Method for forming semiconductor structure and semiconductor structure

Through multi-step cleaning and isolation layer formation, the problem of difficulty in cleaning residues after metal gate cutting is solved, and the performance and yield of the semiconductor structure are improved.

CN112289675BActive Publication Date: 2024-11-19SEMICON MFG INT (SHANGHAI) CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN201910662591.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-07-22
Publication Date
2024-11-19
Estimated Expiration
2039-07-22

AI Technical Summary

Technical Problem

During semiconductor manufacturing, the residue after metal gate cutting is difficult to clean, affecting device performance and yield.

Method used

A multi-step cleaning treatment method is adopted, including the first cleaning to remove non-metal residues, the second cleaning to remove metal residues, and the formation of an isolation layer after cleaning to prevent subsequent formation of conductive paths.

Benefits of technology

It effectively reduces the leakage caused by metal residues and improves the performance and yield of semiconductor structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112289675B_ABST
    Figure CN112289675B_ABST
Patent Text Reader

Abstract

A method for forming a semiconductor structure and a semiconductor structure, comprising: providing a substrate; forming a gate structure on the substrate, the gate structure extending in a first direction; removing part of the gate structure, forming a groove in the gate structure, the groove penetrating the gate structure in a second direction, the second direction being different from the first direction; performing a first cleaning process on the groove, the first cleaning process being used to remove non-metallic residues; performing a second cleaning process on the groove, the second cleaning process being used to remove metal residues. The non-metallic residues formed in the groove are removed by the first cleaning process; the metal residues in the groove are removed by the second cleaning process, thereby reducing the metal residues from being electrically connected to adjacent gate structures at the bottom of the groove, thereby reducing leakage between adjacent gate structures, and improving the performance and yield of the final product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor manufacturing technology, and in particular to a method for forming a semiconductor structure and a semiconductor structure. Background Art

[0002] The electronics industry has experienced a growing demand for smaller and faster electronic devices that can simultaneously support a greater number of increasingly complex and sophisticated functions. Therefore, a continuing trend in the semiconductor industry is to manufacture low-cost, high-performance, and low-power integrated circuits (ICs). To date, these goals have been achieved to a large extent by scaling down semiconductor IC sizes (e.g., minimum feature sizes) and thereby increasing production efficiency and reducing associated costs. However, this scaling down also increases the complexity of semiconductor manufacturing processes. Therefore, the realization of continued advancements in semiconductor ICs and devices requires similar advancements in semiconductor manufacturing processes and technologies.

[0003] As a part of the device, the gate material greatly affects the performance of the device. The traditional polysilicon gate process has the "polysilicon depletion" effect, which affects the conduction of the device, so the metal gate is introduced. In order to obtain better epitaxial stress, the dummy gate needs to be cut off when the metal gate exceeds the 5nm node. This process can not only obtain a good shape profile, but also shrink the feature size of more than 20nm. However, after the metal gate is removed, the residue formed at the bottom of the trench is very difficult to clean.

[0004] How to ensure that the semiconductor structure is effectively cleaned of its residues after metal gate cutting, so as to improve the yield of the final product, is an urgent problem that needs to be solved. Summary of the invention

[0005] The problem solved by the present invention is to provide a method for forming a semiconductor structure and a semiconductor structure, which can effectively remove residues formed by cutting a metal gate, thereby improving the yield of the final product.

[0006] To solve the above problems, the present invention provides a method for forming a semiconductor structure, comprising: providing a substrate; forming a gate structure on the substrate, wherein the gate structure extends along a first direction; removing part of the gate structure to form a groove in the gate structure, wherein the groove penetrates the gate structure along a second direction, and the second direction is different from the first direction; performing a first cleaning process on the groove, wherein the first cleaning process is used to remove non-metallic residues; and performing a second cleaning process on the groove, wherein the second cleaning process is used to remove metal residues.

[0007] Optionally, the method further includes: forming a dielectric layer on the substrate, wherein the dielectric layer covers the sidewalls of the gate structure and exposes the top surface of the gate structure.

[0008] Optionally, the gate structure includes a gate layer and a sidewall located on a sidewall surface of the gate layer.

[0009] Optionally, the gate structure further includes a gate dielectric layer located on the substrate, and the gate layer is located on the gate dielectric layer; a material of the gate dielectric layer includes a high-K dielectric material.

[0010] Optionally, the material of the gate layer includes metal; the material of the sidewall spacer includes one or more combinations of silicon nitride, silicon oxide and silicon oxynitride.

[0011] Optionally, the method for forming the dielectric layer and the gate structure includes: forming a dummy gate layer on the substrate; forming the sidewall on the sidewall surface of the dummy gate layer; forming an initial dielectric layer on the substrate, the initial dielectric layer covering the dummy gate layer and the sidewall; planarizing the initial dielectric layer until the dummy gate layer is exposed to form the dielectric layer; after forming the dielectric layer, removing the dummy gate layer to form a first opening; forming the gate dielectric layer on the bottom surface of the first opening; and forming the gate layer on the gate dielectric layer.

[0012] Optionally, the method for forming the trench includes: forming a mask structure on the dielectric layer and the gate structure, the mask structure exposing a portion of the gate structure; and etching the gate layer and the sidewall using the mask structure as a mask to form the trench.

[0013] Optionally, the mask structure includes a first mask layer and a second mask layer located on the first mask layer; a material of the first mask layer is different from a material of the second mask layer.

[0014] Optionally, the material of the first mask layer is nitrogen-doped silicon oxycarbide; the material of the second mask layer is titanium nitride, silicon carbide, silicon carbonitride, silicon carbonitride oxide, silicon oxynitride, boron nitride or boron carbonitride.

[0015] Optionally, there are multiple gate structures, and the multiple gate structures are parallel to the first direction; and the trench runs through the multiple gate structures.

[0016] Optionally, the method of the first cleaning treatment includes: performing plasma treatment on the groove; and after the plasma treatment, performing a cleaning process on the groove.

[0017] Optionally, the sidewalls are etched to form non-metallic residues, wherein the non-metallic residues include nitrides or oxides; and the gate layer is etched to form metal residues.

[0018] Optionally, the plasma treatment process includes: the plasma treatment process includes: the gas is hydrogen, helium or argon, the gas flow rate is 10sccm~1000sccm, the power is 50W~2000W; the bias voltage is 0V~5000V, and the temperature is 30℃~150℃.

[0019] Optionally, the cleaning process is a SiCoNi process; the SiCoNi process includes: the gas is nitrogen trifluoride or ammonia, the gas flow rate is 100 sccm to 2000 sccm, and the temperature is less than 50°C.

[0020] Optionally, the second cleaning process includes dry cleaning or wet cleaning.

[0021] Optionally, the dry cleaning process includes: the gas is carbon tetrafluoride, sulfur hexafluoride or boron trichloride; the gas flow rate is 5sccm~500sccm, the power is 50W~1500W, the bias voltage is 50V~2000V, and the temperature is less than 150°C.

[0022] Optionally, the solution used for wet cleaning is concentrated sulfuric acid and hydrogen peroxide.

[0023] Optionally, the second cleaning process is performed after the first cleaning process.

[0024] Optionally, after performing the first cleaning process and the second cleaning process, the method further includes: forming an isolation layer in the groove; the material of the isolation layer includes one or more combinations of silicon oxide, silicon nitride, silicon oxynitride, low-K dielectric material and ultra-low-K dielectric material.

[0025] Correspondingly, the present invention also provides a semiconductor structure, including one formed by the above method.

[0026] Compared with the prior art, the technical solution of the present invention has the following advantages:

[0027] In the technical solution of the present invention, the groove is used to cut off the gate structure and reduce the characteristic size of the original gate structure to achieve a highly integrated effect; the non-metallic residues formed in the groove are removed by a first cleaning process; the metal residues in the groove are removed by a second cleaning process, thereby reducing the metal residues from electrically connecting adjacent gate structures at the bottom of the groove, thereby reducing leakage between adjacent gate structures and improving the performance and yield of the final product.

[0028] Furthermore, after the first cleaning process, the second cleaning process is performed. The non-metallic residues are first removed by the first cleaning process, so that the metal residues can be exposed as much as possible, which is convenient for the subsequent second cleaning process to completely remove the metal residues as much as possible, thereby reducing the leakage problem caused by the metal residues conductively connecting the adjacent gate structures, thereby improving the performance and yield of the final product.

[0029] Furthermore, after the first cleaning process and the second cleaning process, an isolation layer is formed in the trench. The purpose of forming the isolation layer is to fill the groove in the trench to prevent metal residues from filling the groove in the future, causing the gate layer on both sides of the trench to form a conductive path and cause leakage, which will affect the final performance and yield of the finished product. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 to Figure 2 It is a structural schematic diagram of the formation process of a semiconductor structure;

[0031] Figures 3 to 12 It is a schematic diagram of the structures of the steps of an embodiment of a method for forming a semiconductor structure of the present invention. DETAILED DESCRIPTION

[0032] As described in the background art, the final product performance and yield of the semiconductor structure in the prior art need to be improved.

[0033] refer to Figure 1 , providing a substrate; forming a gate structure 100 and a dielectric layer (not shown) on the substrate, wherein the dielectric layer exposes the top of the gate structure 100, and the gate structure 100 extends along a first direction; the gate structure 100 includes a gate layer 101 and a sidewall 102 located on the sidewall surface of the gate layer 101; forming a first trench 103 in the gate structure 100, wherein the first trench 103 penetrates the gate structure 100 along a second direction, and the second direction is different from the first direction; metal residues 104 and nitride residues 105 remain on the bottom surface of the first trench 103.

[0034] refer to Figure 2 , Figure 2 yes Figure 1In the enlarged schematic diagram of part A, when the nitride residue 105 is easily partially oxidized to form an oxide layer 106, the oxide layer 106 is very easy to be washed away. After the oxide layer 106 is washed away, a second groove connecting the gate structure 100 on both sides of the first groove 103 will be formed. The second groove is easily filled with the metal residue 104. At this time, the gate structure 100 on both sides of the first groove 103 is easy to form a conductive path to cause leakage, which will affect the final performance and yield of the finished product.

[0035] On this basis, the present invention provides a method for forming a semiconductor structure, performing a first cleaning process in the first trench to remove non-metallic residues, and performing a second cleaning process in the first trench to remove metal residues, thereby solving the leakage problem caused by the gate structure on both sides of the first trench being connected by the metal residues, and improving the performance and yield of the final product.

[0036] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0037] Figures 3 to 12 It is a structural schematic diagram of a formation process of a semiconductor structure according to an embodiment of the present invention.

[0038] Please refer to Figure 3 , providing a substrate 200.

[0039] In this embodiment, the material of the substrate 200 is silicon; in other embodiments, the material of the substrate may also be germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium; in other embodiments, the substrate may also be a silicon substrate on an insulator or a germanium substrate on an insulator.

[0040] Please continue to refer to Figure 3 , a gate structure 201 is formed on the substrate 200, and the gate structure 201 extends along a first direction.

[0041] Please continue to refer to Figure 3 , a dielectric layer 202 is formed on the substrate 200 , wherein the dielectric layer 202 covers the sidewalls of the gate structure 201 and exposes the top surface of the gate structure 201 .

[0042] The material of the dielectric layer 202 includes silicon dioxide, low-k dielectric material (low-k dielectric material refers to dielectric material with a relative dielectric constant lower than 3.9) or ultra-low-k dielectric material (ultra-low-k dielectric material refers to dielectric material with a relative dielectric constant lower than 2.5).

[0043] When the material of the dielectric layer 202 is a low-k dielectric material or an ultra-low-k dielectric material, the material of the dielectric layer 202 is carbon silicon oxyhydride (SiCOH), fluorine-doped silicon dioxide (FSG), boron-doped silicon dioxide (BSG), phosphorus-doped silicon dioxide (PSG), boron-phosphorus-doped silicon dioxide (BPSG), hydrogenated silsesquioxane or methyl silsesquioxane.

[0044] In this embodiment, the material of the dielectric layer 202 is an ultra-low-k dielectric material (with a dielectric constant less than 2.5), and the ultra-low-k dielectric material is silicon carbon oxyhydride (SiCOH).

[0045] In this embodiment, the gate structure 201 includes a gate layer 203 and a sidewall spacer 204 located on a sidewall surface of the gate layer 203 .

[0046] The material of the gate layer 203 includes metal, and the metal includes one or more combinations of copper, tungsten, nickel, chromium, titanium, tantalum and aluminum. In this embodiment, the material of the gate layer 203 is aluminum.

[0047] The material of the sidewall spacer 204 includes one or more of silicon oxide, silicon nitride and silicon oxynitride. In the present embodiment, the material of the sidewall spacer 204 is silicon nitride.

[0048] In this embodiment, the sidewall 204 is formed by a chemical vapor deposition process; in other embodiments, the sidewall 204 may be formed by an atomic layer deposition process or a physical vapor deposition process.

[0049] In this embodiment, the gate structure 201 further includes a gate dielectric layer 205 located on the substrate 200 , and the gate layer 203 is located on the gate dielectric layer 205 .

[0050] In this embodiment, the gate dielectric layer 205 is made of a high-K dielectric material. In other embodiments, the gate dielectric layer may also be made of silicon oxide.

[0051] In this embodiment, the gate dielectric layer 205 is formed by a thermal oxidation process; in other embodiments, the gate dielectric layer may be formed by an in-situ water vapor generation process.

[0052] In this embodiment, the method for forming the dielectric layer 202 and the gate structure 201 includes: forming a dummy gate layer (not shown) on the substrate 200; forming the sidewall 204 on the sidewall surface of the dummy gate layer; forming an initial dielectric layer (not shown) on the substrate 200, the initial dielectric layer covering the dummy gate layer and the sidewall 204; flattening the initial dielectric layer until the top surface of the dummy gate layer is exposed to form the dielectric layer 202; after forming the dielectric layer 202, removing the dummy gate layer to form a first opening; forming the gate dielectric layer 205 on the bottom surface of the first opening; and forming the gate layer 203 on the gate dielectric layer 205.

[0053] In other embodiments, the method for forming the dielectric layer and the gate structure may further include: forming a gate dielectric layer on the substrate; forming a dummy gate layer on the gate dielectric layer; forming the sidewalls on the sidewall surfaces of the gate dielectric layer and the dummy gate layer; forming an initial dielectric layer on the substrate, the initial dielectric layer covering the gate dielectric layer, the dummy gate layer and the sidewalls; flattening the initial dielectric layer until the top surface of the dummy gate layer is exposed to form the dielectric layer; after forming the dielectric layer, removing the dummy gate layer to form a first opening; forming a gate layer in the first opening; the gate layer is located on the gate dielectric layer.

[0054] In this embodiment, the material of the dummy gate layer is polysilicon.

[0055] The process for forming the initial dielectric layer includes a chemical vapor deposition process, a physical vapor deposition process, an atomic layer deposition process or a spin coating process. In this embodiment, the process for forming the initial dielectric layer adopts a chemical vapor deposition process.

[0056] In this embodiment, the process of planarizing the initial dielectric layer adopts a chemical mechanical polishing process; in other embodiments, the planarizing process can also be an etching process.

[0057] In this embodiment, the process of removing the dummy gate layer is dry etching; in other embodiments, the process of removing the dummy gate layer may also be plasma etching and wet etching performed in sequence.

[0058] Please refer to Figure 4 and Figure 5 , Figure 5 yes Figure 4 The cross-sectional diagram along line AA. It should be noted that: Figure 5 and Figure 3 A portion of the gate structure 201 is removed, and a trench 206 is formed in the gate structure 201. The trench 206 penetrates the gate structure 201 along a second direction, and the second direction is different from the first direction.

[0059] In this embodiment, removing the gate structure 201 forms metal residues 212 and non-metal residues 210 at the bottom of the trench 206 ; the non-metal residues 210 are formed when etching the sidewalls 204 ; the metal residues 212 are formed when etching the gate layer 203 .

[0060] In this embodiment, the method for forming the trench 206 includes: forming a mask structure 207 on the dielectric layer 202 and the gate structure 201, wherein the mask structure 207 exposes a portion of the gate structure 201; and etching the gate layer 203 and the sidewall 204 using the mask structure 207 as a mask to form the trench 206. In this embodiment, the mask structure 207 includes a first mask layer 208 and a second mask layer 209 located on the first mask layer 208, and the first mask layer 208 and the second mask layer 209 are made of different materials.

[0061] In the present embodiment, the material of the first mask layer 208 is nitrogen-doped silicon carbide. The first mask layer 208 formed by the nitrogen-doped silicon carbide has good bonding ability with the dielectric layer 202. When the gate structure 201 is subsequently etched using the etched first mask layer 208 as a mask, the first mask layer 208 is not prone to peeling or warping. Therefore, the first mask layer 208 has a good ability to maintain the etching pattern, which is beneficial to making the opening morphology formed in the gate structure 201 good, and effectively improving the accuracy of the pattern after etching.

[0062] In this embodiment, the material of the second mask layer 209 is titanium nitride; the second mask layer 209 has good bonding ability with the first mask layer 208, and the second mask layer 209 can protect the surface of the first mask layer 208 when the layer to be etched is subsequently etched, so that the first mask layer 208 will not be thinned; moreover, the physical strength of the second mask layer 208 is relatively large, and when the gate structure 201 is subsequently etched, the patterns of the second mask layer 209 and the first mask layer 208 can remain stable, which is conducive to forming an opening with a good morphology.

[0063] In other embodiments, the material of the second mask layer may be silicon carbide, silicon carbonitride, silicon carbonitride oxide, silicon nitride oxide, boron nitride or boron carbonitride.

[0064] In other embodiments, the mask structure may also adopt a single-layer structure; the material of the single-layer mask structure may be silicon nitride, silicon carbide, silicon carbonitride, silicon carbonitride oxide, silicon nitride oxide, boron nitride or boron carbonitride.

[0065] In this embodiment, the mask structure 207 and the method for forming the mask structure 207 that exposes a portion of the gate structure 201 include: forming a first initial mask layer on the dielectric layer 202; forming a second initial mask layer on the first initial mask layer; forming a patterned layer (not shown) on the second initial mask layer, the patterned layer having a patterned opening that exposes a portion of the surface of the second initial mask layer, and the patterned opening extending along the second direction; etching portions of the first initial mask layer and the second initial mask layer using the second patterned layer as a mask until the top surface of the dielectric layer 202 is exposed, thereby forming the first mask layer 208, the second mask layer 209, and the second opening that exposes the portion of the gate structure 201; after forming the first mask layer 208, the second mask layer 209, and the second opening that exposes the portion of the gate structure 201, removing the patterned layer.

[0066] The material of the patterned layer includes photoresist, and the process of forming the patterned layer includes a photolithography patterning process; the process of removing the patterned layer includes a wet stripping process or an ashing process, and the gas of the ashing process is an oxygen-containing gas, such as oxygen or ozone.

[0067] In this embodiment, the material of the first initial mask layer is nitrogen-doped silicon oxycarbide, and the process for forming the first initial mask layer adopts a chemical vapor deposition process, wherein the chemical vapor deposition process is as follows: the gas includes SiH4, CO2 and N2O, the flow rate of SiH4 is 10 standard ml / min to 10000 standard ml / min, the flow rate of CO2 is 10 standard ml / min to 10000 standard ml / min, the flow rate of N2O is 10 standard ml / min to 10000 standard ml / min, the gas pressure is 0.1 Torr to 10 Torr, and the power is 100 W to 5000 W. Among them, SiH4 gas and CO2 gas react to form silicon oxycarbide, and N2O gas is used to in-situ dope nitrogen ions in the silicon oxycarbide during the process of forming the silicon oxycarbide, and the nitrogen ions in the silicon oxycarbide are evenly distributed, so that the performance of the formed first initial mask layer is stable.

[0068] In this embodiment, the second initial mask layer is formed by an atomic layer deposition process; in other embodiments, the second initial mask layer may be formed by a chemical vapor deposition process, a physical vapor deposition process, or a spin coating process.

[0069] In this embodiment, there are multiple gate structures 201 , and the multiple gate structures 201 are all parallel to the first direction.

[0070] The trench 206 penetrates one or more gate structures 201 . In the present embodiment, the trench 206 penetrates a plurality of the gate structures 201 .

[0071] In this embodiment, the first direction and the second direction are perpendicular to each other; in other embodiments, the angle between the first direction and the second direction may be an acute angle or an obtuse angle.

[0072] See also Figure 6 and Figure 7 , Figure 7 yes Figure 6 The schematic cross-sectional view along line AA shows that after the trench 206 is formed, the first mask layer 208 and the second mask layer 209 are removed.

[0073] The process of removing the first mask layer and the second mask layer includes: a dry etching process or a wet etching process. In this embodiment, the process of removing the first mask layer and the second mask layer is a dry etching process.

[0074] In this embodiment, the groove 206 is subsequently subjected to a first cleaning process, and the first cleaning process is used to remove the non-metallic residue 210; the method of the first cleaning process includes: performing a plasma treatment on the groove 206; after the plasma treatment, performing a cleaning process on the groove 206. For details, please refer to Figures 8 to 10 .

[0075] Please refer to Figure 8 and Fig. 9 , Fig. 9 yes Figure 8 The schematic cross-sectional view along line AA shows that the trench 206 is subjected to plasma treatment.

[0076] The non-metallic residue 210 includes nitride or oxide. In the present embodiment, the non-metallic residue 210 is nitride, and the trench 206 is first subjected to plasma treatment to form an intermediate 211 with the non-metallic oxide 210. The plasma treatment process includes: the gas used is hydrogen (H2) or helium (He), the gas flow rate is 10sccm to 1000sccm, the power is 50W to 2000W, the bias voltage is 0V to 5000V, and the temperature is 30°C to 150°C.

[0077] In other embodiments, the non-metallic residue is an oxide, and the process parameters of the plasma treatment include: the gas used is hydrogen (H2) or argon (Ar), the gas flow rate is 10sccm~1000sccm, the power is 50W~2000W, the bias voltage is 0V~5000V, and the temperature is 30℃~150℃.

[0078] Please refer to Fig.10 It should be noted that Fig.10 and Figure 8 The viewing direction is consistent with that of FIG. 2 . After the plasma treatment, the trench 206 is cleaned. The intermediate 211 is removed by cleaning the trench 206, thereby removing the non-metallic residue 210.

[0079] In this embodiment, the cleaning process is a SiCoNi process, and the parameters of the SiCoNi process include: the gas is nitrogen trifluoride (NF3) or ammonia (NH3), the gas flow rate is 100 sccm to 2000 sccm; the temperature is less than 50°C.

[0080] In this embodiment, the SiCoNi process is used to remove the intermediate 211 with good isotropy.

[0081] See also Fig.11 , the groove 206 is subjected to a second cleaning process, wherein the second cleaning process is used to remove the metal residue 212 .

[0082] The second cleaning process includes dry cleaning or wet cleaning. In the present embodiment, the second cleaning process adopts dry cleaning, and the dry cleaning process includes: the gas is carbon tetrafluoride, sulfur hexafluoride or boron trichloride; the gas flow rate is 5sccm~500sccm, the power is 50W~1500W, the bias voltage is 50V~2000V, and the temperature is less than 150°C.

[0083] In other embodiments, the second cleaning process uses wet cleaning, and the solution used for the wet cleaning is concentrated sulfuric acid and hydrogen peroxide.

[0084] In this embodiment, the second cleaning process is performed after the first cleaning process. The non-metallic residue 210 is first removed by the first cleaning process, so that the metal residue 212 can be exposed as much as possible, so that the subsequent second cleaning process can completely remove the metal residue 212 as much as possible.

[0085] If the second cleaning process is performed first to remove the metal residue 212, a portion of the metal residue 212 will be mixed with the non-metal residue 210 and cannot be removed. After the first cleaning process is performed to remove the non-metal residue 210, these mixed remaining metal residues 212 can be exposed and processed. At this time, it is necessary to perform a process to remove the metal residue 212. This process will increase the cleaning process, which will not only increase the processing cost, but also reduce the processing efficiency.

[0086] See also Fig.12 After the first cleaning process and the second cleaning process, an isolation layer 213 is formed in the trench 206 .

[0087] The purpose of forming the isolation layer 213 is to fill the groove in the groove 206 to prevent the metal residue 212 from filling the groove in the future, causing the gate layer 203 on both sides of the groove 206 to form a conductive path and cause leakage, which will affect the final performance and yield of the finished product.

[0088] The material of the isolation layer 213 is one or more combinations of silicon oxide, silicon nitride, silicon oxynitride, low-K dielectric material (low-k dielectric material refers to dielectric material with a relative dielectric constant lower than 3.9) and ultra-low-k dielectric material (ultra-low-k dielectric material refers to dielectric material with a relative dielectric constant lower than 2.5); in the present embodiment, the material of the isolation layer 213 is silicon oxide.

[0089] In this embodiment, the method for forming the isolation layer 213 includes: forming an initial isolation layer on the bottom surface of the trench 206 ; and planarizing the initial isolation layer to form the isolation layer 213 .

[0090] The process of forming the initial isolation layer includes: the atomic layer is formed by chemical vapor deposition, physical vapor deposition, atomic layer deposition process or spin coating process; in this embodiment, the process of forming the initial isolation layer is atomic layer deposition process.

[0091] The process of planarizing the initial isolation layer includes an etching process or a chemical mechanical polishing process; in this embodiment, the process of planarizing the initial isolation layer is a chemical mechanical polishing process.

[0092] Please continue to refer to Fig.11 An embodiment of the present invention also provides a semiconductor structure formed by the above method.

[0093] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A method for forming a semiconductor structure, characterized in that: include: providing a substrate; A gate structure and a dielectric layer are formed on the substrate, wherein the gate structure comprises: a gate layer, a sidewall located on the sidewall surface of the gate layer, and a gate dielectric layer located on the substrate, wherein the gate layer is located on the gate dielectric layer, the gate structure extends along a first direction, and the dielectric layer covers the sidewall of the gate structure and exposes the top surface of the gate structure; wherein, The method for forming the dielectric layer and the gate structure comprises: forming a dummy gate layer on the substrate; forming the sidewall on the sidewall surface of the dummy gate layer; forming an initial dielectric layer on the substrate, the initial dielectric layer covering the dummy gate layer and the sidewall; flattening the initial dielectric layer until the dummy gate layer is exposed to form the dielectric layer; after forming the dielectric layer, removing the dummy gate layer to form a first opening; forming the gate dielectric layer on the bottom surface of the first opening; and forming the gate layer on the gate dielectric layer. removing a portion of the gate structure to form a trench in the gate structure, wherein the trench penetrates the gate structure along a second direction, and the second direction is different from the first direction; Performing a first cleaning process on the groove, wherein the first cleaning process is used to remove non-metallic residues; The trench is subjected to a second cleaning process, wherein the second cleaning process is used to remove metal residues.

2. The method for forming a semiconductor structure according to claim 1, wherein: The material of the gate dielectric layer includes a high-K dielectric material.

3. The method for forming a semiconductor structure according to claim 1, wherein: The material of the gate layer includes metal; the material of the sidewall spacer includes one or more combinations of silicon nitride, silicon oxide and silicon oxynitride.

4. The method for forming a semiconductor structure according to claim 1 or 3, characterized in that: The method for forming the trench comprises: forming a mask structure on the dielectric layer and the gate structure, wherein the mask structure exposes a portion of the gate structure; and etching the gate layer and the sidewall using the mask structure as a mask to form the trench.

5. The method for forming a semiconductor structure according to claim 4, wherein: The mask structure includes a first mask layer and a second mask layer located on the first mask layer; a material of the first mask layer is different from a material of the second mask layer.

6. The method for forming a semiconductor structure according to claim 5, wherein: The material of the first mask layer is nitrogen-doped silicon oxycarbide; the material of the second mask layer is titanium nitride, silicon carbide, silicon carbonitride, silicon carbonitride oxide, silicon oxynitride, boron nitride or boron carbonitride.

7. The method for forming a semiconductor structure according to claim 1, wherein: There are multiple gate structures, and the multiple gate structures are parallel to the first direction; the trench runs through the multiple gate structures.

8. The method for forming a semiconductor structure according to claim 1, wherein: The method of the first cleaning treatment includes: performing a plasma treatment on the trench; and performing a cleaning process on the trench after the plasma treatment.

9. The method for forming a semiconductor structure according to claim 4, wherein: The sidewall spacer is etched to form a non-metallic residue, wherein the non-metallic residue comprises a nitride or an oxide; and the gate layer is etched to form a metal residue.

10. The method for forming a semiconductor structure according to claim 8, wherein: The plasma treatment process includes: the gas is hydrogen, helium or argon, and the gas flow rate is 10 sccm to 1000 sccm; The power is 50W~2000W, the bias is 0V~5000V, and the temperature is 30℃~150℃.

11. The method for forming a semiconductor structure according to claim 8, wherein: The cleaning process is a SiCoNi process; the SiCoNi process includes: the gas is nitrogen trifluoride or ammonia, the gas flow rate is 100 sccm to 2000 sccm, and the temperature is less than 50°C.

12. The method for forming a semiconductor structure according to claim 1, wherein: The second cleaning process includes dry cleaning or wet cleaning.

13. The method for forming a semiconductor structure according to claim 12, wherein: The dry cleaning process includes: the gas is carbon tetrafluoride, sulfur hexafluoride or boron trichloride, the gas flow rate is 5sccm-500sccm, the power is 50W-1500W, the bias voltage is 50V-2000V; and the temperature is less than 150°C.

14. The method for forming a semiconductor structure according to claim 12, wherein: The solution used for the wet cleaning is concentrated sulfuric acid and hydrogen peroxide.

15. The method for forming a semiconductor structure according to claim 1, wherein: After the first cleaning process is performed, the second cleaning process is performed.

16. The method for forming a semiconductor structure according to claim 1, wherein: After performing the first cleaning process and the second cleaning process, the method further includes: forming an isolation layer in the groove; the material of the isolation layer includes one or more combinations of silicon oxide, silicon nitride, silicon oxynitride, low-K dielectric material and ultra-low-K dielectric material.

17. A semiconductor structure formed by the method of any one of claims 1 to 16.

Citation Information

Patent Citations

  • Fin shape for fin field-effect transistors and method of forming

    CN104051266A

  • Transistor forming method

    CN104701170A

  • Metal gate, semiconductor device and manufacturing method thereof

    CN109786448A

  • Method for manufacturing semiconductor device with trenches in substrate surface

    US20060154438A1