Horizontal glass anti-glare treatment system and treatment process

Through the horizontal glass anti-glare treatment system and water-soluble treatment agent, the hazardous waste and quality unstable prepared by traditional frosting powder spray is solved, and high-quality and low-waste anti-glare glass treatment is achieved. It is suitable for A variety of glass types and high-end applications.

CN112059781BActive Publication Date: 2024-11-15SUZHOU NINO CHEM MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010825925.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-17
Publication Date
2024-11-15
Estimated Expiration
2040-08-17

AI Technical Summary

Technical Problem

Traditional frosted powder spray-produced anti-glare glass has a large amount of harmful waste, complex processes and cannot be produced in standardized manner, resulting in unstable product quality and limited application in high-end fields.

Method used

Adopt a horizontal glass anti-glare treatment system, using water-soluble anti-glare treatment agent to immerse the glass, design a new process flow, including pre-throwing, water absorption, anti-glare treatment, polishing and drying, reducing solid waste and achieving standardization operate.

Benefits of technology

It reduces the amount of solid waste, improves product quality stability, avoids the "flash point" problem, is suitable for high-end fields, and expands the treatment range to 2.5D, 3D and small curve glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112059781B_ABST
    Figure CN112059781B_ABST
Patent Text Reader

Abstract

The present invention relates to a horizontal glass anti-glare treatment system, comprising a feeding mechanism, a pre-polishing mechanism, a first flushing mechanism, a water absorbing mechanism, an anti-glare treatment mechanism, a polishing mechanism, a second flushing mechanism, an air knife drying mechanism and a discharging mechanism arranged in sequence, wherein the anti-glare treatment mechanism is used to perform an immersion anti-glare treatment on the glass after absorbing water, and during the treatment process, the glass is horizontally placed on the pre-polishing mechanism, the first flushing mechanism, the water absorbing mechanism, the anti-glare treatment mechanism, the polishing mechanism, the second flushing mechanism and the air knife drying mechanism, and the glass is transmitted through a transmission mechanism. In the system, a water-soluble anti-glare treatment agent is used to perform an anti-glare treatment on the glass, and the solid waste generated during the treatment process is only about one-tenth of that of a traditional frosting powder agent, which is friendly to the human body and the environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to anti-glare glass, and in particular to a horizontal glass anti-glare processing system and a processing process. Background Art

[0002] Anti-glare glass, also known as non-reflective glass or anti-reflective glass, is a glass substrate that has undergone special surface treatment to make it have a lower reflectance than ordinary glass, which basically does not affect the transmission of light, and the light reflectance is reduced from 8% to less than 1%. Anti-glare glass can increase the viewing angle and brightness of the display, making the image clearer, the color more vivid, and the color more saturated, thereby significantly improving the display effect. It can be widely used in the production of LCD screens, rear-projection TVs, educational machine displays, mobile phone covers, electronic picture frames, and instrument display panels.

[0003] At present, frosting powder spraying is mostly used to prepare AG (anti-glare) glass. The traditional process has the following disadvantages: First, the traditional chemicals contain a large amount of hydrochloric acid, fluoride, etc., which are harmful to the human body and produce a large amount of fluorine-containing hazardous waste, with high treatment costs; second, the traditional acid etching process is complicated, production management is difficult, standardized production is impossible, quality fluctuates greatly, and the product defective rate is high; third, display panels produced by traditional processes have a "flash point" problem, which restricts their application in high-end fields. Summary of the invention

[0004] In order to overcome the above-mentioned defects, the present invention provides a horizontal glass anti-glare treatment system, in which water-soluble anti-glare treatment agents are used to treat glass for anti-glare. The solid waste generated during the treatment process is only about one-tenth of that of traditional frosting powder agents, which is friendly to the human body and the environment.

[0005] The technical solution adopted by the present invention to solve its technical problem is:

[0006] A horizontal glass anti-glare treatment system comprises a feeding mechanism, a pre-polishing mechanism, a first flushing mechanism, a water absorbing mechanism, an anti-glare treatment mechanism, a polishing mechanism, a second flushing mechanism, an air knife drying mechanism and a discharging mechanism which are arranged in sequence, wherein the feeding mechanism is used to feed the glass to the pre-polishing mechanism, the pre-polishing mechanism is used to clean and pre-polish the glass, the first flushing mechanism is used to spray and rinse the pre-polished glass for the first time, the water absorbing mechanism is used to absorb water from the rinsed glass, the anti-glare treatment mechanism is used to perform an immersion anti-glare treatment on the water-absorbed glass, the polishing mechanism is used to polish the anti-glare treated glass, the second flushing mechanism is used to spray and rinse the polished glass for the second time, the air duct drying mechanism is used to air-dry the rinsed glass, and the discharging mechanism is used to discharge the air-dried glass. During the treatment process, the glass is horizontally placed on the pre-polishing mechanism, the first flushing mechanism, the water absorbing mechanism, the anti-glare treatment mechanism, the polishing mechanism, the second flushing mechanism and the air knife drying mechanism, and the glass is transmitted through a transmission mechanism.

[0007] Preferably, the pre-polishing mechanism comprises a first pre-polishing area, a second pre-polishing area and a third pre-polishing area, and the glass located in the first pre-polishing area, the second pre-polishing area and the third pre-polishing area is cleaned and etched by spraying a pre-polishing agent.

[0008] Preferably, the first flushing mechanism includes a first flushing area, a second flushing area and a third flushing area, the second flushing mechanism includes a fourth flushing area, a fifth flushing area, a sixth flushing area and a seventh flushing area, and the water absorption mechanism includes a water absorption area, in which four sponge rollers are used to absorb water from the glass surface.

[0009] Preferably, the anti-glare treatment mechanism is provided with an anti-glare treatment tank, and a circulating water pump is provided in the anti-glare treatment tank. During treatment, the glass is horizontally immersed in the water-soluble anti-glare treatment agent in the anti-glare treatment tank.

[0010] Preferably, the polishing mechanism includes first to nineteenth polishing areas, the first, second and third polishing grooves are rough polishing areas, the fourth to nineteenth polishing areas are fine polishing areas, wherein the fourth to seventh polishing areas are a group, the eighth to eleventh polishing areas are a group, the twelfth to fifteenth polishing areas are a group, and the sixteenth to nineteenth polishing areas are a group, and the wind knife drying mechanism includes a frame, a fan and a wind knife, the wind knife is installed above and below the frame, the fan is installed outside the frame and the fan is used to supply air to the wind knife.

[0011] Preferably, an intermediate inspection area is provided between the anti-glare treatment mechanism and the polishing mechanism, the length of the pre-polishing mechanism is 1.5-2.1m, the length of the first flushing mechanism is 1-1.5m, the length of the water absorption mechanism is 0.5-0.8m, the length of the anti-glare treatment mechanism is 3-6m, the length of the polishing mechanism is 10-13m, the length of the second flushing mechanism is 1-2.1m, the length of the air knife drying mechanism is 1-1.5m, and the conveying speed of the conveying mechanism is 1-1.5m / min.

[0012] The present invention also provides a horizontal glass anti-glare treatment process, the steps are as follows:

[0013] Step 1: Pre-polishing: The glass to be processed is sent to the pre-polishing mechanism through the feeding mechanism, and the glass is sprayed with a pre-polishing agent. The pre-polishing time is 45s-90s;

[0014] Step 2: First spray rinse: The pre-polished glass is transferred to the first rinse mechanism for spray rinse with clean water. The rinse time is 45s-90s.

[0015] Step 3: Water absorption: The cleaned glass is transferred to the water absorption mechanism for water absorption. The absorption mechanism uses a sponge roller to absorb water droplets on the glass and ensure the wetness of the glass surface. The water absorption time is 20s-50s.

[0016] Step 4: Anti-glare treatment: The glass after water absorption is transferred to the anti-glare treatment mechanism for immersion anti-glare treatment using a water-soluble anti-glare treatment agent. The anti-glare treatment time is 2-5 minutes.

[0017] Step 5: Polishing: The anti-glare treated glass is sent to the polishing mechanism for spray polishing with a polishing agent. The polishing time is 6-12 minutes.

[0018] Step 6: Second spray rinse: The polished glass is transferred to the second rinse mechanism for water spray rinse, and the rinse time is 1min-2min;

[0019] Step 7: Drying and discharging: The cleaned glass is dried by air knife, and the drying time is 45s-90s; the dried glass is sent out by the discharging mechanism.

[0020] Preferably, in step one, the pre-polishing mechanism comprises a first pre-polishing zone, a second pre-polishing zone and a third pre-polishing zone, the pre-polishing agent is a mixture of hydrofluoric acid and sulfuric acid, wherein the hydrofluoric acid is 50% by mass, and the sulfuric acid is 50% by mass. The configuration method of the pre-polishing agent is as follows: 10-30 parts by weight of hydrofluoric acid, 5-15 parts by weight of sulfuric acid and 55-85 parts by weight of water are mixed;

[0021] In step 5, the polishing mechanism includes first to nineteenth polishing areas, and the glass in the first to third polishing areas is roughly polished by a polishing agent, and the glass in the fourth to nineteenth polishing areas is finely polished by a polishing agent, wherein the polishing agent is a mixture of hydrofluoric acid and sulfuric acid, wherein the hydrofluoric acid is 50% by mass, and the sulfuric acid is 50% by mass. The polishing agent is configured as follows: 20 to 35 parts by weight of hydrofluoric acid, 10 to 20 parts by weight of sulfuric acid, and 45 to 70 parts by weight of water are mixed;

[0022] In step six, the second flushing mechanism includes a fourth flushing area, a fifth flushing area, a sixth flushing area and a seventh flushing area, and the fourth flushing area, the fifth flushing area and the sixth flushing area are three-chamber circulating water spray flushing areas.

[0023] Preferably, the water-soluble anti-glare treatment agent is a mixture of component one, component two, component three, component four, component five, component six and water, wherein component one is at least one of ammonium bifluoride, ammonium fluoride, sodium fluoride, sodium bifluoride, potassium fluoride and potassium bifluoride, component two is at least one of barium chloride, calcium chloride, potassium chloride, ferric chloride and ferrous chloride, component three is at least one of ammonium sulfate, ferric sulfate, ferrous sulfate, sodium sulfate, potassium sulfate, barium nitrate and potassium nitrate, component four is citric acid or oxalic acid, component five is hydrochloric acid or sulfuric acid, and component six is ​​hydrofluoric acid or fluorosilicic acid.

[0024] Preferably, the water-soluble anti-glare treatment agent comprises the following components in parts by weight: 8-12 parts of component one, 5-10 parts of component two, 8-12 parts of component three, 20-50 parts of component four; 20-50 parts of component five, 8-12 parts of component six and 30-50 parts of water.

[0025] The beneficial effects of the present invention are:

[0026] 1) The present invention uses a novel anti-glare treatment agent, which is a fully water-soluble agent, neutral or weakly acidic, not easily volatile, and does not cause non-contact harm to the human body. The solid waste generated during the treatment process is only about one-tenth of that of the traditional frosting powder agent, and is friendly to the human body and the environment;

[0027] 2) Using the characteristics of water-soluble anti-glare treatment agents, a new treatment process is designed. The process parameters are easy to control and standardized operation can be achieved, which breaks away from the production mode that relies entirely on experience in traditional processes, improves product quality, and has high product quality stability. In the anti-glare treatment process, different formulas of potions and different process products can be used to obtain products with different roughness and haze to meet a wide range of market needs;

[0028] 3) Different from the traditional "masking method" etching, the anti-glare treatment in this process adopts chemical etching. During the etching process, a uniform chemical protective film is first formed on the glass surface, and then chemical etching is performed. The product has no "flash point", which is more conducive to the application of glass in high-end. Therefore, the products treated by the present invention cover high, medium and low application fields, such as computer mouse boards, mobile phone panels, mobile phone covers, computer display screens, car central control screens, outdoor display screens, etc.;

[0029] 4) The glass in the present invention adopts a horizontal immersion method as a supplement to the vertical immersion method. Users who currently use frosting powder spraying horizontal lines can change the traditional spraying anti-glare treatment mechanism to a horizontal immersion method, and can use the water-soluble anti-glare treatment agent in the present invention. In addition to being applicable to flat glass, the present invention can also produce 2.5D, 3D and small-curved glass, which broadens the scope of use of horizontal lines and is more suitable for the treatment of high-end products;

[0030] 5) During on-site production, the present invention does not use powdered medicines, and the feeding and discharging of medicines are automated, so that operators will not come into direct contact with the medicines. In addition, a filtering and ventilation system is provided on-site, thereby ensuring a good on-site operating environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 is a simplified diagram of the processing system in the present invention;

[0032] In the figure: 10-feeding mechanism, 20-pre-polishing mechanism, 21-first pre-polishing area, 22-second pre-polishing area, 23-third pre-polishing area, 30-first rinsing mechanism, 31-first rinsing area, 32-second rinsing area, 33-third rinsing area, 40-water absorption mechanism, 50-anti-glare treatment mechanism, 60-polishing mechanism, 70-second rinsing mechanism, 71-fourth rinsing area, 72-second rinsing area, 73-third rinsing area, 74-fourth rinsing area, 80-wind knife drying mechanism, 90-discharging mechanism. DETAILED DESCRIPTION

[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0034] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0035] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.

[0036] like Figure 1As shown, a horizontal glass anti-glare treatment system comprises a feeding mechanism 10, a pre-polishing mechanism 20, a first flushing mechanism 30, a water absorbing mechanism 40, an anti-glare treatment mechanism 50, a polishing mechanism 60, a second flushing mechanism 70, an air knife drying mechanism 80 and a discharging mechanism 90 which are arranged in sequence. The feeding mechanism 10 is used to feed the glass to the pre-polishing mechanism 20, the pre-polishing mechanism 20 is used to clean and pre-polish the glass, the first flushing mechanism 30 is used to spray and rinse the pre-polished glass for the first time, the water absorbing mechanism 40 is used to absorb water from the rinsed glass, and the anti-glare treatment mechanism 50 is used to The glass after water absorption is subjected to immersion anti-glare treatment, the polishing mechanism 60 is used to polish the glass after anti-glare treatment, the second flushing mechanism 70 is used to spray and flush the polished glass for the second time, the air duct drying mechanism 80 is used to air-dry the flushed glass, and the discharging mechanism 90 is used to discharge the air-dried glass. During the treatment process, the glass is horizontally placed on the pre-polishing mechanism 20, the first flushing mechanism 30, the water absorbing mechanism 40, the anti-glare treatment mechanism 50, the polishing mechanism 60, the second flushing mechanism 70 and the air knife drying mechanism 80, and the glass is transported through the transmission mechanism. The feeding mechanism, the pre-polishing mechanism, the first flushing mechanism, the water absorbing mechanism, the anti-glare treatment mechanism, the polishing mechanism, the second flushing mechanism, the air duct drying mechanism and the discharging mechanism are all provided with independent transmission mechanisms for the transmission of the glass. Different from the traditional spraying method, when the glass in the present invention is subjected to anti-glare treatment, the glass is immersed in a water-soluble anti-glare treatment agent, so the anti-glare treatment process is easy to control.

[0037] The pre-polishing mechanism 20 includes a first pre-polishing area 21, a second pre-polishing area 22 and a third pre-polishing area 23. The glass in the first pre-polishing area 21, the second pre-polishing area 22 and the third pre-polishing area 23 is cleaned and etched by spraying a pre-polishing agent. After the feeding mechanism delivers the glass to the pre-polishing mechanism, the feeding operation of the glass is completed. The pre-polishing mechanism is provided with a first pre-polishing area, a second pre-polishing area and a third pre-polishing area. The function of the first pre-polishing area is to apply the acid etching principle, spray a pre-polishing agent on the glass surface to clean the glass surface, so as to remove dirt on the glass surface and provide a clean etching surface for subsequent processes. The function of the second pre-polishing area and the third pre-polishing area is to use the pre-polishing agent to etch the glass surface, and form an etching honeycomb on the glass surface to improve the roughness of the glass surface; the rotation speed of the transmission roller in the transmission mechanism is controlled to control the travel speed of the glass, that is, to control the etching time.

[0038] The first flushing mechanism 30 includes a first flushing area 31, a second flushing area 32 and a third flushing area 33, the second flushing mechanism 70 includes a fourth flushing area 71, a fifth flushing area 72, a sixth flushing area 73 and a seventh flushing area 74, and the water absorbing mechanism 40 includes a water absorbing area, in which four sponge rollers are used to absorb water from the glass surface. The first flushing mechanism is used to clean the pre-polished glass to remove the pre-polishing agent remaining on the glass surface, the second flushing mechanism is used to clean the polished glass to remove the polishing agent remaining on the glass surface, and the fourth flushing area, the fifth flushing area and the sixth flushing area are three-chamber circulating water spray flushing areas; the sponge rollers are used to absorb water droplets on the glass and maintain a certain degree of wetness on the glass surface.

[0039] The anti-glare treatment mechanism 50 is provided with an anti-glare treatment tank, and a circulating water pump is provided in the anti-glare treatment tank. During treatment, the glass is horizontally immersed in the water-soluble anti-glare treatment agent in the anti-glare treatment tank. The water pump realizes the internal circulation of the water-soluble anti-glare treatment agent, and the glass is treated by immersing the water-soluble anti-glare agent, which facilitates the control of the anti-glare treatment parameters to obtain products with different roughness and haze, thereby meeting a wide range of market demands.

[0040] The polishing mechanism 60 includes the first to nineteenth polishing areas, the first, second and third polishing grooves are rough polishing areas, the fourth to nineteenth polishing areas are fine polishing areas, wherein the fourth to seventh polishing areas are a group, the eighth to eleventh polishing areas are a group, the twelfth to fifteenth polishing areas are a group, and the sixteenth to nineteenth polishing areas are a group, and the air knife drying mechanism 80 includes a frame, a fan and an air knife, the air knife is installed above and below the frame, the fan is installed outside the frame and the fan is used to supply air to the air knife. The polishing agent in each group of polishing areas can be configured to different concentrations, and multiple groups of polishing areas can be freely combined and used according to the needs of the product to improve the polishing efficiency; the air knife drying mechanism is used to air dry the cleaned glass.

[0041] A mid-inspection area is provided between the anti-glare treatment mechanism 50 and the polishing mechanism 60, the length of the pre-polishing mechanism 20 is 1.5-2.1 m, the length of the first flushing mechanism 30 is 1-1.5 m, the length of the water absorption mechanism 40 is 0.5-0.8 m, the length of the anti-glare treatment mechanism 50 is 3-6 m, the length of the polishing mechanism 60 is 10-13 m, the length of the second flushing mechanism 70 is 1-2.1 m, the length of the air knife drying mechanism 80 is 1-1.5 m, and the conveying speed of the conveying mechanism is 1-1.5 m / min. The glass after anti-glare treatment is preliminarily inspected in the intermediate inspection area. The length of each pre-polishing area is 0.5-0.7m, the length of the first rinsing area and the second rinsing area is 0.4-0.6m, the length of the third rinsing area is 0.2-0.3m, and the length of the water absorption area is 0.5-0.8m. Preferably, the length of the anti-glare treatment tank is 4-5m, and the length of each polishing area is 0.5-0.7m. The lengths of the polishing areas can be set to be the same or different as needed. The lengths of the fourth, fifth and sixth polishing areas are 0.3-0.6m, and the length of the seventh polishing area is 0.1-0.3m.

[0042] A horizontal glass anti-glare treatment process, the steps are as follows:

[0043] Step 1: Pre-polishing: The glass to be processed is sent to the pre-polishing mechanism through the feeding mechanism, and the glass is sprayed with a pre-polishing agent for a period of 45s-90s. The pre-polishing mechanism cleans and pre-polishes the glass.

[0044] Step 2: First spray rinse: The pre-polished glass is transferred to the first rinse mechanism for spray rinse with clean water. The rinse time is 45s-90s.

[0045] Step 3: Water absorption: The cleaned glass is transferred to the water absorption mechanism for water absorption. The absorption mechanism uses a sponge roller to absorb water droplets on the glass and ensure the wetness of the glass surface. The water absorption time is 20s-50s.

[0046] Step 4: Anti-glare treatment: The glass after water absorption is transferred to the anti-glare treatment mechanism for immersion anti-glare treatment using a water-soluble anti-glare treatment agent. The anti-glare treatment time is 2-5 minutes.

[0047] Step 5: Polishing: The anti-glare treated glass is sent to the polishing mechanism for spray polishing with a polishing agent. The polishing time is 6-12 minutes.

[0048] Step 6: Second spray rinse: The polished glass is transferred to the second rinse mechanism for water spray rinse, and the rinse time is 1min-2min;

[0049] Step 7: Drying and discharging: The cleaned glass is dried by air knife, and the drying time is 45s-90s; the dried glass is sent out by the discharging mechanism.

[0050] More preferably, in step 1, the pre-polishing mechanism includes a first pre-polishing zone, a second pre-polishing zone and a third pre-polishing zone, the pre-polishing agent is a mixture of hydrofluoric acid and sulfuric acid, wherein the hydrofluoric acid is 50% by mass, and the sulfuric acid is 50% by mass. The pre-polishing agent is configured as follows: 10-30 parts by weight of hydrofluoric acid, 5-15 parts by weight of sulfuric acid and 55-85 parts by weight of water are mixed;

[0051] In step 5, the polishing mechanism includes first to nineteenth polishing areas, and the glass in the first to third polishing areas is roughly polished by a polishing agent, and the glass in the fourth to nineteenth polishing areas is finely polished by a polishing agent, wherein the polishing agent is a mixture of hydrofluoric acid and sulfuric acid, wherein the hydrofluoric acid is 50% by mass, and the sulfuric acid is 50% by mass. The polishing agent is configured as follows: 20 to 35 parts by weight of hydrofluoric acid, 10 to 20 parts by weight of sulfuric acid, and 45 to 70 parts by weight of water are mixed;

[0052] In step six, the second flushing mechanism includes a fourth flushing area, a fifth flushing area, a sixth flushing area and a seventh flushing area, and the fourth flushing area, the fifth flushing area and the sixth flushing area are three-chamber circulating water spray flushing areas.

[0053] The water-soluble anti-glare treatment agent is a mixture of component one, component two, component three, component four, component five, component six and water, wherein component one is at least one of ammonium bifluoride, ammonium fluoride, sodium fluoride, sodium bifluoride, potassium fluoride and potassium bifluoride, component two is at least one of barium chloride, calcium chloride, potassium chloride, ferric chloride and ferrous chloride, component three is at least one of ammonium sulfate, ferrous sulfate, ferrous sulfate, sodium sulfate, potassium sulfate, barium nitrate and potassium nitrate, component four is citric acid or oxalic acid, component five is hydrochloric acid or sulfuric acid, and component six is ​​hydrofluoric acid or fluorosilicic acid. Further, the water-soluble anti-glare treatment agent includes the following components in parts by weight: 8-12 parts of component one, 5-10 parts of component two, 8-12 parts of component three, 20-50 parts of component four; 20-50 parts of component five, 8-12 parts of component six and 30-50 parts of water.

[0054] Embodiment and comparative example:

[0055] Example 1: The water-soluble anti-glare treatment agent of the present invention is used to treat glass, and the treatment process is as follows:

[0056] Step 1: Pre-polishing: Send the glass to be treated to the pre-polishing mechanism, and use the pre-polishing agent to spray the glass for pre-polishing. The pre-polishing time is 60s, wherein the pre-polishing agent is a mixture of hydrofluoric acid and sulfuric acid, wherein the hydrofluoric acid is 50% by mass, and the sulfuric acid is 50% by mass. The configuration method of the pre-polishing agent is as follows: 20 parts by weight of hydrofluoric acid, 10 parts by weight of sulfuric acid and 70 parts by weight of water are mixed;

[0057] Step 2: First spray rinse: The pre-polished glass is transferred to the first rinse mechanism for spray rinse with clean water for 90 seconds;

[0058] Step 3: Water absorption: The cleaned glass is transferred to the water absorption mechanism for water absorption. A sponge roller is used in the absorption mechanism to absorb water droplets on the glass and ensure the wetness of the glass surface. The water absorption time is 30 seconds.

[0059] Step 4: Anti-glare treatment: The glass after water absorption is transferred to the anti-glare treatment mechanism and subjected to immersion anti-glare treatment using a water-soluble anti-glare treatment agent. The anti-glare treatment time is 2 minutes. The water-soluble anti-glare treatment agent includes the following components in parts by weight: 5 parts of ammonium bifluoride, 5 parts of sodium fluoride, 4 parts of barium chloride, 3 parts of calcium chloride, 4 parts of ammonium sulfate, 6 parts of sodium sulfate, 30 parts of citric acid, 30 parts of hydrochloric acid, 8 parts of hydrofluoric acid and 50 parts of water.

[0060] Step 5: Polishing: The anti-glare treated glass is transferred to a polishing treatment mechanism and spray-polished with a polishing agent. The polishing time is 8 minutes. The polishing agent is a mixture of hydrofluoric acid and sulfuric acid, wherein the hydrofluoric acid is 50% by mass and the sulfuric acid is 50% by mass. The configuration method of the polishing agent is as follows: 30 parts by weight of hydrofluoric acid, 15 parts by weight of sulfuric acid and 55 parts by weight of water are mixed;

[0061] Step 6: Second spray rinse: The polished glass is transferred to the second rinse mechanism for water spray rinse, and the rinse time is 1.5 minutes;

[0062] Step 7: Drying: Use air knife to dry the cleaned glass for 60 seconds.

[0063] Example 2: The only difference from Example 1 is that the anti-glare treatment time is 2.5 minutes;

[0064] Embodiment 3: The only difference from Embodiment 1 is that the anti-glare treatment time is 3 minutes;

[0065] Example 4: The only difference from Example 1 is that the anti-glare treatment time is 3.5 minutes;

[0066] Example 5: The only difference from Example 1 is that the anti-glare treatment time is 4 minutes;

[0067] Example 6: The only difference from Example 1 is that the anti-glare treatment time is 4.5 minutes;

[0068] Example 7: The only difference from Example 1 is that the anti-glare treatment time is 5 minutes;

[0069] Comparative Example 1: The glass is treated with traditional frosting powder and traditional process, and the treatment process is as follows:

[0070] Step 1: Pretreatment: Place the glass in an ultrasonic cleaning machine and use ultrasonic cleaning on the glass;

[0071] Step 2: frosting treatment: frosting the glass by spraying sand with frosting powder, wherein the frosting powder includes the following components by weight: 30 parts of ammonium fluoride, 20 parts of potassium hydrogen fluoride, 8 parts of calcium fluoride, 15 parts of ammonium sulfate, 5 parts of barium sulfate, 8 parts of potassium sulfate and 50 parts of hydrochloric acid, and the frosting treatment time is 45 seconds;

[0072] Step 3: Cleaning: Place the glass in an ultrasonic cleaning machine and use ultrasonic cleaning on the glass;

[0073] Step 4: Liquid polishing: put the polishing liquid into the jet machine and use the jet machine to polish the glass;

[0074] Step 5: Cleaning: Place the glass in an ultrasonic cleaning machine and use ultrasonic cleaning on the glass;

[0075] Step 6: Drying: Use a baking machine to dry the glass and take it out.

[0076] Comparative Example 2: The only difference from Comparative Example 1 is that the frosting treatment time is 50S;

[0077] Comparative Example 3: The only difference from Comparative Example 1 is that the frosting treatment time is 55S;

[0078] Comparative Example 4: The only difference from Comparative Example 1 is that the frosting treatment time is 60S;

[0079] Comparative Example 5: The only difference from Comparative Example 1 is that the frosting treatment time is 65S;

[0080] Comparative Example 6: The only difference from Comparative Example 1 is that the frosting treatment time is 70 seconds;

[0081] Comparative Example 7: The only difference from Comparative Example 1 is that the frosting treatment time is 75S;

[0082] In the present embodiments 1-7 and comparative examples 1-7, display glasses are treated. The parameters of the treated glasses are as follows: roughness (Ra) of 0.1-0.2 μm, haze (H) of 10-18 degrees, and gloss (G) of 80-100 degrees. The above three indicators are tested on the treated glasses of the embodiments and comparative examples. The test results are shown in Table 1.

[0083] Roughness (Ra): measured using a Mitutoyo SJ-210 surface roughness tester produced by Japan;

[0084] Haze (H): measured using a SGW-820 transmittance / haze meter produced by Shanghai Yidian Physical Optical Instrument Co., Ltd.

[0085] Gloss (G): measured using NHG268 gloss meter produced by Shenzhen Sanenshi Technology Co., Ltd.

[0086] Table 1: Test results list

[0087] project Ra, 0.1-0.2μm H, 10-18 degrees G, 80-100 degrees Example 1 0.158 13.8 97.0 Example 2 0.147 14.2 95.3 Example 3 0.160 13.2 92.4 Example 4 0.149 15.9 89.7 Example 5 0.157 14.7 89.1 Example 6 0.169 16.6 86.5 Example 7 0.181 15.8 85.7 Comparative Example 1 0.096 9.4 106.5 Comparative Example 2 0.103 11.7 95.8 Comparative Example 3 0.124 12.5 93.7 Comparative Example 4 0.157 14.2 90.1 Comparative Example 5 0.181 15.7 82.6 Comparative Example 6 0.213 19.3 73.1 Comparative Example 7 0.259 22.9 68.4

[0088] According to the test results, Examples 1-7 can all meet the requirements of the indicators: roughness (Ra) is 0.1-0.2 μm, haze (H) is 10-18 degrees and gloss (G) is 80-100 degrees, while the results of Comparative Examples 1, 6 and 7 do not meet the set indicator requirements. The time for water-based AG treatment in Examples 1-7 is 2-5 minutes, while the time for frosting powder AG treatment in Comparative Examples 1-7 is 45-75 seconds. It can be seen that the use of traditional frosting powder for AG treatment has strict requirements on process parameters, and a difference of a few seconds may produce defective products, thereby increasing the difficulty of AG treatment. The process parameters of the treatment system of the present invention are easy to control, standardized operation can be achieved, and the qualified rate of products is improved.

[0089] It should be noted that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these modifications and improvements all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A horizontal glass anti-glare treatment system, characterized in that: The invention comprises a feeding mechanism (10), a pre-polishing mechanism (20), a first flushing mechanism (30), a water absorbing mechanism (40), an anti-glare treatment mechanism (50), a polishing mechanism (60), a second flushing mechanism (70), an air knife drying mechanism (80) and a discharging mechanism (90) which are arranged in sequence. The feeding mechanism (10) is used to feed the glass to the pre-polishing mechanism (20), the pre-polishing mechanism (20) is used to clean and pre-polish the glass, the first flushing mechanism (30) is used to spray and rinse the pre-polished glass for the first time, the water absorbing mechanism (40) is used to absorb water from the rinsed glass, and the anti-glare treatment mechanism (50) is used to dry the glass after absorbing water. The glass is subjected to an immersion anti-glare treatment, the polishing mechanism (60) is used to polish the glass after the anti-glare treatment, the second flushing mechanism (70) is used to spray and flush the polished glass for a second time, the air knife drying mechanism (80) is used to air-dry the flushed glass, and the discharging mechanism (90) is used to discharge the air-dried glass. During the treatment process, the glass is horizontally placed on the pre-polishing mechanism (20), the first flushing mechanism (30), the water absorbing mechanism (40), the anti-glare treatment mechanism (50), the polishing mechanism (60), the second flushing mechanism (70) and the air knife drying mechanism (80), and the glass is transported through the transmission mechanism; The anti-glare treatment mechanism (50) is provided with an anti-glare treatment tank, in which a circulating water pump is provided. During treatment, the glass is horizontally immersed in the water-soluble anti-glare treatment agent in the anti-glare treatment tank. The polishing mechanism (60) includes first to nineteenth polishing areas, the first, second and third polishing grooves are rough polishing areas, the fourth to nineteenth polishing areas are fine polishing areas, wherein the fourth to seventh polishing areas are a group, the eighth to eleventh polishing areas are a group, the twelfth to fifteenth polishing areas are a group, and the sixteenth to nineteenth polishing areas are a group, the air knife drying mechanism (80) includes a frame, a fan and an air knife, the air knife is installed above and below the frame, the fan is installed outside the frame and the fan is used to supply air to the air knife; A middle inspection area is provided between the anti-glare treatment mechanism (50) and the polishing mechanism (60); the length of the pre-polishing mechanism (20) is 1.5-2.1 m; the length of the first flushing mechanism (30) is 1-1.5 m; the length of the water absorption mechanism (40) is 0.5-0.8 m; the length of the anti-glare treatment mechanism (50) is 3-6 m; the length of the polishing mechanism (60) is 10-13 m; the length of the second flushing mechanism (70) is 1-2.1 m; the length of the air knife drying mechanism (80) is 1-1.5 m; and the transmission speed of the transmission mechanism is 1-1.5 m / min.

2. The horizontal glass anti-glare treatment system according to claim 1, characterized in that: The pre-polishing mechanism (20) comprises a first pre-polishing area (21), a second pre-polishing area (22) and a third pre-polishing area (23); the glass located in the first pre-polishing area (21), the second pre-polishing area (22) and the third pre-polishing area (23) is cleaned and etched by spraying a pre-polishing agent.

3. The horizontal glass anti-glare treatment system according to claim 1, characterized in that: The first flushing mechanism (30) comprises a first flushing area (31), a second flushing area (32) and a third flushing area (33); the second flushing mechanism (70) comprises a fourth flushing area (71), a fifth flushing area (72), a sixth flushing area (73) and a seventh flushing area (74); and the water absorption mechanism (40) comprises a water absorption area, in which four sponge rollers are used to absorb water from the glass surface.

4. A horizontal glass anti-glare treatment process, using the horizontal glass anti-glare treatment system according to any one of claims 1 to 3, characterized in that: Here are the steps: Step 1: Pre-polishing: The glass to be processed is sent to the pre-polishing mechanism through the feeding mechanism, and the glass is sprayed with a pre-polishing agent. The pre-polishing time is 45s-90s; Step 2: First spray rinse: The pre-polished glass is transferred to the first rinse mechanism for spray rinse with clean water. The rinse time is 45s-90s. Step 3: Water absorption: The cleaned glass is transferred to the water absorption mechanism for water absorption. The absorption mechanism uses a sponge roller to absorb water droplets on the glass and ensure the wetness of the glass surface. The water absorption time is 20s-50s. Step 4: Anti-glare treatment: The glass after water absorption is transferred to the anti-glare treatment mechanism for immersion anti-glare treatment using a water-soluble anti-glare treatment agent. The anti-glare treatment time is 2-5 minutes. Step 5: Polishing: The anti-glare treated glass is sent to the polishing mechanism for spray polishing with a polishing agent. The polishing time is 6-12 minutes. Step 6: Second spray rinse: The polished glass is transferred to the second rinse mechanism for water spray rinse, and the rinse time is 1min-2min; Step 7: Drying and discharging: The cleaned glass is dried by air knife for 45s-90s; the dried glass is sent out by the discharging mechanism.

5. The horizontal glass anti-glare treatment process according to claim 4, characterized in that: In step 1, the pre-polishing mechanism includes a first pre-polishing area, a second pre-polishing area and a third pre-polishing area, the pre-polishing agent is a mixture of hydrofluoric acid and sulfuric acid, wherein the hydrofluoric acid is 50% by mass, and the sulfuric acid is 50% by mass. The configuration method of the pre-polishing agent is as follows: 10-30 parts by weight of hydrofluoric acid, 5-15 parts by weight of sulfuric acid and 55-85 parts by weight of water are mixed; In step 5, the polishing mechanism includes first to nineteenth polishing areas, and the glass in the first to third polishing areas is roughly polished by a polishing agent, and the glass in the fourth to nineteenth polishing areas is finely polished by a polishing agent, wherein the polishing agent is a mixture of hydrofluoric acid and sulfuric acid, wherein the hydrofluoric acid is 50% by mass, and the sulfuric acid is 50% by mass. The polishing agent is configured as follows: 20 to 35 parts by weight of hydrofluoric acid, 10 to 20 parts by weight of sulfuric acid, and 45 to 70 parts by weight of water are mixed; In step six, the second flushing mechanism includes a fourth flushing area, a fifth flushing area, a sixth flushing area and a seventh flushing area, and the fourth flushing area, the fifth flushing area and the sixth flushing area are three-chamber circulating water spray flushing areas.

6. The horizontal glass anti-glare treatment process according to claim 5, characterized in that: The water-soluble anti-glare treatment agent is a mixture of component one, component two, component three, component four, component five, component six and water, wherein component one is at least one of ammonium bifluoride, ammonium fluoride, sodium fluoride, sodium bifluoride, potassium fluoride and potassium bifluoride, component two is at least one of barium chloride, calcium chloride, potassium chloride, ferric chloride and ferrous chloride, component three is at least one of ammonium sulfate, ferric sulfate, ferrous sulfate, sodium sulfate, potassium sulfate, barium nitrate and potassium nitrate, component four is citric acid or oxalic acid, component five is hydrochloric acid or sulfuric acid, and component six is ​​hydrofluoric acid or fluorosilicic acid.

7. The horizontal glass anti-glare treatment process according to claim 6, characterized in that: The water-soluble anti-glare treatment agent comprises the following components in parts by weight: 8-12 parts of component one, 5-10 parts of component two, 8-12 parts of component three, 20-50 parts of component four, 20-50 parts of component five, 8-12 parts of component six and 30-50 parts of water.