Semiconductor structure and method for forming the same
By forming a polymer layer on top of the dielectric layer and combining it with a dry etching process, the dielectric layer is protected from damage, thus solving the etching problem of the dielectric layer during the sidewall removal process in semiconductor structures and improving the formation quality of metal gate structures.
Patent Information
- Application Number
- CN202010398232.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-06-14
- Filing Date
- 2020-05-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-05-12
AI Technical Summary
In the prior art, during the etching process of removing part of the sidewalls in a semiconductor structure, the dielectric layer is easily damaged, affecting the formation quality of the metal gate structure.
A polymer layer is formed on the top surface of the dielectric layer to protect it from etching. The sidewalls are gradually removed using a dry etching process to ensure the integrity of the dielectric layer, and a metal gate structure is filled into the groove.
It effectively protects the dielectric layer from etching, ensures the integrity and filling quality of the metal gate structure, and improves the performance of the semiconductor structure.
Smart Images

Figure CN112086349B_ABST
Abstract
Description
[0001] This application claims the priority of the Chinese patent application filed with the China Patent Office on June 14, 2019, with application number 2019105178272 and invention name “Semiconductor structure and method for forming the same”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present invention relates to the field of semiconductor manufacturing technology, and in particular to a semiconductor structure and a forming method thereof. Background Art
[0003] The miniaturization of transistor size is a trend in the development of semiconductor structures. However, the continuous reduction in the size of transistors also brings about a series of technical problems. For example, the gate dielectric layer is too thin, resulting in a high leakage current between the gate and the channel, and the size reduction causes a significant increase in the resistance of the polysilicon gate.
[0004] Researchers have found that transistors made of high-k metal gate (HKMG) transistors can effectively solve the above problems by replacing silicon oxide or silicon oxynitride materials with high-k gate dielectric layers and replacing traditional polysilicon gate materials with metal gates. On the one hand, the high-k gate dielectric layer can reduce the tunneling current between the gate and the channel; on the other hand, the resistivity of the metal gate is extremely small, which can effectively prevent the increase of gate resistance.
[0005] However, the performance of semiconductor structures in the prior art still needs to be improved. Summary of the invention
[0006] The problem solved by the present invention is to provide a semiconductor structure and a method for forming the same, which can protect the dielectric layer and prevent the dielectric layer from being etched during the process of removing part of the sidewall.
[0007] To solve the above problems, the present invention provides a method for forming a semiconductor structure, comprising: providing a substrate, on which a dielectric layer is formed, wherein the dielectric layer has a groove and a sidewall located on the sidewall of the groove; forming a polymer layer on the top surface of the dielectric layer; after forming the polymer layer, removing part of the sidewall located on the sidewall of the groove.
[0008] Optionally, the substrate is a base; or the substrate is: a base and fins separated from each other on the base.
[0009] Optionally, in the step of providing a substrate, a plurality of discretely arranged gates are also formed on the substrate, the gates fill the grooves, the tops of the gates are lower than the tops of the dielectric layer, and the sidewalls of the grooves expose the sidewalls; in the process of removing a portion of the sidewalls located on the sidewalls of the grooves, the sidewalls exposed by the sidewalls of the grooves are removed.
[0010] Optionally, the steps of forming the gate, the side wall, the dielectric layer and the groove are: forming a plurality of discretely arranged gates on the substrate; forming a side wall on the side wall of the gate; filling a dielectric layer between adjacent gates, the dielectric layer covering the side wall, adjacent dielectric layers surrounding the groove, and the gate filling the groove; etching to remove part of the thickness of the gate.
[0011] Optionally, the steps of forming the gate, the side wall, the dielectric layer and the groove are: forming a dielectric layer covering the surface of the substrate; etching the dielectric layer to form a groove in the dielectric layer; forming a side wall on the side wall of the groove; filling the groove to form a gate; and etching to remove part of the thickness of the gate.
[0012] Optionally, the process gas for forming the polymer layer includes silicon tetrachloride, oxygen and methyl fluoride.
[0013] Optionally, the thickness of the polymer layer is 1 nm to 5 nm.
[0014] Optionally, a dry etching process is used to remove the sidewalls exposed by the sidewalls of the groove.
[0015] Optionally, the process parameters of the dry etching process include: the process gas includes silicon tetrachloride, oxygen, fluoromethane and helium, the flow rate of the process gas is 100 sccm to 800 sccm, and the pulse power is 200W to 800W.
[0016] Optionally, the process parameters of the dry etching process include: the process gas includes silicon tetrachloride, hydrogen, nitrogen trifluoride and helium, the flow rate of the process gas is 100 sccm to 800 sccm, and the pulse power is 200W to 800W.
[0017] Optionally, after removing part of the side wall located on the side wall of the groove, the opening size of the groove gradually decreases along the top of the groove toward the bottom of the groove.
[0018] Optionally, in the process of forming the side wall, the side wall includes a first side wall and a second side wall, the first side wall covers the side wall of the dielectric layer, and the first side wall is located between the second side wall and the dielectric layer.
[0019] Optionally, in the process of removing a portion of the sidewalls located on the sidewalls of the groove, all of the second sidewalls exposed by the sidewalls of the groove are removed by etching, and the first sidewalls exposed by the sidewalls of the groove are retained.
[0020] Optionally, the steps of forming the polymer layer and removing the second sidewall exposed by the sidewall of the groove are repeated until the second sidewall exposed by the sidewall of the groove is completely removed.
[0021] Optionally, the process of removing a portion of the sidewall located on the sidewall of the groove further includes: etching and removing a portion of the first sidewall exposed by the sidewall of the groove.
[0022] Optionally, after removing part of the side wall located on the side wall of the groove, the remaining first side wall exposed by the side wall of the groove is in an arc shape, and the groove has a trumpet-shaped opening; or, the remaining first side wall exposed by the side wall of the groove is in a slope shape, and the groove has an inverted trapezoidal opening.
[0023] Optionally, in the process of removing a portion of the sidewalls on the sidewalls of the groove, all of the second sidewalls and all of the first sidewalls exposed by the sidewalls of the groove are removed by etching.
[0024] Optionally, the steps of forming the polymer layer and removing the second sidewall and the first sidewall exposed by the sidewall of the groove are cyclically performed until the second sidewall and the first sidewall exposed by the sidewall of the groove are completely removed.
[0025] Optionally, the process of removing a portion of the sidewall located on the sidewall of the groove further includes: etching and removing a portion of the sidewall of the dielectric layer exposed by the sidewall of the groove.
[0026] Optionally, after removing the second side wall and the first side wall exposed by the groove side wall, the remaining side wall of the dielectric layer exposed by the groove side wall is in an arc shape, and the groove has a trumpet-shaped opening; or, the remaining side wall of the dielectric layer exposed by the groove side wall is in an inclined shape, and the groove has an inverted trapezoidal opening.
[0027] Correspondingly, the present invention also provides a semiconductor structure formed by the above method, comprising: a substrate; a dielectric layer located on the substrate, the dielectric layer having a groove and a sidewall located on the sidewall of the groove, and the opening size of the top of the groove is larger than the opening size of the bottom of the groove.
[0028] Optionally, the substrate is a base; or the substrate is: a base and fins separated from each other on the base.
[0029] Optionally, the side wall includes a first side wall and a second side wall, the first side wall covers the side wall of the dielectric layer, and the first side wall is located between the second side wall and the dielectric layer.
[0030] Optionally, the first sidewall spacer covers the sidewall surface of the dielectric layer, and the top of the second sidewall spacer is lower than the top of the first sidewall spacer.
[0031] Optionally, the side wall of the first side wall higher than the second side wall is in an arc shape, and the groove is in a trumpet-shaped opening; or, the side wall of the first side wall higher than the second side wall is in an inclined shape, and the groove is in an inverted trapezoidal opening.
[0032] Optionally, the first sidewall exposes a portion of the sidewall of the dielectric layer, and the top of the second sidewall is flush with the top of the first sidewall.
[0033] Optionally, the dielectric layer sidewall exposed by the first sidewall is in an arc shape, and the groove has a trumpet-shaped opening; or, the dielectric layer sidewall exposed by the groove sidewall is in an inclined shape, and the groove has an inverted trapezoidal opening.
[0034] Compared with the prior art, the technical solution of the present invention has the following advantages:
[0035] Before removing the portion of the sidewall located on the sidewall of the groove, a polymer layer is formed on the top surface of the dielectric layer to isolate the top surface of the dielectric layer from the etching process environment, thereby protecting the top surface of the dielectric layer and preventing the top surface of the dielectric layer from being etched. Subsequently, the gate is removed and a metal gate structure is filled in the groove. Protecting the top surface of the dielectric layer helps to prevent the height of the metal gate structure from being reduced, thereby improving the formation quality of the metal gate structure.
[0036] In an optional solution, after removing part of the side wall located on the side wall of the groove, the opening size of the groove gradually decreases along the top of the groove toward the bottom of the groove. Subsequently, the gate is removed and a metal gate structure is filled in the groove. The metal gate structure is easy to fill in the groove, which is beneficial to further improve the filling quality of the metal gate structure and reduce the pores formed in the metal gate structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 and Figure 2 It is a schematic structural diagram corresponding to each step in a method for forming a semiconductor structure;
[0038] Figures 3 to 12 is a schematic structural diagram corresponding to each step in the first embodiment of the semiconductor structure forming method of the present invention;
[0039] Figures 13 to 20 is a schematic structural diagram corresponding to each step in the second embodiment of the semiconductor structure forming method of the present invention;
[0040] Figure 21 to Figure 29 is a schematic structural diagram corresponding to each step in the third embodiment of the semiconductor structure forming method of the present invention;
[0041] Fig.30 is a structural schematic diagram of an embodiment of a method for forming a semiconductor structure of the present invention;
[0042] Fig.31 It is a structural schematic diagram of another embodiment of the semiconductor structure forming method of the present invention. DETAILED DESCRIPTION
[0043] Now we analyze it in combination with a method for forming a semiconductor structure, referring to Figure 1 The process steps for forming the semiconductor structure include: providing a substrate 10; forming a dielectric layer 20 on the substrate 10; forming a groove 21 in the dielectric layer 20; forming a sidewall 30 on the sidewall of the groove 21; forming a gate 40 in the groove 21, wherein the top of the gate 40 is lower than the top of the dielectric layer 20; referring to Figure 2 , remove part of the side wall 30 located on the side wall of the groove 21.
[0044] In the process of removing part of the sidewall 30, the etching selectivity of the etching process to the sidewall 30 and the dielectric layer 20 is not high enough, resulting in the surface of the dielectric layer 20 being etched. Figure 1 As shown, before removing part of the sidewall 30, the thickness of the dielectric layer 20 is H1. Figure 2 As shown, after a portion of the sidewall 30 is removed, the thickness of the dielectric layer 20 is H2, where H2 is less than H1.
[0045] The inventors have studied the method for forming the above-mentioned semiconductor structure. Through creative work, the inventors noticed that by forming a polymer layer on the top surface of the dielectric layer, the top surface of the dielectric layer can be protected, thereby preventing the dielectric layer surface from being etched.
[0046] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0047] Figures 3 to 12 It is a schematic structural diagram corresponding to each step in the first embodiment of the semiconductor structure forming method of the present invention.
[0048] refer to Figure 3 and Figure 4 , Figure 4 yes Figure 3 The cross-sectional structural diagrams along the A1A2 cut lines respectively provide a substrate 101 , wherein the substrate 101 is a base; or the substrate 101 is: a base and a discrete fin 110 located on the base.
[0049] In this embodiment, the substrate 101 is used to form a FinFET, and the substrate 101 includes a base and a discrete fin 110 located on the base. The base provides a process platform for the subsequent formation of the FinFET, and the fin 110 provides a channel for the formed FinFET.
[0050] The material of the substrate is silicon, germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium. In this embodiment, the substrate is a silicon substrate.
[0051] The material of the fin 110 is the same as that of the substrate. In this embodiment, the material of the fin 110 is silicon. In other embodiments, the material of the fin may also be germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium.
[0052] In this embodiment, after the fin 110 is formed, the method further includes: forming a pad oxide layer 120 on the top and sidewall of the fin 110 and the substrate where the fin 110 is exposed.
[0053] The formation process of the pad oxide layer 120 includes a deposition process or an oxidation process.
[0054] In this embodiment, after the liner oxide layer 120 is formed, the method further includes: forming an isolation structure 130 between adjacent fins 110 , wherein the isolation structure 130 covers a portion of the sidewalls of the fins 110 .
[0055] The pad oxide layer 120 can enhance the interface bonding strength between the isolation structure 130 and the fin 110 .
[0056] In this embodiment, the material of the isolation structure 130 is silicon oxide. In other embodiments, the material of the isolation structure may also be silicon nitride or silicon oxynitride.
[0057] The isolation structure 130 serves to isolate adjacent fins 110 and is used to isolate adjacent devices.
[0058] The steps of forming the isolation structure 130 include: filling an isolation film (not shown) between adjacent fins 110, wherein the top of the isolation film is higher than the top of the fin 110; grinding and removing the isolation film above the top of the fin 110; etching back a portion of the remaining isolation film to expose the top and part of the side wall of the fin 110, thereby forming the isolation structure 130.
[0059] refer to Figure 5 After forming the isolation structure 130 , a plurality of gates 410 are formed which are arranged discretely and cross the fin 110 .
[0060] In this embodiment, the semiconductor structure is formed by a gate-last process, and the gate 410 is a dummy gate structure. The gate 410 occupies a space position for a metal gate structure formed subsequently.
[0061] The gate 410 is a single-layer structure or a stacked structure. In this embodiment, the gate 410 is a single-layer structure, and the gate 410 includes a dummy gate layer, and the material of the dummy gate layer is polysilicon, silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, silicon carbonitride, silicon carbon nitride or amorphous carbon.
[0062] In other embodiments, the gate is a stacked structure, the gate includes a dummy oxide layer and a dummy gate layer located on the dummy oxide layer, and the material of the dummy oxide layer is silicon oxide or silicon oxynitride.
[0063] In this embodiment, the steps of forming the gate 410 include: forming a dummy gate film (not marked) on the isolation structure 130; forming a gate mask (not marked) on the surface of the dummy gate film, wherein the gate mask defines the pattern of the dummy gate structure to be formed; using the gate mask as a mask, patterning the dummy gate film, and forming the gate 410 on the isolation structure 130.
[0064] refer to Figure 6 , forming a sidewall spacer 330 on the sidewall of the gate 410 .
[0065] The sidewall spacer 330 is used to define the position of the doped epitaxial layer in the subsequent process, and can protect the sidewall of the metal gate structure in the subsequent process.
[0066] The sidewall spacer 330 may be a single-layer structure or a stacked structure. In this embodiment, the sidewall spacer 330 is a stacked structure, and includes a first sidewall spacer 331 and a second sidewall spacer 332 , wherein the second sidewall spacer 332 covers the sidewall of the gate 410 , and the first sidewall spacer 331 covers the sidewall of the second sidewall spacer 332 .
[0067] In this embodiment, the step of forming the sidewall 330 includes: forming a second sidewall film (not marked) covering the top, sidewall and top of the isolation structure 130 of the gate 410; forming a first sidewall film (not marked) conformally covering the second sidewall film; removing the second sidewall film and the first sidewall film on the top of the gate 410 and the top of the isolation structure 130; retaining the second sidewall film and the first sidewall film located on the sidewall of the gate 410, and the remaining second sidewall film serves as the second sidewall 332, and the remaining first sidewall film serves as the first sidewall 331.
[0068] The material of the sidewall spacer 330 may be silicon oxide, silicon nitride, silicon carbide, silicon carbonitride, silicon carbonitride oxide, silicon nitride oxide, boron nitride or boron carbonitride. In this embodiment, the material of the second sidewall spacer 332 is silicon nitride, and the material of the first sidewall spacer 331 is silicon carbonitride oxide.
[0069] refer to Figure 7A dielectric layer 220 is filled between adjacent gate electrodes 410 , the dielectric layer 220 covers the sidewalls of the spacer 330 , and adjacent dielectric layers 220 form a groove, which is fully filled with the gate electrodes 410 .
[0070] In this embodiment, the step of forming the dielectric layer 220 includes: forming a dielectric film (not shown) covering the top of the gate 410, the top of the fin 110 and the top of the isolation structure 130; grinding and removing the dielectric film above the top of the gate 410, and the remaining dielectric film serves as the dielectric layer 220.
[0071] In this embodiment, the material of the dielectric layer 220 is silicon oxide. In other embodiments, the material of the dielectric layer may also be silicon nitride, silicon carbide, silicon carbonitride, silicon carbonitride oxide, silicon nitride oxide, boron nitride or boron carbonitride.
[0072] In this embodiment, a chemical vapor deposition process is used to form the dielectric layer 220. In other embodiments, a physical vapor deposition process or an atomic layer deposition process may also be used to form the dielectric layer.
[0073] refer to Figure 8 , etching to remove a portion of the thickness of the gate 410 .
[0074] Part of the thickness of the gate 410 is removed by etching, and the sidewalls of the groove 230 are exposed to expose the sidewalls of the sidewalls 330 , which is convenient for the subsequent removal of part of the sidewalls 330 to increase the opening width of the groove 230 and facilitate the subsequent filling of the metal gate structure in the groove 230 .
[0075] After etching away a portion of the thickness of the gate 410, the remaining gate 410 still covers a portion of the top surface and the sidewall surface of the fin 110. If the thickness of the gate 410 removed by etching is too small, the remaining top surface of the gate 410 is too much higher than the top of the fin 110, and the sidewall 330 is subsequently exposed by etching, the volume increase of the groove 230 is small, which affects the effect of reducing the difficulty of the subsequent filling process of the metal gate structure; if the thickness of the gate 410 removed by etching is too large, the remaining top surface of the gate 410 is too little higher than the top of the fin 110, and the sidewall 330 is subsequently exposed by etching, the gate 410 is removed, and the metal gate structure is filled, and the remaining sidewall 330 covers a small area of the sidewall of the metal gate structure, which affects the protection effect of the sidewall 330 on the sidewall surface of the metal gate structure; in this embodiment, the remaining top surface of the gate 410 is higher than the top of the fin 110.
[0076] In this embodiment, a dry etching process is used to remove a portion of the gate 410. The dry etching process has a high selectivity between the gate 410 material and the dielectric layer 220 material, so the top surface of the dielectric layer 220 is not easily etched in the dry etching process.
[0077] In another embodiment, a wet etching process is used to remove a portion of the thickness of the gate 410 .
[0078] refer to Fig. 9 , a polymer layer 510 is formed on the top surface of the dielectric layer 220 .
[0079] In the subsequent process of etching the side wall 330, the polymer layer 510 can protect the top surface of the dielectric layer 220, prevent the top surface of the dielectric layer 220 from being etched, and prevent the top etching of the dielectric layer 220 from causing the depth of the groove 230 to decrease, thereby ensuring that the height of the subsequently formed metal gate structure meets the process requirements.
[0080] In this embodiment, the process gas for forming the polymer layer 510 includes silicon tetrachloride, oxygen and methyl fluoride. The polymer layer 510 is a chemical reaction product of silicon tetrachloride, oxygen and methyl fluoride.
[0081] On the one hand, the polymer layer 510 is easily adsorbed on a flat surface, so most of the polymer layer 510 is located on the top surface of the dielectric layer 220. The rest of the polymer layer 510 is mainly located on the top surface of the gate 410. On the other hand, at the side wall of the side wall 330, due to the high inclination, the polymer layer 510 is difficult to adsorb, so the content of the polymer layer 510 on the side wall surface of the side wall 330 is small and can even be ignored. In addition, since the top surface of the side wall 330 is adjacent to the groove 230, the difficulty of adsorbing the polymer layer 510 is between the above two aspects, so a small part of the polymer layer 510 can be adsorbed on the top surface of the side wall 330.
[0082] If the thickness of the polymer layer 510 located on the top surface of the dielectric layer 220 is too large, correspondingly, the content of the polymer layer 510 located on the side wall surface of the side wall 330 is too large, resulting in a large difficulty in the subsequent process of removing the side wall 330. If the thickness of the polymer layer 510 located on the top of the dielectric layer 220 is too small, the protective effect of the polymer layer 510 on the top surface of the dielectric layer 220 is affected. When the side wall 330 is removed later, the top surface of the dielectric layer 220 is easily etched. In this embodiment, the thickness of the polymer layer 510 is 1nm to 5nm.
[0083] refer to Fig.10 and Fig.11, remove the sidewall 330 exposed by the sidewall of the groove 230.
[0084] The gate 410 is subsequently removed to form a metal gate structure that fills the groove 230. Removing the sidewall 330 exposed by the sidewall of the groove 230 can increase the opening width of the groove 230, further expand the accommodation space for the metal gate structure, and facilitate the subsequent filling of the metal gate structure in the groove 230.
[0085] In this embodiment, in the process of removing the sidewall 330 exposed by the sidewall of the groove 230 , all of the second sidewall 332 exposed by the sidewall of the groove 230 are removed by etching, and the first sidewall 331 is retained.
[0086] In this embodiment, a dry etching process is used to remove the second sidewall 332 exposed by the sidewall of the groove 230 . In other embodiments, a wet etching process may also be used.
[0087] like Fig.10 As shown, in this embodiment, during the dry etching process, the etching gas includes a high-energy plasma 610. The plasma 610 enters the groove 230, and the speed direction of the plasma 610 is changed to the side wall of the second sidewall 332, thereby bombarding the side wall surface of the second sidewall 332 exposed by the gate 410, thereby removing the second sidewall 332 above the top of the gate 410.
[0088] During the dry etching process, part of the plasma 610 bombards the polymer layer 510, and the polymer layer 510 can play a buffering role, reducing the bombardment speed of the plasma 610, thereby reducing the force of the plasma 610 on the top surface of the dielectric layer 220. Therefore, the polymer layer 510 can protect the top surface of the dielectric layer 220 and prevent the top surface of the dielectric layer 220 from being etched.
[0089] In this embodiment, the polymer layer 510 located on the surface of the gate 410 can also protect the surface of the gate 410 .
[0090] In this embodiment, the process parameters of the dry etching process include: the process gas includes silicon tetrachloride, oxygen, fluoromethane and helium, and the flow rate of the process gas is 100 sccm to 800 sccm.
[0091] In the dry etching process, the bombardment speed and direction of the plasma 610 are related to the pulse power. If the pulse power is too small, the bombardment speed of the plasma 610 is small, the direction of the plasma 610 is too dispersed, and the plasma 610 is difficult to etch and remove the sidewall 330 exposed by the gate 410. In this embodiment, the pulse power is 200W to 800W, the bombardment speed of the plasma 610 is appropriate, and the movement direction is concentrated, which can improve the efficiency of removing part of the sidewall 330.
[0092] In other embodiments, the process parameters of the dry etching process include: the process gas includes silicon tetrachloride, hydrogen, nitrogen trifluoride and helium, the flow rate of the process gas is 100 sccm to 800 sccm, and the pulse power is 200W to 800W.
[0093] Combined with reference Figures 9 to 11 In this embodiment, the process of removing the second sidewall 332 exposed by the sidewall of the groove 230 is performed in multiple steps. Before each step, a step of forming a polymer layer 510 on the top surface of the dielectric layer 220 is performed. The steps of forming the polymer layer 510 and removing the second sidewall 332 exposed by the sidewall of the groove 230 are performed repeatedly until the second sidewall 332 exposed by the sidewall of the groove 230 is completely removed, and the top of the remaining second sidewall 332 is flush with the top of the gate 410.
[0094] Under the continuous bombardment of the plasma 610, the thickness of the polymer layer 510 will be reduced, so that the protective effect of the polymer layer 510 on the top surface of the dielectric layer 220 is weakened. Therefore, the process of etching the second side wall 332 exposed by the side wall of the groove 230 is carried out in multiple steps, and the polymer layer 510 is re-formed on the top surface of the dielectric layer 220 to make up for the loss of the polymer layer 510, thereby ensuring the protective effect of the polymer layer 510.
[0095] In another embodiment, after the step of forming a polymer layer on the top surface of the dielectric layer is performed once, all of the second sidewall spacers exposed by the sidewalls of the groove are removed by etching.
[0096] like Fig.11 As shown, in this embodiment, the process of removing the exposed sidewall 330 of the groove 230 further includes: etching and removing a portion of the exposed sidewall of the first sidewall 331 .
[0097] In this embodiment, after the second sidewall 332 exposed by the sidewall of the groove 230 is etched, the first sidewall 331 is further exposed, and the plasma 610 (refer to Fig.10) further bombards the exposed sidewall of the first sidewall 331. In the same time, the closer to the top of the groove 230, the greater the etching amount of the sidewall of the first sidewall 331, so that from the top to the bottom of the groove 230, the opening size of the groove 230 gradually decreases, that is, the width of the groove 230 parallel to the extension direction of the fin 110 gradually decreases.
[0098] The opening size of the groove 230 gradually decreases from the top to the bottom of the groove 230, which facilitates the subsequent filling of the metal gate structure in the groove 230, helps to further improve the filling quality of the metal gate structure, and reduces the pores formed in the metal gate structure.
[0099] In this embodiment, after the process of removing the side wall 330 exposed by the side wall of the groove 230 is completed, the remaining side wall of the first side wall 331 exposed by the side wall of the groove 230 is in an arc shape, so that the groove 230 has a trumpet-shaped opening, thereby, along the top of the groove 230 pointing to the bottom of the groove 230, the opening size of the groove 230 gradually decreases.
[0100] In another embodiment, after the process of removing the side wall 330 exposed by the side wall of the groove 230 is completed, the remaining side wall of the first side wall 331 exposed by the side wall of the groove 230 is inclined, so that the groove 230 has an inverted trapezoidal opening, thereby, the opening size of the groove 230 gradually decreases from the top of the groove 230 to the bottom of the groove 230.
[0101] Fig.12 It is a schematic diagram of the corresponding structure after the process of removing the sidewall 330 exposed by the sidewall of the groove 230 is completed in other embodiments.
[0102] refer to Fig.12 In other embodiments, in the process of removing the sidewall 330 exposed by the sidewall of the groove 230 , all of the second sidewall 332 and all of the first sidewall 331 exposed by the sidewall of the groove 230 are etched away.
[0103] The etching process adopts a dry etching process or a wet etching process.
[0104] The process of removing the second sidewall 332 and the first sidewall 331 exposed by the sidewall of the groove 230 is performed in multiple steps, and before each step, a step of forming a polymer layer 510 on the top surface of the dielectric layer 220 is performed. The steps of forming the polymer layer 510 and removing the second sidewall 332 and the first sidewall 331 exposed by the sidewall of the groove 230 are performed cyclically until the second sidewall 332 and the first sidewall 331 exposed by the sidewall of the groove 230 are completely removed, and the remaining top of the second sidewall 332 and the remaining top of the first sidewall 331 are flush with the top of the gate 410.
[0105] The steps of forming the polymer layer 510 and removing the second sidewall 332 and the first sidewall 331 exposed by the sidewall of the groove 230 are cyclically performed to replenish the polymer layer 510 on the top surface of the dielectric layer 220 in time to prevent the top surface of the dielectric layer 220 from being etched.
[0106] In another embodiment, after the step of forming a polymer layer on the top surface of the dielectric layer is performed once, all of the second sidewall spacer and the first sidewall spacer exposed by the sidewall of the groove are removed by etching.
[0107] Continue to refer Fig.12 In the process of removing the sidewall 330 exposed by the sidewall of the groove 230, the process further includes: etching and removing the exposed part of the sidewall of the dielectric layer 220.
[0108] Specifically, after the second sidewall 332 and the first sidewall 331 exposed by the sidewall of the groove 230 are etched, the sidewall of the dielectric layer 220 is further exposed, and the plasma 610 entering the groove 230 further bombards the exposed sidewall of the dielectric layer 220. In the same time, the closer to the top of the groove 230, the greater the etching amount of the sidewall of the dielectric layer 220, and the opening size of the groove 230 gradually decreases from the top of the groove 230 to the bottom of the groove 230, that is, the width of the groove 230 parallel to the extension direction of the fin 110 gradually decreases.
[0109] The opening size of the groove 230 gradually decreases from the top to the bottom of the groove 230 , which helps to further reduce the difficulty of the subsequent process of filling the metal gate structure in the groove 230 and improve the filling quality of the metal gate structure.
[0110] In this embodiment, after the process of removing the side wall 330 exposed by the side wall of the groove 230 is completed, the remaining side wall of the dielectric layer 220 exposed by the side wall of the groove 230 is in an arc shape, so that the groove 230 has a trumpet-shaped opening, thereby gradually reducing the opening size of the groove 230 from the top to the bottom of the groove 230.
[0111] In another embodiment, after the process of removing the side wall 330 exposed by the side wall of the groove 230 is completed, the remaining side wall of the dielectric layer 220 exposed by the side wall of the groove 230 is inclined, so that the groove 230 has an inverted trapezoidal opening, thereby, the opening size of the groove 230 gradually decreases from the top of the groove 230 to the bottom of the groove 230.
[0112] Figures 13 to 20 It is a schematic structural diagram corresponding to each step in the second embodiment of the semiconductor structure forming method of the present invention.
[0113] refer to Fig.13 , providing a substrate 100.
[0114] The material of the substrate 100 is silicon, germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium. In this embodiment, the substrate 100 is a silicon substrate.
[0115] refer to Fig.14 , a dielectric layer 200 is formed on the substrate 100 .
[0116] In this embodiment, the material of the dielectric layer 200 is silicon oxide. In other embodiments, the material of the dielectric layer may also be silicon nitride, silicon carbide, silicon carbonitride, silicon carbonitride oxide, silicon nitride oxide, boron nitride or boron carbonitride.
[0117] In this embodiment, the dielectric layer 200 is formed by chemical vapor deposition process. In other embodiments, the dielectric layer 200 may be formed by physical vapor deposition process or atomic layer deposition process.
[0118] refer to Fig.15 , a groove 210 is formed in the dielectric layer 200 .
[0119] In this embodiment, the depth of the groove 210 is equal to the thickness of the dielectric layer 200. The bottom of the groove 210 is exposed from the surface of the substrate 100. In other embodiments, the depth of the groove may be less than the thickness of the dielectric layer.
[0120] In this embodiment, the process steps for forming the groove 210 include: forming a patterned layer (not shown in the figure) on the top of the dielectric layer 200, wherein the patterned layer exposes a portion of the surface of the dielectric layer 200; using the patterned layer as a mask, etching the dielectric layer 200 until the surface of the substrate 100 is exposed to form the groove 210.
[0121] In this embodiment, a dry etching process is used to etch the dielectric layer 200. In other embodiments, a wet etching process may also be used to etch the dielectric layer.
[0122] In this embodiment, the number of the grooves 210 is two. In other embodiments, the number of the grooves may also be one, or greater than two.
[0123] refer to Fig.16 , a sidewall 300 is formed on the sidewall of the groove 210 .
[0124] In this embodiment, the sidewall 300 is located on the sidewall and bottom surface of the groove 210 .
[0125] The sidewall 300 is a single-layer structure or a multi-layer structure. In this embodiment, the sidewall 300 has two layers. The sidewall 300 includes a first sidewall 310 and a second sidewall 320, wherein the first sidewall 310 is located between the second sidewall 320 and the dielectric layer 200. The first sidewall 310 covers the sidewall and bottom surface of the groove 210, and the second sidewall 320 covers the surface of the first sidewall 310.
[0126] The material of the first sidewall spacer 310 is silicon oxide, silicon nitride, silicon oxynitride or silicon oxycarbonitride. In this embodiment, the material of the first sidewall spacer 310 is silicon oxycarbonitride.
[0127] The material of the second sidewall spacer 320 is silicon oxide, silicon nitride, silicon oxynitride or silicon carbon nitride oxide. In this embodiment, the material of the second sidewall spacer 320 is silicon nitride.
[0128] In this embodiment, after the sidewall spacer 300 is formed, the method further includes: forming a gate 400 in the groove 210 , wherein the gate 400 covers a portion of the sidewall of the sidewall spacer 300 , and the top of the gate 400 is lower than the top of the dielectric layer 200 .
[0129] In this embodiment, the semiconductor structure is formed by a gate-last process, that is, the gate 400 is a dummy gate. The dummy gate is subsequently removed, and a metal gate is formed in the groove 210 .
[0130] In this embodiment, the process steps for forming the sidewall 300 and the gate 400 include: forming a first sidewall film (not shown in the figure) on the top of the dielectric layer 200, the sidewall and the bottom surface of the groove 210; forming a second sidewall film (not shown in the figure) on the first sidewall film; forming a gate film (not shown in the figure) that fills the groove 210, and the gate film covers the surface of the second sidewall film; removing the first sidewall film, the second sidewall film and the gate film located on the top of the dielectric layer 200, and the remaining first sidewall film serves as the first sidewall 310, and the remaining second sidewall film serves as the second sidewall 320; the remaining gate film serves as an initial gate (not shown in the figure), and the top of the initial gate is flush with the top of the dielectric layer 200; etching to remove part of the thickness of the initial gate, and the remaining top of the initial gate is lower than the top of the dielectric layer 200, to form the gate 400.
[0131] The first spacer film, the second spacer film and the gate film located on the top of the dielectric layer 200 are removed by a chemical mechanical polishing process.
[0132] In this embodiment, a dry etching process is used to remove a portion of the thickness of the initial gate. In other embodiments, a wet etching process may also be used to remove a portion of the thickness of the initial gate.
[0133] In this embodiment, the gate 400 is made of polysilicon. In other embodiments, the gate may be made of polycrystalline germanium. In addition, the gate may be made of metal.
[0134] In this embodiment, since the top of the gate 400 is lower than the top of the dielectric layer 200 , the gate 400 exposes a portion of the sidewall of the second spacer 320 .
[0135] In other embodiments, when the material of the first sidewall is silicon oxide and the material of the second sidewall is silicon oxynitride, the method for forming the second sidewall film includes: nitriding a portion of the first sidewall film to form the second sidewall film.
[0136] In this embodiment, after forming the second spacer film and before forming the gate film, it also includes: forming a high-k gate dielectric film (not shown in the figure) on the second spacer film, and the gate film covers the surface of the high-k gate dielectric film. In the process of removing the first spacer film, the second spacer film and the gate film located on the top of the dielectric layer 200, it also includes: removing the high-k gate dielectric film located on the top of the dielectric layer 200. In the process of etching and removing a portion of the thickness of the initial gate, it also includes: etching and removing a portion of the high-k gate dielectric film located on the sidewall of the groove 210, and the top of the remaining high-k gate dielectric film is flush with the top of the gate 400 to form a high-k gate dielectric layer.
[0137] refer to Fig.17 , a polymer layer 500 is formed on the top surface of the dielectric layer 200 .
[0138] The function of the polymer layer 500 is to protect the top surface of the dielectric layer 200 and prevent the top surface of the dielectric layer 200 from being etched, so as to ensure that the depth of the groove 210 meets the process requirements.
[0139] In this embodiment, the process gas for forming the polymer layer 500 includes silicon tetrachloride, oxygen and fluoromethane. The polymer layer 500 is a chemical reaction product of silicon tetrachloride, oxygen and fluoromethane.
[0140] On the one hand, the polymer layer 500 is easily adsorbed on a flat surface, so most of the polymer layer 500 is located on the top surface of the dielectric layer 200. The rest of the polymer layer 500 is mainly located on the top surface of the gate 400. On the other hand, at the side wall of the side wall 300, due to the high inclination, the adsorption of the polymer layer 500 is difficult, so the content of the polymer layer 500 on the side wall surface of the side wall 300 is small and can even be ignored. In addition, since the top surface of the side wall 300 is adjacent to the groove 210, the adsorption difficulty of the polymer layer 500 is between the above two aspects, so a small part of the polymer layer 500 can be adsorbed on the top surface of the side wall 300.
[0141] If the thickness of the polymer layer 500 located on the top surface of the dielectric layer 200 is too large, correspondingly, the content of the polymer layer 500 located on the side wall surface of the side wall 300 is too large, resulting in a large difficulty in the subsequent process of removing the side wall 300. If the thickness of the polymer layer 500 located on the top of the dielectric layer 200 is too small, the protective effect of the polymer layer 500 on the top surface of the dielectric layer 200 is affected. When the side wall 300 is removed later, the top surface of the dielectric layer 200 is easily etched. In this embodiment, the thickness of the polymer layer 500 is 1nm to 5nm.
[0142] refer to Fig.18 and Fig.19 , remove part of the side wall 300 located on the side wall of the groove 210.
[0143] The gate 400 is subsequently removed to form a metal gate that fills the groove 210. Removing part of the sidewall 300 can further expand the accommodation space for the metal gate, thereby increasing the volume of the metal gate.
[0144] like Fig.19 As shown, in this embodiment, only a portion of the second sidewall 320 is removed.
[0145] like Fig.18 As shown, in this embodiment, a dry etching process is used to remove a portion of the sidewall 300 located on the sidewall of the groove 210. In other embodiments, a wet etching process may also be used to remove a portion of the sidewall located on the sidewall of the groove.
[0146] In this embodiment, during the dry etching process, the etching gas includes a high-energy plasma 600. The plasma 600 enters the groove 210, and the speed direction of the plasma 600 is changed to the side wall of the second sidewall 320, thereby bombarding the side wall surface of the second sidewall 320 exposed by the gate 400, thereby removing the second sidewall 320 above the top of the gate 400.
[0147] During the dry etching process, part of the plasma 600 bombards the polymer layer 500, and the polymer layer 500 can play a buffering role, reducing the bombardment speed of the plasma 600, thereby reducing the force of the plasma 600 on the top surface of the dielectric layer 200. Therefore, the polymer layer 500 can protect the top surface of the dielectric layer 200 and prevent the top surface of the dielectric layer 200 from being etched.
[0148] In this embodiment, the polymer layer 500 located on the surface of the gate 400 can also protect the surface of the gate 400 .
[0149] In this embodiment, the steps of forming the polymer layer 500 and removing a portion of the sidewall spacer 300 are repeated until the height of the remaining sidewall spacer 300 reaches a predetermined value.
[0150] In this embodiment, the predetermined value is equal to the thickness of the gate 400 .
[0151] Under the continuous bombardment of the plasma 600, the thickness of the polymer layer 500 will be reduced, so that the protective effect of the polymer layer 500 on the top surface of the dielectric layer 200 is weakened. Therefore, after removing part of the sidewall 300, the polymer layer 500 needs to be re-formed on the top surface of the dielectric layer 200 to make up for the loss of the polymer layer 500, thereby ensuring the protective effect of the polymer layer 500.
[0152] In this embodiment, the process parameters of the dry etching process include: the process gas includes silicon tetrachloride, oxygen, fluoromethane and helium, and the flow rate of the process gas is 100 sccm to 800 sccm.
[0153] In the dry etching process, the bombardment speed and direction of the plasma 600 are related to the pulse power. If the pulse power is too small, the bombardment speed of the plasma 600 is small, the direction of the plasma 600 is too dispersed, and the plasma 600 is difficult to etch and remove the sidewall 300 exposed by the gate 400. In this embodiment, the pulse power is 200W to 800W, the bombardment speed of the plasma 600 is appropriate, and the movement direction is concentrated, which can improve the efficiency of removing part of the sidewall 300.
[0154] In other embodiments, the process parameters of the dry etching process include: the process gas includes silicon tetrachloride, hydrogen, nitrogen trifluoride and helium, the flow rate of the process gas is 100 sccm to 800 sccm, and the pulse power is 200W to 800W.
[0155] refer to Fig. 20 In other embodiments, part of the first sidewall spacer 310 and part of the second sidewall spacer 320 may be removed. Specifically, the first sidewall spacer 310 and part of the second sidewall spacer 320 above the top of the gate 400 are removed.
[0156] In other embodiments, when a portion of the first sidewall 310 and a portion of the second sidewall 320 are removed, the plasma 600 (refer to Fig.18 ) can also further bombard the sidewall surface of the dielectric layer 200 to increase the groove 210 (refer to Fig.17 ) width, thereby further increasing the volume of the subsequently formed metal gate.
[0157] Figure 21 to Figure 29 It is a schematic structural diagram corresponding to each step in the third embodiment of the semiconductor structure forming method of the present invention.
[0158] refer to Fig.21 , providing a substrate 102.
[0159] The difference between this embodiment and the first embodiment is that the substrate 102 is used to form a planar field effect transistor, and the substrate 102 is a base.
[0160] The material of the substrate 102 is silicon, germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium. In this embodiment, the substrate 102 is a silicon substrate.
[0161] In this embodiment, after providing the substrate 102 , the method further includes: forming a pad oxide layer 121 covering the surface of the substrate 102 .
[0162] refer to Fig. 22 , a plurality of discretely arranged gates 420 are formed on the pad oxide layer 121 .
[0163] In this embodiment, the gate 420 is a dummy gate structure, which occupies a space position for the subsequent formation of a metal gate structure.
[0164] refer to Fig.23 , forming a sidewall spacer 340 on the sidewall of the gate 420 .
[0165] In this embodiment, the sidewall spacer 340 is a stacked structure, and includes a first sidewall spacer 341 and a second sidewall spacer 342 . The second sidewall spacer 342 covers the sidewall of the gate 420 , and the first sidewall spacer 341 covers the sidewall of the second sidewall spacer 342 .
[0166] refer to Fig.24A dielectric layer 240 is filled between adjacent gate electrodes 420 , the dielectric layer 240 covers the sidewalls of the spacer 340 , and adjacent dielectric layers 240 form a groove, which is fully filled with the gate electrodes 420 .
[0167] refer to Fig.25 , etching removes a portion of the thickness of the gate 420 , and the sidewalls of the groove 250 are exposed to expose the sidewalls of the sidewall 340 .
[0168] refer to Fig.26 , a polymer layer 520 is formed on the top surface of the dielectric layer 240 .
[0169] refer to Fig. 27 and Fig.28 , remove the sidewall 340 exposed by the sidewall of the groove 250.
[0170] In this embodiment, in the process of removing the sidewall 340 exposed by the sidewall of the groove 250 , all of the second sidewall 342 exposed by the sidewall of the groove 250 are removed by etching, and the first sidewall 341 is retained.
[0171] In this embodiment, a dry etching process is used to remove the second sidewall 342 exposed on the sidewall of the groove 250 , and the etching gas includes high-energy plasma 620 .
[0172] In this embodiment, the process of removing the sidewall 340 exposed by the sidewall of the groove 250 further includes: etching and removing a portion of the exposed sidewall of the first sidewall 341 .
[0173] Fig.29 It is a schematic diagram of the corresponding structure after the process of removing the sidewall 340 exposed by the sidewall of the groove 250 is completed in other embodiments.
[0174] refer to Fig.29 In other embodiments, in the process of removing the sidewall 340 exposed by the sidewall of the groove 250 , all of the second sidewall 342 and all of the first sidewall 341 exposed by the sidewall of the groove 250 are etched away.
[0175] The process of removing the sidewall 340 exposed by the sidewall of the groove 250 further includes: etching and removing the exposed part of the sidewall of the dielectric layer 240 .
[0176] Reference Fig.30 The present invention also provides a semiconductor structure obtained by the above-mentioned formation method, comprising: a substrate; a dielectric layer 220, located on the substrate, wherein the dielectric layer 220 has a groove 230 and a sidewall 330 located on the sidewall of the groove, and the top opening size of the groove 230 is larger than the bottom opening size of the groove 230.
[0177] The substrate is a base; or, the substrate is: a base and a discrete fin 110 located on the base. In this embodiment, the substrate is used to form a FinFET, and the substrate is: a base and a discrete fin 110 located on the base.
[0178] The sidewall 330 includes a second sidewall 332 and a first sidewall 331 . The first sidewall 331 covers the sidewall of the dielectric layer 220 , that is, the first sidewall 331 covers the sidewall of the groove 230 . The first sidewall 331 is located between the second sidewall 332 and the dielectric layer 220 .
[0179] In this embodiment, the first sidewall 331 covers the entire sidewall surface of the dielectric layer 220 , and the top of the second sidewall 332 is lower than the top of the first sidewall 331 .
[0180] The sidewall of the groove 230 exposes the sidewall of the first sidewall 331 which is higher than the second sidewall 332 .
[0181] In this embodiment, the first side wall 331 exposed by the side wall of the groove 230 is in an arc shape, and the groove 230 has a trumpet-shaped opening. In other embodiments, the remaining first side wall 331 exposed by the side wall of the groove 230 is in an inclined shape, and the groove 230 has an inverted trapezoidal opening.
[0182] Fig.31 It is a schematic structural diagram of another embodiment of the semiconductor structure of the present invention.
[0183] refer to Fig.31 In this embodiment, the first sidewall 331 exposes a portion of the sidewall of the dielectric layer 220 , and the top of the second sidewall 332 is flush with the top of the first sidewall 331 .
[0184] In this embodiment, the side wall of the dielectric layer 220 exposed by the side wall of the groove 230 is in an arc shape, and the groove 230 has a trumpet-shaped opening; in other embodiments, the side wall of the dielectric layer 220 exposed by the side wall of the groove 230 is in an inclined shape, and the groove 230 has an inverted trapezoidal opening.
[0185] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A method for forming a semiconductor structure, characterized in that: include: Providing a substrate, on which a dielectric layer is formed, wherein the dielectric layer has a groove and a sidewall located on a sidewall of the groove; forming a polymer layer on the top surface of the dielectric layer, wherein the process gas used to form the polymer layer includes silicon tetrachloride, oxygen and fluoromethane, and the polymer layer is a chemical reaction product of silicon tetrachloride, oxygen and fluoromethane; After forming the polymer layer, a portion of the sidewalls on the sidewalls of the groove is removed.
2. The forming method according to claim 1, characterized in that: The substrate is a base; or the substrate is: a base and separate fins located on the base.
3. The forming method according to claim 2, characterized in that: In the step of providing a substrate, a plurality of discretely arranged gates are also formed on the substrate, the gates fill the grooves, the tops of the gates are lower than the tops of the dielectric layers, and the sidewalls of the grooves expose the sidewalls of the sidewalls; In the process of removing a portion of the sidewall located on the sidewall of the groove, the sidewall exposed by the sidewall of the groove is removed.
4. The forming method according to claim 3, characterized in that: The steps of forming the gate, the sidewall, the dielectric layer and the groove are as follows: forming a plurality of discretely arranged gates on the substrate; forming a sidewall spacer on the sidewall of the gate; A dielectric layer is filled between adjacent gates, the dielectric layer covers the sidewalls of the spacer, the adjacent dielectric layers surround the groove, and the gate fully fills the groove; The gate is partially removed by etching.
5. The forming method according to claim 3, characterized in that: The steps of forming the gate, the sidewall, the dielectric layer and the groove are as follows: forming a dielectric layer covering the surface of the substrate; Etching the dielectric layer to form a groove in the dielectric layer; forming a side wall on the side wall of the groove; Filling the groove to form a gate; The gate is partially removed by etching.
6. The forming method according to claim 1, characterized in that: The thickness of the polymer layer is 1 nm to 5 nm.
7. The forming method according to claim 3, characterized in that: The exposed sidewalls of the groove are removed by dry etching process.
8. The forming method according to claim 7, characterized in that: The process parameters of the dry etching process include: the process gas includes silicon tetrachloride, oxygen, fluoromethane and helium, the flow rate of the process gas is 100 sccm to 800 sccm, and the pulse power is 200W to 800W.
9. The forming method according to claim 7, characterized in that: The process parameters of the dry etching process include: the process gas includes silicon tetrachloride, hydrogen, nitrogen trifluoride and helium, the flow rate of the process gas is 100 sccm to 800 sccm, and the pulse power is 200W to 800W.
10. The forming method according to claim 4 or 5, characterized in that: After removing part of the side wall located on the side wall of the groove, the opening size of the groove gradually decreases along the top of the groove toward the bottom of the groove.
11. The forming method according to claim 10, characterized in that: In the process of forming the sidewall, the sidewall includes a first sidewall and a second sidewall, the first sidewall covers the sidewall of the dielectric layer, and the first sidewall is located between the second sidewall and the dielectric layer.
12. The forming method according to claim 11, characterized in that: In the process of removing a portion of the sidewalls on the sidewalls of the groove, all of the second sidewalls exposed by the sidewalls of the groove are removed by etching, and the first sidewalls exposed by the sidewalls of the groove are retained.
13. The forming method according to claim 12, characterized in that: The steps of forming the polymer layer and removing the second sidewall exposed by the groove sidewall are repeated until the second sidewall exposed by the groove sidewall is completely removed.
14. The forming method according to claim 12, characterized in that: The process of removing a portion of the sidewall located on the sidewall of the groove further includes: etching and removing a portion of the first sidewall exposed by the sidewall of the groove.
15. The forming method according to claim 14, characterized in that: After removing part of the side wall located on the side wall of the groove, the remaining first side wall exposed by the side wall of the groove is in an arc shape, and the groove has a trumpet-shaped opening; Alternatively, the remaining first side wall exposed by the side wall of the groove is in a slope shape, and the groove has an inverted trapezoidal opening.
16. The forming method according to claim 11, characterized in that: In the process of removing a portion of the sidewall spacer located on the sidewall of the groove, all of the second sidewall spacer and all of the first sidewall spacer exposed by the sidewall of the groove are removed by etching.
17. The forming method according to claim 16, characterized in that: The steps of forming the polymer layer and removing the second sidewall and the first sidewall exposed by the groove sidewall are repeated until the second sidewall and the first sidewall exposed by the groove sidewall are completely removed.
18. The forming method according to claim 17, characterized in that: The process of removing a portion of the sidewall located on the sidewall of the groove further includes: etching and removing a portion of the sidewall of the dielectric layer exposed by the sidewall of the groove.
19. The forming method according to claim 18, characterized in that: After removing the second side wall and the first side wall exposed by the side wall of the groove, the remaining side wall of the dielectric layer exposed by the side wall of the groove is in an arc shape, and the groove has a trumpet-shaped opening; Alternatively, the remaining side wall of the dielectric layer exposed by the side wall of the groove is in a slope shape, and the groove has an inverted trapezoidal opening.
20. A semiconductor structure, characterized in that: The semiconductor structure is formed by the forming method according to any one of claims 1 to 19, and the semiconductor structure comprises: substrate; A dielectric layer is located on the substrate, wherein the dielectric layer has a groove and a sidewall located on the sidewall of the groove; The polymer layer is located on the top surface of the dielectric layer, and the polymer layer is a chemical reaction product of silicon tetrachloride, oxygen and fluoromethane.
21. The semiconductor structure according to claim 20, wherein: The substrate is a base; or the substrate is: a base and separate fins located on the base.
22. The semiconductor structure according to claim 21, wherein: The sidewall includes a first sidewall and a second sidewall, the first sidewall covers the sidewall of the dielectric layer, and the first sidewall is located between the second sidewall and the dielectric layer.
23. The semiconductor structure according to claim 22, wherein: The first sidewall spacer covers the sidewall surface of the dielectric layer, and the top of the second sidewall spacer is lower than the top of the first sidewall spacer.
24. The semiconductor structure according to claim 23, wherein: The first side wall higher than the second side wall is in an arc shape, and the groove is in a trumpet-shaped opening; or, the first side wall higher than the second side wall is in an inclined shape, and the groove is in an inverted trapezoidal opening.
25. The semiconductor structure according to claim 22, wherein: The first sidewall exposes a portion of the sidewall of the dielectric layer, and the top of the second sidewall is flush with the top of the first sidewall.
26. The semiconductor structure according to claim 25, wherein: The dielectric layer sidewall exposed by the first sidewall is in an arc shape, and the groove is in a trumpet-shaped opening; or, the dielectric layer sidewall exposed by the groove sidewall is in an inclined shape, and the groove is in an inverted trapezoidal opening.