis is preferably carried out at a temperature of ≤90° C., more preferably at a temperature of <50° C., and preferably over a period of at least 2 hours.

[0078] Another aspect of the process according to the invention is that the hydrolysis is preferably carried out in an aqueous alkaline system in such a way that the base used is added in such a way that the pH of the reaction solution during the duration of the hydrolysis does not fall below 10. In this case, the high reactivity of the acetoxysilanes and / or acetoxysiloxanes obtained by the process according to the invention facilitates their simple conversion into the corresponding hydroxy-functional silanes and / or siloxanes (here, for example, into PDM siloxanes).

[0079] From the point of view of complete recycling, the process according to the invention is also particularly attractive, since it allows simple removal and separation of fillers and pigments from a silicone matrix which has been modified with fillers and pigments and crosslinked to a high molecular weight. After carrying out the digestion according to the invention, the fillers and pigments can be separated in a very simple manner, for example by sedimentation, filtration, centrifugation, etc. (filtration in Example 5, recycling of the white bonding compound).

[0080] The invention therefore further provides for removing fillers present in the silicone to be recycled, in particular in the silicone rubber to be recycled, by sedimentation and / or filtration and / or centrifugation at the end of the digestion. DETAILED DESCRIPTION

[0081] Example

[0082] Unless otherwise expressly stated, all percentages used herein are to be understood as figures in mass percentage. In the context of the present invention, the chromatograms were dissolved in CDCl3 at 22°C and measured relative to an external standard of tetramethylsilane (TMS) [δ( 29 Si)=0.0ppm] analysis 29 Si NMR samples.

[0083] Example 1 (Invention)

[0084] An opaque silicone hose with an outer diameter of 9 mm and an inner diameter of 6 mm (from Büchi, product number: 048355) was cut into irregular geometric pieces with an average size of about 3 mm to 4 mm. 50 g of these silicone pieces were heated to 130° C. for 6 hours in a 500 ml four-necked flask with a precision glass stirrer and an overhead reflux condenser together with 50 g of decamethylcyclopentasiloxane and 12.5 g of acetic anhydride, 3.7 g of acetic acid and 0.23 g of trifluoromethanesulfonic acid. Only after about 45 minutes, the reaction mixture was an opaque homogeneous liquid without any noticeable solid components.

[0085] After the reaction mixture has cooled, record 29 Si NMR spectrum which is characteristic of linear α,ω-diacetoxypolydimethylsiloxane with all its typical signal positions.

[0086] Example 2 (Invention)

[0087] Silicone oil (polydimethylsiloxane with an average chain length of N=50) was heat treated at 130°C for 6 hours in a digestion system consisting of acetic anhydride (4.6 mol based on 1 mol of polydimethylsiloxane), acetic acid (3.0 mass % based on the total mixture) and trifluoromethanesulfonic acid (0.2 mass % based on the total mixture). The silicone obtained was 29 Si NMR spectroscopy showed the formation of acetoxy-functionalized siloxanes containing a certain proportion of trimethylsilyl acetate (derived from the trimethylsilyl end groups of the silicone oil).

[0088] Example 3 (Invention)

[0089] While stirring, 0.20 g of solid potassium acetate was added to a trifluoromethanesulfonic acid solution of 30 g of the linear α,ω-diacetoxydimethylsiloxane obtained in Example 1 in a 100 ml three-necked flask with a magnetic stirrer, an internal thermometer and an overhead reflux condenser. 14.7 ml of technical ethanol (99%, 300% stoichiometric excess) were then added and the mixture was heated to 80° C. for 6 hours so that a gentle reflux was always established. After the reaction mixture had cooled and the precipitated salts had been filtered off, the volatiles consisting of ethyl acetate and excess alcohol were removed on a rotary evaporator. The residue consisted of the corresponding ethoxy-carrying siloxane, such as the corresponding 29 Si NMR spectrum shown.

[0090] Example 4 (Invention)

[0091] While stirring, 14.7 ml of technical-grade ethanol (99%, 300% excess) were added to a trifluoromethanesulfonic acid solution of 30 g of the linear α,ω-diacetoxydimethylsiloxane obtained in Example 1 in a 100 ml three-necked flask with magnetic stirrer, internal thermometer and overhead reflux condenser, and the mixture was heated to 80° C. for 6 hours so that a gentle reflux was always established. After the reaction mixture had cooled, the volatiles consisting of ethyl acetate and excess alcohol were removed on a rotary evaporator. The residue consisted of a mixture of siloxanes carrying ethoxy groups and hydroxy groups in approximately equal proportions, which showed a chain extension based on the acetoxysilanes used, such as by the corresponding 29 Si NMR spectrum shown.

[0092] Example 5 (Invention)

[0093] First, 30 g of a fully cured silicone linking compound with white filler (MEM Universal Silicone, Indoor + Outdoor, Product No. 308226) was cut into pieces of irregular geometry with an average size of about 3-4 mm, and then 70 g of decamethylcyclopentasiloxane, 12.5 g of acetic anhydride, 3.7 g of acetic acid and 0.69 g of concentrated sulfuric acid were added thereto in a 500 ml four-necked flask with a precision glass stirrer, an internal thermometer and an overhead reflux condenser. While stirring, the reaction base was heated to 130° C. and after 30 minutes the now completely liquefied reaction mixture was contacted with another portion (40 g) of the fully cured white silicone linking compound previously cut into pieces.

[0094] After 2 hours at 130° C., the reaction mixture had assumed such a high viscosity that a further amount of acetic anhydride (12.5 g) was added.

[0095] After a further 6 hours at 130° C. and cooling to 100° C., 2.76 g of potassium acetate were introduced to neutralize the sulfuric acid. With further continuous stirring, the mixture was cooled to 25° C. and the solid was separated off with the aid of a filter press (Seitz K300 filter disc). 38.5 g of white filter residue were separated off.

[0096] Record the light yellow transparent filtrate 29 Si NMR spectrum which is characteristic of linear α,ω-diacetoxypolydimethylsiloxane with all its typical signal positions.

[0097] Example 6 (Invention)

[0098] The siloxane containing acetoxy groups obtained in Example 5 was further processed to give siloxanes carrying hydroxyl groups.

[0099] While stirring, 100 g of distilled water and 1.0 g of sodium bicarbonate (NaHCO 3 ) were added at 25° C. in a 500 ml four-necked flask with a precision glass stirrer, an internal thermometer and an overhead reflux condenser. 100 g of the clear filtrate of Example 5 were added quickly (slightly foaming) and a total of 17.2 g of sodium bicarbonate were added in portions, and the pH of the reaction medium was checked with the aid of a moist universal test paper to be about 10. Thereafter, the mixture was heated to 80° C. for 6 hours.

[0100] After cooling the mixture, the alkaline aqueous phase was separated from the silicone phase by means of a separatory funnel. The silicone phase was dried over sodium sulfate. 29 Si NMR spectroscopy confirmed the formation of linear α,ω-dihydroxypolydimethylsiloxane through its typical signal positions.

[0101] Example 7 (Invention)

[0102] Disinfection of Red Silicone Baking Trays

[0103] 90 g of a red / orange silicone baking pan (muffin pan from TEDI, product number 915270410510000000) which had been cut into irregular geometric pieces with an average size of about 3-4 mm was heated in a 500 ml four-necked flask with a precision glass stirrer, an internal thermometer and an overhead reflux condenser and heated to 120° C. while stirring with 160 g of decamethylcyclopentasiloxane, 12.5 g of acetic anhydride and 0.5 g of trifluoromethanesulfonic acid.

[0104] All silicone flakes were completely dissolved after only about 1 hour. The mixture was allowed to cool and a sample was taken, the corresponding 29 The Si NMR spectrum is characteristic of linear α,ω-diacetoxypolydimethylsiloxane with all typical signal positions.

Claims

1. A method for recycling silicone by chemically converting it into silane and / or siloxane having an acetoxy group, characterized in that: The silicone to be recycled is thermally treated in a digestion system comprising acetic anhydride and / or acetoxysiloxane and at least one Bronsted acid, and at the end of the digestion, the fillers and / or pigments present in the silicone to be recycled are removed by sedimentation and / or filtration and / or centrifugation.

2. The method according to claim 1, wherein the silicone is silicone rubber and / or silicone oil.

3. The method according to claim 1, wherein acetic acid is added to the digestion system.

4. The method according to claim 1, characterized in that The digestion system comprises: a) acetic anhydride and Bronsted acid, b) acetic anhydride, siloxane ring and / or hydroxyl functional siloxane and Bronsted acid, c) acetoxysiloxane and Bronsted acid, or d) Acetoxysiloxanes, siloxane rings and / or hydroxy-functional siloxanes, acetic anhydride and Bronsted acids.

5. The method according to claim 4, characterized in that The digestion system was in each case supplemented with acetic acid.

6. The method according to any one of claims 1 to 5, characterized in that The Bronsted acid used was a protic acid with a pKa of less than -1.

30.

7. The method according to claim 6, characterized in that The Bronsted acid used was a protic acid with a pKa of less than -2.

90.

8. The method according to claim 6, characterized in that The Bronsted acid used was a protic acid with a pKa of less than -4.

90.

9. The method according to claim 6, characterized in that The Bronsted acid used is selected from nitric acid, methanesulfonic acid, p-toluenesulfonic acid, concentrated sulfuric acid, heptafluoropropanesulfonic acid, pentafluoroethanesulfonic acid, trifluoromethanesulfonic acid, perchloric acid, chlorosulfonic acid, sulfonic acid or perfluoroalkylsulfonic acid ion exchange resin.

10. The method according to claim 6, characterized in that The Bronsted acid used is selected from perfluoroalkanesulfonic acids.

11. The method according to any one of claims 3, 5, 7-10, characterized in that: The amount of the Bronsted acid used in the digestion system is 0.1-1.5 mass % based on the total mass of the digestion system including the added acetic acid.

12. The method according to claim 11, characterized in that The amount of the Bronsted acid used in the digestion system is 0.15-1.0 mass % based on the total mass of the digestion system including the added acetic acid.

13. The method according to claim 11, characterized in that The amount of the Bronsted acid used in the digestion system is 0.2-0.8 mass % based on the total mass of the digestion system including the added acetic acid.

14. The method according to claim 3 or 5, characterized in that: The amount of acetic acid added to the digestion system is 0.5-4.0 mass % based on the total mass of the digestion system.

15. The method according to claim 14, characterized in that The amount of acetic acid added to the digestion system is 1.5-3.5 mass % based on the total mass of the digestion system.

16. The method according to any one of claims 1 to 5, 7 to 10, 12 to 13, 15, characterized in that: The heat treatment in the digestion system is carried out at standard pressure (1013 hPa), at elevated pressure or at reduced pressure.

17. The method according to claim 16, characterized in that The heat treatment in the digestion system was carried out at standard pressure.

18. The method according to any one of claims 1-5, 7-10, 12-13, 15, 17, characterized in that: The heat treatment in the digestion system is carried out in a temperature range of 50°C to 200°C.

19. The method according to claim 18, characterized in that The heat treatment in the digestion system is carried out in a temperature range of 80°C-160°C.

20. The method according to claim 18, characterized in that The heat treatment in the digestion system is carried out in the temperature range of 120-150°C.

21. The method according to claim 1, characterized in that The silicone to be recycled is silicone rubber to be recycled.

22. A method for converting silanes and / or siloxanes having acetoxy groups obtained in a digestion system according to any one of claims 1 to 21 into silanes and / or siloxanes having alkoxy groups, characterized in that: a) the Bronsted-acidic acetoxysilane and / or acetoxysiloxane is first contacted with at least an amount of a base sufficient to neutralize the Bronsted acid, b) optionally removing the resulting salt precipitate, c) adding an excess of alcohol of 100% to 500% based on the acetoxy equivalents present in the acetoxysilane and / or acetoxysiloxane, and d) exchanging the alkoxy groups with silicon-bonded acetoxy functional groups at a temperature in the range of 60°C to 130°C, and e) removing the acetate obtained, optionally by distillation together with the excess alcohol.

23. The method according to claim 22, characterized in that c) adding an excess of alcohol of 150% to 350% based on the acetoxy equivalents present in the acetoxysilane and / or acetoxysiloxane.

24. The method according to claim 22, characterized in that d) exchanging the alkoxy groups with silicon-bonded acetoxy functional groups at a temperature in the range of 70°C to 120°C.

25. The method according to claim 22, characterized in that d) exchanging the alkoxy groups with the silicon-bonded acetoxy functional groups over a period of 1 to 10 hours.

26. The method according to claim 22, characterized in that Alcohol used Selected from C1-C 10 The alkanol group, Polyether alcohol or phenol.

27. The method according to claim 26, characterized in that Alcohol used is selected from the group consisting of methanol, ethanol, 1-propanol, 2-propanol, isopropanol, 1-butanol, 2-butanol, isobutanol, tert-butanol, pentanol, hexanol, heptanol, octanol, nonanol, decanol and isomers thereof, and selected from the group comprising allyl alcohol, 1-hexenol, butynediol, dodecanol, stearyl alcohol, vinyloxybutanol, 2-ethylhexanol, cyclohexanol, benzyl alcohol, ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol and polyethylene glycol, 1,2-propylene glycol, dipropylene glycol and polypropylene glycol, 1,4-butanediol, 1,6-hexanediol, trimethylolpropane, glycerol, pentaerythritol, sorbitol and / or compounds with hydroxyl groups based on natural products, Selected from compounds having 1 to 8 phenolic OH functional groups.

28. The method according to claim 27, characterized in that The compound having 1 to 8 phenolic OH functional groups is selected from phenol, alkylphenol and arylphenol, bisphenol A and novolac.

29. A method for converting silanes and / or siloxanes having acetoxy groups obtained in a digestion system according to any one of claims 1 to 21 into silanes and / or siloxanes having hydroxyl groups, characterized in that They are subjected to hydrolysis in an alkaline system.

30. The method according to claim 29, characterized in that The base used is an alkali metal hydroxide and / or an alkaline earth metal hydroxide and / or an alkali metal carbonate and / or a bicarbonate and / or an alkaline earth metal carbonate and / or a bicarbonate.

31. The method according to claim 29, characterized in that The alkaline system is a bicarbonate aqueous solution.

32. The method according to any one of claims 29 to 31, characterized in that The hydrolysis is carried out at a temperature of ≤ 90°C.

33. The method according to claim 32, characterized in that The hydrolysis is carried out at a temperature < 50°C.

34. The method according to claim 32, characterized in that The hydrolysis is carried out over a period of at least 2 hours.