A method for generating clear dislocation pits on the {101} crystal plane of KH2PO4 crystal

By using a water-ethanol mixed solution on the surface of KDP crystals for controlling corrosion and polishing, the problems of excessive corrosion and impurity corrosion pits in the existing technology are solved, and the generation of clear dislocation pits is achieved, and the accuracy of observation of dislocation structures is improved. and research effects.

CN112213173BActive Publication Date: 2024-12-06SHANDONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011045463.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-29
Publication Date
2024-12-06
Estimated Expiration
2040-09-29

AI Technical Summary

Technical Problem

The prior art can easily cause excessive corrosion when the KDP crystal surface is clearly dislocation pit, affecting the analysis of dislocation structure, and other defects will also cause erosion pits, affecting the judgment of dislocation density, direction and distribution.

Method used

Use water-ethanol mixed solution as the corrosion liquid to control the water quality content of the corrosion liquid to be 72-78%, and corrosion and polish at room temperature to ensure that the corrosion time is 10-20 seconds. Polished by a polishing machine to remove impurities and form Clear dislocation erosion pit.

Benefits of technology

It effectively generates clear dislocation erosion pits, avoids the influence of other defects, improves the accuracy of observation and research of dislocation structures, and can accurately obtain dislocation density and type information.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002707832260000021
    Figure BDA0002707832260000021
  • Figure HDA0002707832270000011
    Figure HDA0002707832270000011
  • Figure HDA0002707832270000012
    Figure HDA0002707832270000012
Patent Text Reader

Abstract

The present invention relates to a KH 2 PO 4 A method for producing clear dislocation pits on a {101} crystal face belongs to the technical field of crystal characterization. A KDP crystal face sample is cut and the front and back surfaces of the sample are polished for later use. A water-ethanol mixed solution with a water content of 74% to 76% is prepared as a crystal etching solution, the crystal sample is placed in the etching solution at room temperature and kept for 10 to 20 seconds, and after being taken out, the etching solution is used to polish the crystal surface for 2 to 4 seconds, the polishing machine speed is set at 120 to 200 r / min, the solution on the crystal surface is wiped clean and dried, and the treated crystal surface is observed under an optical microscope and a 3D laser confocal microscope to obtain clear dislocation pit photos.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for generating clear dislocation pits on the surface of a KH2PO4 (KDP for short) crystal, belonging to the technical field of crystal characterization. Background Art

[0002] Crystals grown by aqueous solution methods have always been widely valued. KH2PO4 (KDP for short) crystals are typical aqueous solution crystals with large nonlinear optical coefficients and laser damage thresholds, and high transmittance in the near-infrared to ultraviolet bands, so they are often used to make laser frequency doubling devices. Dislocations are common in crystal growth, and dislocations will produce residual stress in the crystal, increasing the risk of crystal cracking. The presence of dislocations affects the performance of the crystal. For example, the dislocation density in KDP crystals used in high-power laser systems has a great influence on the laser damage threshold (Endert & Melle, 1981). Therefore, characterizing dislocations in KDP crystals is one of the key processes for the preparation of frequency doubling devices, and is also necessary for studying and improving KDP crystal growth technology.

[0003] At present, the characterization of dislocations in KDP crystals mainly includes optical observation and X-ray morphology detection (Zaitseva & Carman, 2001). Optical observation has the advantages of simple sample preparation, high measurement accuracy and wide application range, and is currently the main method used for dislocation structure research. The premise of using optical detection of dislocations is to produce dislocation pits of good quality on the crystal surface. Traditional KDP crystal etchants must include water, glacial acetic acid + water and glacial acetic acid + water + concentrated sulfuric acid mixture (Koziejowska & Sangwal, 1988). KDP is an aqueous solution crystal. When using the above etchants, it is easy to cause excessive corrosion of the crystal surface, affecting the analysis of dislocation structure. In addition, there are still some problems in the current research on crystal surface pits. Surface pits can be generated not only at dislocations, but also at other locations, such as impurities, crystal cracks and other defects. If the pit morphology is not clear, it will affect the judgment of dislocation type, density, direction, distribution and pit source. CN103698339A discloses a method for detecting crystal dislocation corrosion, and the main technical scheme includes the following steps: processing the sample surface to be tested to a predetermined surface finish; determining and marking the observation point of the sample; coating the surface of the sample except the observation point; polishing the coated sample; cleaning the polished sample; supplementary coating the surface of the sample except the observation point; corroding the coated sample; cleaning the corroded sample; measuring the dislocation of the sample observation point, and calculating the dislocation density of the sample. The invention is mainly aimed at the (1 1 3) and (1 0 0) crystal planes of germanium single crystals and the (1 1 1) crystal plane of silicon single crystals. The etching solution is prepared by hydrofluoric acid and nitric acid in a certain volume ratio, and it does not show the morphology of the generated dislocation pits.

[0004] Producing clear dislocation etch pits on the crystal surface will provide more powerful assistance to the characterization of dislocation structure. For this reason, the present invention is proposed. Summary of the invention

[0005] In view of the problems and shortcomings of the prior art, the present invention provides a method for generating clear dislocation pits on the surface of an aqueous solution crystal.

[0006] The present invention is achieved through the following technical solutions:

[0007] A method for generating clear dislocation pits on the surface of an aqueous solution crystal comprises the following steps:

[0008] The polished aqueous solution crystal is immersed in a corrosive solution to corrode the crystal surface. The corrosive solution is a water-ethanol mixed solution with a water content of 72-78% by mass. The corroded crystal is polished again to obtain a crystal with clear dislocation pits on the surface.

[0009] According to the present invention, preferably, the temperature difference between the etching solution and the crystal is within 2° C., so as to avoid cracks on the crystal surface; further preferably, the temperatures of the etching solution and the crystal are both room temperature.

[0010] According to the present invention, preferably, the crystal immersion time is 10 to 20 seconds.

[0011] According to the present invention, preferably, the mass content of water in the etching solution is 74-76%, and most preferably 75%.

[0012] According to the present invention, preferably, polishing is performed using a polishing liquid, and the polishing liquid is a corresponding crystal etching liquid.

[0013] According to the present invention, preferably, the polishing operation is performed in a polishing machine; further preferably, the rotation speed of the polishing machine is 120-200 r / min, which can effectively remove impurities in the etch pits.

[0014] According to the present invention, preferably, the polishing time is 2 to 4 seconds. If the time is too long, excessive corrosion may be easily caused to the crystal surface.

[0015] According to the present invention, preferably, the aqueous solution crystals are potassium dihydrogen phosphate crystals (KDP crystals) or potassium dideuterium phosphate crystals (DKDP crystals). Other crystals grown by aqueous solution methods may also be applicable to the present invention.

[0016] The principle of the present invention is:

[0017] The present invention etches the upper and lower crystal faces of the aqueous solution crystal, mainly including the corrosion at the dislocation, the corrosion at the impurity ions and other defects, and the overall corrosion on the crystal face. These processes will produce pits. Only when the tangential corrosion rate Vs at the step is greater than the corrosion rate Vd at the corrosion site perpendicular to the crystal face, and these two corrosion rates are much greater than the overall corrosion rate Vc of the crystal face, will observable pits be produced. According to the Cabrera thermodynamic model, there is a critical undersaturation for the dissolution of the crystal to produce dislocation pits, σ c , as shown in formula (1),

[0018]

[0019] Where γ is the surface free energy of the crystal, Ω is the molecular molar volume, k is the Boltzmann constant, T is the absolute temperature, G is the crystal shear modulus, b is the Burgers vector of the dislocation, α is a constant related to the dislocation type, and its value is between 1 and 1 / (1-μ), and μ is the Poisson's ratio. In the cone of the KDP crystal, γ = 2×10 -2 J / m 2 ,Ω=9.67×10 -29 m 3 , k = 1.38 × 10 -23 J / K, G=1.26×10 10 N / m 2 , b = 5 × 10 -10 m, the critical undersaturation of the cone surface of the KDP crystal is obtained as σ c =0.0587. When the absolute value of the undersaturation of the corrosion solution is less than σ c , the dissolution belongs to steady-state dissolution. At this time, the cause of corrosion is attributed to the more uniform dissolution of atoms or molecules around the dislocation line and other parts into the corrosive solution, and the dislocation energy does not play a major role. When the absolute value of the undersaturation of the corrosive solution is greater than σ c When the dislocation is formed, the strain energy around the dislocation is the main reason for the non-steady-state dissolution, and dislocation pits will be generated at this time. Considering the critical undersaturation when dislocation pits are generated, the deionized water-anhydrous ethanol mixture was used as the corrosion solvent for surface corrosion in the experiment, which not only ensures the generation of dislocation pits, but also ethanol as a buffer can slow down the corrosion rate and prolong the corrosion time.

[0020] In a preferred embodiment, when a 75% water content etching solution is used to etch a crystal, the pits generated in the first 10 seconds include not only dislocation pits, but also pits formed at other crystal defects. However, as the etching time increases, due to the continuity of dislocations in the crystal, only dislocation pits can continue to exist. Therefore, when the etching time reaches 10 seconds, a part of the pits disappear, and the remaining pits are dislocation pits. When the etching time exceeds 20 seconds, new pits will appear and affect the observation of dislocation pits. During the crystal etching process, there is a diffusion boundary layer between the crystal surface and the etching solution. When the etching time is 10 to 20 seconds, the solution concentration in the boundary layer exceeds the critical under-supersaturation, which can ensure that the dislocation pits are exposed; if it exceeds 20 seconds, it will lead to excessive corrosion of the crystal, and other corrosion pits are likely to appear, affecting the observation of dislocation pits. Therefore, when the etching time is 10 to 20 seconds, it can be ensured that most of the pits on the crystal surface are dislocation pits. The crystal is taken out from the etching liquid and polished. The purpose of this operation is to smooth the crystal surface outside the dislocation etch pit. There will be residual etching liquid in the crystal etch pit to continue to corrode the dislocation etch pit, thereby enhancing the contrast of the etch pit and facilitating the observation of the dislocation etch pit.

[0021] The beneficial effects of the present invention are:

[0022] 1. The present invention can conveniently and quickly produce clear dislocation pits on the surface of aqueous solution crystals, avoiding the influence of other defects.

[0023] 2. The generation of clear dislocation pits facilitates the subsequent observation and study of dislocation structures in crystals. For example, more accurate dislocation density information can be obtained through the number of pits, and the dislocation type and dislocation direction information can be preliminarily inferred through the observation of pit morphology. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic diagram of the corrosion directions on the crystal surface.

[0025] Figure 2 This is a microscope picture of the KDP crystal in the embodiment after the first polishing and before being immersed in the etching solution.

[0026] Figure 3 These are the microscope images and 3D laser confocal microscope images of the dislocation pits in Example 1; a is the microscope image, and b is the 3D laser confocal microscope image.

[0027] Figure 4 These are the microscope images and 3D laser confocal microscope images of dislocation pits in Comparative Example 1; c is the microscope image, and d is the 3D laser confocal microscope image.

[0028] Figure 5These are the microscope images and 3D laser confocal microscope images of the dislocation pits in Example 2; a is the microscope image, and b is the 3D laser confocal microscope image.

[0029] Figure 6 These are the microscope images and 3D laser confocal microscope images of dislocation pits in Comparative Example 2; c is a microscope image, and d is a 3D laser confocal microscope image.

[0030] Figure 7 These are the microscope images and 3D laser confocal microscope images of the dislocation pits in Example 3; a is the microscope image, and b is the 3D laser confocal microscope image.

[0031] Figure 8 These are the microscope images and 3D laser confocal microscope images of dislocation pits in Comparative Example 3; c is the microscope image, and d is the 3D laser confocal microscope image. DETAILED DESCRIPTION

[0032] The present invention will be further described below in conjunction with the accompanying drawings and specific implementation modes, but is not limited thereto.

[0033] The "%" in the examples are all mass percentages. The examples were all carried out at room temperature. The raw materials used in the examples were all conventional commercially available products.

[0034] The aqueous solution crystal used in the embodiment is KDP crystal. The microscope picture before immersion in the etching solution after the first polishing is as follows Figure 2 As shown. Figure 2 It can be seen that the crystal surface after polishing is clean and flat, with no corrosion pits and no obvious defects, which can meet the experimental requirements.

[0035] Example 1

[0036] The polished KDP crystal sample was immersed in a water-ethanol mixed etching solution with a water content of 75%, the sample surface was corroded and kept for 15 seconds, then the sample was taken out and polished for 3 seconds using a polishing machine, and the crystal surface was wiped clean with a cotton ball to obtain dislocation pits.

[0037] The dislocation pits obtained in Example 1 were observed using a microscope and a 3D laser confocal microscope. The morphology obtained is as follows: Figure 3 As shown, a is a microscope image, and b is a 3D laser confocal microscope image. Figure 3 It can be seen that after 75% water-ethanol corrosion and polishing, the dislocation pits on the crystal surface are clear, showing an inverted triangular pyramid shape, with clear boundaries and a density of about 10 / cm 2 .

[0038] Comparative Example 1

[0039] As described in Example 1, the polished KDP crystal sample was immersed in a water-ethanol mixed etching solution with a water content of 25%, and other conditions remained unchanged.

[0040] The dislocation pits obtained in Comparative Example 1 were observed using a microscope and a 3D laser confocal microscope. The morphology obtained is as follows: Figure 4 As shown, c is a microscope image, and d is a 3D laser confocal microscope image. Figure 4 It can be seen that after 25% water-ethanol corrosion and polishing treatment, the dislocation pits on the crystal surface are unclear and difficult to distinguish, the inverted triangular pyramid shape is fuzzy, the boundary is unclear, and the measurement error of the dislocation density is large.

[0041] Example 2

[0042] The polished KDP crystal sample was immersed in a water-ethanol mixed etching solution with a water content of 75%, the sample surface was corroded and kept for 18 seconds, then the sample was taken out and polished for 3 seconds using a polishing machine, and the crystal surface was wiped clean with a cotton ball to obtain dislocation pits.

[0043] The dislocation pits obtained in Example 2 were observed using a microscope and a 3D laser confocal microscope. The morphology obtained is as follows: Figure 5 As shown, a is a microscope image, and b is a 3D laser confocal microscope image. Figure 5 It can be seen that after etching for 18s and polishing for 3s, the dislocation pits on the crystal surface are clear, showing an inverted triangular pyramid shape, with clear boundaries and a density of about 13 / cm 2 .

[0044] Comparative Example 2

[0045] As described in Example 2, the etching time was changed to 3 s, and the other processing conditions remained unchanged.

[0046] The dislocation pits obtained in Comparative Example 2 were observed using a microscope and a 3D laser confocal microscope. The morphology obtained is as follows: Figure 6 As shown, c is a microscope image, and d is a 3D laser confocal microscope image. Figure 6 It can be seen that after 3s of corrosion, the longitudinal corrosion depth is shallow, the dislocation pits on the crystal surface are unclear and difficult to distinguish, the inverted triangular pyramid shape is fuzzy, the boundary is unclear, and the measurement error of the dislocation density is large. It can be seen that the crystal corrosion time is also a key factor in producing clear dislocation pits.

[0047] Example 3

[0048] The polished KDP crystal sample was immersed in a water-ethanol mixed etching solution with a water content of 75%, the sample surface was corroded and kept for 15 seconds, then the sample was taken out and polished for 3 seconds using a polishing machine, and the crystal surface was wiped clean with a cotton ball to obtain dislocation pits.

[0049] The dislocation pits obtained in Example 3 were observed using a microscope and a 3D laser confocal microscope. The morphology obtained is as follows: Figure 7 As shown, a is a microscope image, and b is a 3D laser confocal microscope image. Figure 7 It can be seen that after 75% water-ethanol corrosion and polishing, the dislocation pits on the crystal surface are clear, showing an inverted triangular pyramid shape, with clear boundaries and a density of about 6 / cm 2 .

[0050] Comparative Example 3

[0051] As described in Example 3, the ratio of the etching solution was changed to prepare an etching agent with a water content of 80%, and the other conditions were the same as in Example 3.

[0052] The dislocation pits obtained in Comparative Example 3 were observed using a microscope and a 3D laser confocal microscope. The morphology obtained is as follows: Figure 8 As shown, c is a microscope image, and d is a 3D laser confocal microscope image. Figure 8 It can be seen that after the crystal was etched by water-ethanol with a water content of 80% and polished, the surface dislocation pits were unclear and difficult to distinguish, the inverted triangular pyramid shape was fuzzy, the boundary was unclear, and the measurement error of the dislocation density was large. It can be seen that increasing the water content of the etching solution will cause excessive corrosion on the crystal surface and affect the observation of dislocation pits.

Claims

1. A method for generating clear dislocation pits on the surface of an aqueous solution crystal, comprising the following steps: The polished aqueous solution crystal is immersed in the etching solution to etch the crystal surface. The crystal immersion time is 10 to 20 seconds. The etched crystal is polished again to obtain a crystal with clear dislocation pits on the surface. The etching liquid is a water-ethanol mixed solution, the mass content of water in the etching liquid is 72-78%, the aqueous solution crystals are potassium dihydrogen phosphate crystals or potassium dideuterium phosphate crystals, and polishing is performed using a polishing liquid, which is a corresponding crystal etching liquid.

2. The method for generating clear dislocation pits on the surface of aqueous solution crystal according to claim 1, characterized in that: The temperature difference between the etching solution and the crystal is within 2°C.

3. The method for generating clear dislocation pits on the surface of aqueous solution crystal according to claim 1, characterized in that: The mass content of water in the corrosive solution is 74~76%.

4. The method for generating clear dislocation pits on the surface of aqueous solution crystal according to claim 3, characterized in that: The mass content of water in the corrosive solution is 75%.

5. The method for generating clear dislocation pits on the surface of aqueous solution crystal according to claim 1, characterized in that: The polishing operation is carried out in a polishing machine.

6. The method for generating clear dislocation pits on the surface of aqueous solution crystal according to claim 5, characterized in that: The speed of the polishing machine is 120~200 r / min.

7. The method for generating clear dislocation pits on the surface of aqueous solution crystal according to claim 1, characterized in that: The polishing time is 2~4 s.