Negative electrode for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery

By using a composite material layer with a double-layer structure on the negative electrode of the nonaqueous electrolyte secondary battery, the combination of Si-based active substances and high-tap density carbon-based active substances is solved, the problem of conducting paths detached during charge and discharge of Si-based active substances is solved. , improves the input characteristics, cycle characteristics and high-temperature storage characteristics of the battery.

CN112385059BActive Publication Date: 2024-11-22PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980044985.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-07-25
Filing Date
2019-03-18
Publication Date
2024-11-22
Estimated Expiration
2039-03-18

AI Technical Summary

Technical Problem

During the charge and discharge cycle of Si-based active substance negative electrode, it is prone to volume changes, causing the conductive path to detach, resulting in the decline of the battery input characteristics, circulation characteristics and high-temperature storage characteristics. The existing technology is prone to more battery performance when adding bonding materials or conductive materials. On the one hand, it has declined.

Method used

Using a two-layer structure of a negative electrode composite material layer, the first layer contains Si-based active substance, polyacrylic acid or its salt and fibrous carbon, and the second layer contains carbon-based active substances with a tap density higher than that of the first layer, through this The structural design improves the input characteristics, cycle characteristics and high-temperature storage characteristics of the battery.

Benefits of technology

The high capacity of the Si-based active material negative electrode is achieved, the input characteristics, circulation characteristics and high temperature storage characteristics of the battery are improved, and the performance reduction in the single-layer structure is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112385059B_ABST
    Figure CN112385059B_ABST
Patent Text Reader

Abstract

In a negative electrode for a non-aqueous electrolyte secondary battery, the negative electrode composite material layer comprises: a first layer, comprising a first carbon-based active material, a Si-based active material, polyacrylic acid or a salt thereof, and fibrous carbon, and formed on a negative electrode collector; and a second layer, comprising a second carbon-based active material having a tap density greater than that of the first carbon-based active material and formed on the first layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a negative electrode for a nonaqueous electrolyte secondary battery and a nonaqueous electrolyte secondary battery. Background Art

[0002] It is known that Si-containing compounds can absorb more lithium ions per unit volume than carbon-based active materials such as graphite. For example, Patent Document 1 discloses a negative electrode for a non-aqueous electrolyte secondary battery, which has a negative electrode composite material layer containing Si-containing compounds and graphite as negative electrode active materials. In addition, in the negative electrode disclosed in Patent Document 1, a carbon-containing layer containing carbon and a binding material is formed on the surface of the negative electrode composite material layer on the side opposite to the positive electrode with a thickness of less than 10% of the thickness of the negative electrode composite material layer.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2012-3997 Summary of the invention

[0006] However, for negative electrodes containing Si-based active materials, the decline in charge and discharge cycle characteristics is prone to become a problem. It is generally believed that the main reason is that due to the large volume change of Si-based active materials accompanying charge and discharge, the contact degree between the particles of the negative electrode active material becomes weaker or the contact state disappears, and the number of negative electrode active material particles detached from the conductive path in the negative electrode composite material layer increases. In order to suppress the detachment of such negative electrode active materials (Si-based active materials), countermeasures such as increasing the amount of binding materials and adding conductive materials are considered, but it is expected that at this time, undesirable conditions such as a decrease in the input characteristics of the battery or a decrease in the storage characteristics will occur.

[0007] An object of the present disclosure is to provide a negative electrode for a nonaqueous electrolyte secondary battery, which is a high-capacity negative electrode containing a Si-based active material and can improve the input characteristics, cycle characteristics, and high-temperature storage characteristics of the nonaqueous electrolyte secondary battery.

[0008] A negative electrode for a non-aqueous electrolyte secondary battery as one embodiment of the present disclosure comprises a negative electrode collector and a negative electrode composite material layer formed on the negative electrode collector. The negative electrode composite material layer comprises: a first layer, comprising a first carbon-based active material, a Si-based active material, polyacrylic acid or a salt thereof, and fibrous carbon, and formed on the negative electrode collector; and a second layer, comprising a second carbon-based active material having a tap density greater than that of the first carbon-based active material and formed on the first layer.

[0009] A nonaqueous electrolyte secondary battery as one embodiment of the present disclosure is characterized by comprising the above-mentioned negative electrode for a nonaqueous electrolyte secondary battery, a positive electrode, and a nonaqueous electrolyte.

[0010] According to the negative electrode for a nonaqueous electrolyte secondary battery of the present disclosure, it is possible to provide a nonaqueous electrolyte secondary battery having a high capacity using a Si-based active material and having excellent input characteristics, cycle characteristics, and high-temperature storage characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 It is a perspective view showing a nonaqueous electrolyte secondary battery as an example of an embodiment.

[0012] Figure 2 It is a cross-sectional view of a negative electrode as an example of an embodiment. DETAILED DESCRIPTION

[0013] As mentioned above, for a non-aqueous electrolyte secondary battery using a high-capacity negative electrode containing a Si-based active material, achieving good input characteristics, cycle characteristics and high-temperature storage characteristics is an important issue. However, if the amount of the binding material of the negative electrode composite layer is increased in order to improve the cycle characteristics, the input characteristics will usually decrease. In addition, if a conductive material is added to the negative electrode composite layer in order to improve the cycle characteristics, the storage characteristics will usually decrease. Alternatively, when a carbon-based active material with a fast insertion speed of lithium ions is used to improve the input characteristics, for example, the negative electrode active material particles detached from the conductive path increase and the cycle characteristics will decrease. As a result, it is not easy to improve all the performance of the above-mentioned batteries.

[0014] The present inventors have conducted in-depth research to solve the above-mentioned problems. As a result, by setting the negative electrode composite material layer to a double-layer structure having the above-mentioned first layer and the above-mentioned second layer, good input characteristics, cycle characteristics and high-temperature storage characteristics are successfully achieved. Hereinafter, the embodiments of the negative electrode for a non-aqueous electrolyte secondary battery and the non-aqueous electrolyte secondary battery disclosed in the present invention are described in detail with reference to the accompanying drawings.

[0015] Figure 1 1 is a perspective view showing a nonaqueous electrolyte secondary battery 10 as an example of an embodiment. Figure 1 The nonaqueous electrolyte secondary battery 10 shown as an example is a square battery, but the nonaqueous electrolyte secondary battery of the present disclosure is not limited thereto, and may also be a cylindrical battery having a cylindrical battery case, a laminated battery having an outer body formed of a laminated film including a metal layer, etc. It should be noted that in this specification, the description "numerical value (1) to numerical value (2)" means that the numerical value (1) is greater than or equal to the numerical value (2) and is less than or equal to the numerical value (2).

[0016] like Figure 1As shown, the nonaqueous electrolyte secondary battery 10 includes an electrode body 11, a nonaqueous electrolyte, and a square battery case 14 for accommodating the electrode body 11. The electrode body 11 has a positive electrode, a negative electrode, and a separator. The electrode body 11 is a laminated electrode body in which a plurality of positive electrodes and a plurality of negative electrodes are alternately laminated with a separator sandwiched therebetween. It should be noted that the electrode body is not limited thereto, and may also be a wound electrode body in which a long strip of positive electrode and a long strip of negative electrode are wound with a separator sandwiched therebetween.

[0017] The battery case 14 has a substantially box-shaped case body 15, a sealing body 16 that blocks the opening of the case body 15, a positive terminal 12 electrically connected to the positive electrode, and a negative terminal 13 electrically connected to the negative electrode. The case body 15 and the sealing body 16 are made of, for example, a metal material having aluminum as a main component. The positive terminal 12 and the negative terminal 13 are fixed to the sealing body 16 with an insulating member 17 sandwiched therebetween. Usually, the sealing body 16 is provided with a gas exhaust mechanism (not shown).

[0018] The positive electrode, the negative electrode, the separator, and the nonaqueous electrolyte constituting the nonaqueous electrolyte secondary battery 10 , particularly the negative electrode, will be described in detail below.

[0019] [positive electrode]

[0020] The positive electrode includes a positive electrode collector and a positive electrode composite material layer formed on the positive electrode collector. As the positive electrode collector, a foil of a metal such as aluminum or aluminum alloy that is stable within the potential range of the positive electrode, a film having the metal disposed on the surface, etc. can be used. The positive electrode composite material layer includes, for example, a positive electrode active material, a binding material, and a conductive material. The positive electrode composite material layer is preferably formed on both surfaces of the positive electrode collector. The positive electrode can be manufactured, for example, as follows: a positive electrode composite material slurry including a positive electrode active material, a binding material, a conductive material, etc. is applied to the positive electrode collector, and the coating is dried and rolled to form a positive electrode composite material layer on both surfaces of the positive electrode collector, thereby manufacturing.

[0021] The positive electrode active material is composed of a lithium-containing metal composite oxide as a main component. As the metal elements contained in the lithium-containing metal composite oxide, Ni, Co, Mn, Al, B, Mg, Ti, V, Cr, Fe, Cu, Zn, Ga, Sr, Zr, Nb, In, Sn, Ta, W, Ca, Sb, Pb, Bi, Ge, etc. can be exemplified. An example of a suitable lithium-containing metal composite oxide is a composite oxide containing at least one of Ni, Co, Mn, and Al.

[0022] As the conductive material contained in the positive electrode composite material layer, carbon materials such as carbon black, acetylene black, Ketjen black, and graphite can be exemplified. As the binding material contained in the positive electrode composite material layer, fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyimide, acrylic resin, polyolefin, etc. can be exemplified. These resins can also be used in combination with carboxymethyl cellulose (CMC) or its salt, polyethylene oxide (PEO), etc.

[0023] [negative electrode]

[0024] Figure 2 2 is a cross-sectional view of a negative electrode 20 as an example of an embodiment. Figure 2 As shown, the negative electrode 20 includes a negative electrode current collector 30 and a negative electrode composite material layer 31 formed on the negative electrode current collector 30. As the negative electrode current collector 30, a foil of a metal such as copper or a copper alloy that is stable in the potential range of the negative electrode, a film having the metal disposed on the surface, etc. can be used. The negative electrode composite material layer 31 is preferably formed on both surfaces of the negative electrode current collector 30. The negative electrode 20 can be manufactured, for example, as follows: a negative electrode composite material slurry containing a negative electrode active material, a binding material, etc. is applied to the negative electrode current collector 30, and the coating is dried and rolled to form the negative electrode composite material layer 31 on both surfaces of the negative electrode current collector 30, thereby manufacturing.

[0025] The negative electrode composite material layer 31 has a double-layer structure consisting of a first layer 32 formed on the negative electrode collector 30 and a second layer 33 formed on the first layer 32. The first layer 32 is a layer (lower layer) containing a first carbon-based active material, a Si-based active material, polyacrylic acid or a salt thereof, and fibrous carbon. The second layer 33 is a layer (upper layer) containing a second carbon-based active material. The second layer 33 is a layer in which the content of Si-based active material is lower than that of the first layer 32, or is a layer that does not substantially contain Si-based active material. From the viewpoint of improving the input characteristics of the battery, etc., the second layer 33 preferably contains only carbon-based active materials as negative electrode active materials and does not substantially contain Si-based active materials (for example, less than 0.1% by mass relative to the mass of the second layer 33).

[0026] The tap density of the second carbon-based active material contained in the second layer 33 is greater than the tap density of the first carbon-based active material contained in the first layer 32. It should be noted that as long as the tap density of the second carbon-based active material is greater than the tap density of the first carbon-based active material when comparing the total amount of each carbon-based active material contained in the first layer 32 and the second layer 33.

[0027] The mass of the first layer 32 is 50% by mass or more and less than 90% by mass, preferably 50% to 70% by mass, relative to the mass of the negative electrode composite material layer 31. In addition, the mass of the second layer 33 is more than 10% by mass and less than 50% by mass, preferably 30% to 50% by mass, relative to the mass of the negative electrode composite material layer 31. That is, the mass ratio of the first layer 32 to the second layer 33 (second layer 33 / first layer 32) is more than 0.1 and less than 0.5, preferably 0.3 to 0.5.

[0028] If the mass of the first layer 32 is 90% or more relative to the mass of the negative electrode composite material layer 31, and the mass of the second layer 33 is 10% or less relative to the mass of the negative electrode composite material layer 31, for example, the proportion of the second layer 33 that helps to improve the input characteristics is reduced, and the input characteristics of the battery are reduced. In addition, if the mass of the first layer 32 is less than 50% by mass relative to the mass of the negative electrode composite material layer 31, and the mass of the second layer 33 is more than 50% by mass relative to the mass of the negative electrode composite material layer 31, the proportion of the first layer 32 is reduced (that is, the amount of Si-based active material is reduced), and it is difficult to achieve a high capacity of the battery.

[0029] From the perspective of improving battery capacity, the packing density of the negative electrode composite material layer 31 is preferably 1.65 g / cm 3 The packing density of the negative electrode composite material layer 31 is, for example, 1.65 g / cm 3 ~1.75g / cm 3 The packing density of the first layer 32 and the second layer 33 may be the same or different. The packing density of the second layer 33 is, for example, lower than the packing density of the first layer 32. An example of the packing density of the second layer 33 is 1.40 g / cm 3 ~1.55g / cm 3 An example of the packing density of the first layer 32 is 1.70 g / cm 3 ~1.95g / cm 3 .

[0030] The thickness of the negative electrode composite material layer 31 is, for example, 30 μm to 100 μm or 50 μm to 80 μm, measured on one side of the negative electrode current collector 30. The thicknesses of the first layer 32 and the second layer 33 may be the same or different from each other as long as they satisfy the above-mentioned mass ratio. The thickness of the first layer 32 may be larger or smaller than the thickness of the second layer 33. It should be noted that the negative electrode composite material layer 31 may include layers other than the first layer 32 and the second layer 33, without prejudice to the purpose of the present disclosure.

[0031] As the first and second carbon-based active materials, for example, graphite, amorphous carbon, etc. are used. Among them, graphite is preferred. As graphite, natural graphite such as flaky graphite, blocky artificial graphite, artificial graphite such as graphitized mesophase carbon microspheres, etc. can be listed. In addition, a conductive coating layer such as amorphous carbon can be formed on the surface of the graphite particles. As the first and second carbon-based active materials, one type of graphite, etc. can be used alone, or two or more types of graphite, etc. can be used.

[0032] The first carbon-based active material is preferably an active material that can alleviate the volume change of the Si-based active material. On the other hand, the second carbon-based active material is preferably an active material that has high reactivity for accepting lithium ions and helps to improve input characteristics. The first carbon-based active material is, for example, softer than the second carbon-based active material and is easily crushed during rolling of the electrode plate. In other words, the second carbon-based active material is harder than the first carbon-based active material and is not easily crushed during rolling. The first and second carbon-based active materials are, for example, graphite having a conductive coating layer such as amorphous carbon formed on the surface of the particles, and the amount of the coating layer on the surface of the particles of the second carbon-based active material is greater than the amount of the coating layer on the surface of the particles of the first carbon-based active material. There is a tendency that the more the amount of the coating layer, the harder the graphite particles.

[0033] The tap density of the second carbon-based active material contained in the second layer 33 is preferably higher than the tap density of the first carbon-based active material contained in the first layer 32. When the tap density of the active material particles is high, it is easier to fill in the space, so the degree of contact between the active material particles becomes larger to form a good conductive path, and the input characteristics of the battery are improved. In the negative electrode composite material layer 31, by using a second carbon-based active material with a high tap density in the second layer 33, the movement of lithium ions in the second layer 33 becomes smooth. As a result, the input characteristics of the battery are improved.

[0034] An example of the tap density of the first carbon-based active material is 0.85 g / cm 3 ~1.00g / cm 3 , preferably 0.89 g / cm 3 ~0.95g / cm 3 The tap density of the second carbon-based active material is, for example, 1.00 g / cm 3 Above, preferably 1.00 g / cm 3 ~1.25g / cm 3 The tap density of the carbon-based active material can be measured by the method specified in JIS Z-2504. In this specification, the bulk density after the sample powder collected in the container is tapped 250 times is referred to as the tap density.

[0035] Preferably, the BET specific surface area of ​​the second carbon-based active material contained in the second layer 33 is greater than the BET specific surface area of ​​the first carbon-based active material contained in the first layer 32. If the BET specific surface area of ​​the active material particles increases, the reaction area increases, so the reactivity of accepting lithium ions increases. In the negative electrode composite material layer 31, the input characteristics of the battery are improved by using a second carbon-based active material with a large BET specific surface area in the second layer 33. It should be noted that if the BET specific surface area of ​​the active material particles increases, the amount of the conductive coating layer increases and the particles become harder. The first carbon-based active material with a small BET specific surface area, such as the conductive coating layer, has a smaller amount than the second carbon-based active material and is softer. Therefore, compared with the second carbon-based active material, the first carbon-based active material is more able to mitigate the volume change of the Si-based active material.

[0036] An example of the BET specific surface area of ​​the first carbon-based active material is 0.9 m 2 / g~6.5m 2 / g, the BET specific surface area of ​​the second carbon-based active material is larger than the BET specific surface area of ​​the first carbon-based active material, for example, 2.5 m 2 / g~8.0m 2 The BET specific surface area can be measured according to the BET method (nitrogen adsorption method) described in JIS R1626.

[0037] The first and second carbon-based active materials are usually secondary particles formed by the aggregation of multiple primary particles. The average particle size of the first and second carbon-based active materials (secondary particles) is not particularly limited, for example, 1 μm to 30 μm. The average particle size of the first and second carbon-based active materials refers to: in the particle size distribution measured by laser diffraction scattering method, the volume cumulative value reaches 50% of the volume average particle size (Dv50).

[0038] As described above, the first layer 32 contains Si-based active material, polyacrylic acid (PAA) or its salt, and fibrous carbon in addition to the first carbon-based active material. PAA or its salt firmly binds the negative electrode active material (Si-based active material and first carbon-based active material) particles to each other, so even if the volume of the Si-based active material changes greatly with charge and discharge, the increase in the negative electrode active material particles that are separated from the conductive path in the first layer 32 is suppressed. Therefore, by adding PAA or its salt to the first layer 32, the decline in cycle characteristics is suppressed. In addition, like PAA or its salt, fibrous carbon also forms a good conductive path in the first layer 32.

[0039] The Si-based active material is at least one of Si and a Si-containing compound, and preferably a Si-containing compound whose volume change during charge and discharge is smaller than that of Si. The Si-containing compound is not particularly limited as long as it is a compound containing Si, and preferably SiO x(0.5≤x≤1.5). The Si-containing compound may be used alone or in combination of two or more. It is preferred that a conductive coating composed of a material having a higher conductivity than the compound is formed on the surface of the particles of the Si-containing compound. The average particle size (Dv50) of the Si-containing compound is, for example, 1 μm to 15 μm.

[0040] SiO x For example, in amorphous SiO 2 The structure of Si is dispersed in the matrix. x Lithium silicate (e.g. Li 2z SiO (2+z) The lithium silicate represented by (0<z<2)) may have a structure in which Si is dispersed in the lithium silicate phase.

[0041] The conductive film is preferably a carbon film. x The carbon coating is formed in an amount of 0.5 mass % to 10 mass % of the mass of the particles. As a method for forming the carbon coating, there can be exemplified a method of mixing coal tar or the like with Si-containing compound particles and heat treating them, a chemical deposition method (CVD method) using hydrocarbon gas or the like, etc. In addition, a carbon coating can be formed by fixing carbon black, Ketjen black, etc. to the surface of the Si-containing compound particles using a binding material.

[0042] The mass ratio of the first carbon-based active material to the Si-based active material contained in the first layer 32 is, for example, 95:5 to 70:30, preferably 95:5 to 80:20. If the mass ratio is within this range, the battery can be increased in capacity and the volume change of the Si-based active material can be mitigated by the first carbon-based active material, making it easy to suppress the decrease in cycle characteristics. In the first layer 32, the proportion of the Si-based active material in the negative electrode active material is preferably 5% to 20% by mass, and more preferably 5% to 15% by mass.

[0043] PAA or its salt contained in the first layer 32 acts as a binder. The salt of PAA is, for example, a lithium salt, a sodium salt, a potassium salt, and an ammonium salt. Preferably, the first layer 32 contains a second binder in addition to PAA and its salt. Examples of the second binder include CMC or its salt, styrene-butadiene copolymer (SBR), polyvinyl alcohol (PVA), PEO, and the like. Among them, CMC or its salt and SBR are preferred. The first layer 32 contains, for example, PAA or its salt, CMC or its salt, and SBR as a binder.

[0044] As the binder contained in the second layer 33, CMC or its salt, SBR, PVA, PEO, etc. can be exemplified. Among them, CMC or its salt and SBR are preferred. The second layer 33 is a layer in which the content of PAA or its salt is lower than that of the first layer 32, or a layer that does not substantially contain PAA or its salt. Considering the input characteristics of the battery, it is preferred that the second layer 33 does not substantially contain PAA or its salt (for example, less than 0.1% by mass relative to the mass of the binder contained in the second layer 33). That is, it is preferred that PAA or its salt is contained only in the first layer 32. The second layer 33, for example, contains CMC or its salt and SBR as a binder.

[0045] The content of the binder contained in the first layer 32 is preferably greater than the content of the binder contained in the second layer 33. In this case, it is easy to suppress the decrease in the cycle characteristics of the battery and improve the input characteristics. Regarding the content of the binder contained in the first layer 32, for example, it is preferably 0.5% by mass to 10% by mass relative to the mass of the first layer 32, and more preferably 1% by mass to 5% by mass. From the viewpoint of suppressing the decrease in cycle characteristics, the content of PAA or its salt is preferably 20% by mass or more, for example, 20% by mass to 50% by mass, relative to the mass of the binder in the first layer 32. Regarding the content of the binder contained in the second layer 33, for example, it is preferably 0.5% by mass to 10% by mass relative to the mass of the second layer 33, and more preferably 1% by mass to 5% by mass.

[0046] The fibrous carbon contained in the first layer 32 acts as a conductive material and forms a good conductive path in the first layer 32. Even if the volume of the Si-based active material changes significantly due to charging and discharging, the conductive path formed by the fibrous carbon is not easily cut off. The fibrous carbon is, for example, a carbon material with an aspect ratio of 60 times or more, and has a size that can be added to the first layer 32. The second layer 33 is a layer in which the content of fibrous carbon is lower than that of the first layer 32, or a layer that does not substantially contain fibrous carbon. Considering the storage characteristics of the battery, it is preferred that the second layer 33 does not substantially contain fibrous carbon (for example, less than 0.001% by mass relative to the mass of the second layer 33). That is, it is preferred that the fibrous carbon is only contained in the first layer 32.

[0047] As fibrous carbon, carbon nanotubes (CNT), carbon nanofibers, etc. can be exemplified. CNT can be not only single-layer CNT, but also double-layer CNT, multi-layer CNT and a mixture thereof. In addition, CNT can be a vapor-deposited carbon fiber called VGCF (registered trademark). The diameter of the fibrous carbon is, for example, 2nm to 20μm, and the total length is, for example, 0.03μm to 500μm. Regarding the content of fibrous carbon, for example, relative to the mass of the first layer 32, it is preferably 0.01% to 5% by mass, and more preferably 0.5% to 3% by mass.

[0048] For example, the negative electrode 20 can be manufactured by the following method. A first negative electrode composite material slurry for the first layer 32 is prepared, which contains a first carbon-based active material, a Si-based active material, a binder containing PAA or a salt thereof, fibrous carbon, etc. In addition, a second negative electrode composite material slurry for the second layer 33 is prepared, which contains a second carbon-based active material, a binder, etc. Thereafter, the first negative electrode composite material slurry is applied to the negative electrode collector 30, and the coating is dried to form the first layer 32 on the negative electrode collector 30. Next, the second negative electrode composite material slurry is applied to the first layer 32, and the coating is dried to form the second layer 33 on the first layer 32, and then the first layer 32 and the second layer 33 are compressed. Thus, the negative electrode 20 in which the negative electrode composite material layer 31 including the first layer 32 and the second layer 33 is formed on the negative electrode collector 30 is obtained.

[0049] [Separator]

[0050] The separator may be a porous sheet having ion permeability and insulation. Specific examples of the porous sheet include microporous films, woven fabrics, nonwoven fabrics, etc. As the material of the separator, olefin resins such as polyethylene, polypropylene, copolymers containing at least one of ethylene and propylene, cellulose, etc. are suitable. The separator may be a single-layer structure or a laminated structure. A heat-resistant layer may be formed on the surface of the separator.

[0051] [Non-aqueous electrolyte]

[0052] The non-aqueous electrolyte includes a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. The non-aqueous electrolyte is not limited to a liquid electrolyte (non-aqueous electrolyte solution) and may also be a solid electrolyte using a gel polymer or the like. As the electrolyte salt, for example, LiBF 4 、LiPF 6 As the non-aqueous solvent, esters such as ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propionate (MP), ethers, nitriles, amides, and mixed solvents of two or more thereof can be used. The non-aqueous solvent may also contain a halogen substituted product formed by replacing at least a portion of hydrogen in the above-mentioned solvents with a halogen atom such as fluorine.

[0053] As halogen substitutes, for example, fluorinated cyclic carbonates such as fluorinated ethylene carbonate (FEC), fluorinated chain carbonates, fluorinated chain carboxylates such as fluoromethyl propionate (FMP), etc. can be cited. From the aspects of suppressing the reduction of the charge and discharge cycle characteristics of the non-aqueous electrolyte secondary battery 10 or improving its input characteristics, the non-aqueous electrolyte preferably contains 15% by mass or more of FEC relative to the mass of the non-aqueous electrolyte, and more preferably contains 15% to 25% by mass of FEC.

[0054] Example

[0055] Hereinafter, the present disclosure will be further described by way of examples, but the present disclosure is not limited to these examples.

[0056] <Example 1>

[0057] [positive electrode]

[0058] As the positive electrode active material, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 The lithium transition metal oxide shown. 94.8 parts by mass of the positive electrode active material, 4 parts by mass of acetylene black and 1.2 parts by mass of PVDF are mixed, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) is added to prepare a positive electrode composite material slurry. After that, the positive electrode composite material slurry is applied while leaving a portion of the connecting lead of the positive electrode collector formed by the aluminum foil, and the coating is dried. After rolling the coating with a roller, it is cut into a specified electrode size, thereby preparing a positive electrode having a positive electrode composite material layer formed on both surfaces of the positive electrode collector.

[0059] [negative electrode]

[0060] As the first carbonaceous active material constituting the first layer (lower layer), a carbonaceous active material having a tap density of 0.92 g / cm 3 , BET specific surface area is 4.2m 2 / g of graphite A. Graphite A, SiO x (x=0.94), a lithium salt of PAA, a sodium salt of CMC, a dispersion of CNT and SBR were mixed at a solid content mass ratio of 84.5 / 12 / 1 / 1 / 0.5 / 1, and an appropriate amount of water was added to prepare a first negative electrode composite material slurry for the first layer. In addition, as the second carbon-based active material constituting the second layer (upper layer), a carbon-based active material having a tap density of 1.06 g / cm 3 , BET specific surface area is 4.8m 2 / g of graphite B. A dispersion of graphite B, sodium salt of CMC and SBR was mixed at a solid content mass ratio of 98 / 1 / 1, and an appropriate amount of water was added to prepare a second negative electrode composite material slurry for the second layer.

[0061] Afterwards, the first negative electrode composite material slurry is applied to both surfaces of the negative electrode collector composed of copper foil, leaving the portion for connecting the lead, and the coating is dried, thereby forming the first layer on both surfaces of the negative electrode collector. Next, the second negative electrode composite material slurry is applied to the first layer formed on both surfaces of the negative electrode collector, and the coating is dried to form the second layer. Afterwards, the coating is rolled with a roller and cut into a predetermined electrode size, thereby producing a negative electrode having negative electrode composite material layers including the first layer and the second layer formed on both surfaces of the negative electrode collector.

[0062] The masses of the first layer and the second layer of the negative electrode composite material layer were measured, and the mass ratio of the second layer to the first layer was 1.0. In addition, the packing density of the negative electrode composite material layer was 1.65 g / cm 3 .

[0063] [Non-aqueous electrolyte]

[0064] 1 mass % of vinylene carbonate (VC) was added to a mixed solvent of ethylene carbonate (EC), fluoroethylene carbonate (FEC), and diethyl carbonate (DEC) in a volume ratio of 27:3:70, and LiPF was dissolved at a ratio of 1.2 mol / L. 6 , thereby preparing a non-aqueous electrolyte.

[0065] [Test battery]

[0066] Leads are installed on the negative electrode and the positive electrode respectively, and the electrodes are alternately stacked with separators to produce a laminated electrode body. As a separator, a single-layer polypropylene separator is used. The prepared electrode body is inserted into an outer body composed of an aluminum laminate, and after vacuum drying at 105°C for 2 hours and 30 minutes, the non-aqueous electrolyte is injected, and the opening of the outer body is sealed to produce a test battery (laminated battery). The design capacity of the test battery is 640mAh.

[0067] <Example 2>

[0068] In the preparation of the first negative electrode composite material slurry, graphite A, SiO x (x=0.94), the lithium salt of PAA, the sodium salt of CMC, the dispersion of CNT and SBR were mixed in a solid content mass ratio of 87.5 / 9 / 1 / 1 / 0.5 / 1, and in the preparation of the negative electrode, the first and second negative electrode composite material slurries were coated in such a way that the mass ratio of the second layer / the first layer reached 0.33. The test cell was prepared in the same manner as in Example 1. It should be noted that the packing density of the negative electrode composite material layer was 1.65 g / cm 3 .

[0069] <Comparative Example 1>

[0070] In the preparation of the negative electrode, graphite A, SiO x (x=0.94), the lithium salt of PAA, the sodium salt of CMC and the dispersion of SBR are mixed in a solid content mass ratio of 91 / 6 / 1 / 1 / 1, an appropriate amount of water is added, and the negative electrode composite material slurry prepared in this way is used to form a single-layer negative electrode composite material layer on both surfaces of the negative electrode collector. Except for this, a test battery is prepared in the same manner as Example 1.

[0071] <Comparative Example 2>

[0072] In the preparation of the negative electrode composite material slurry, graphite A, SiO x A test cell was prepared in the same manner as in Comparative Example 1 except that (x=0.94) the lithium salt of PAA, the sodium salt of CMC, and the dispersions of CNT and SBR were mixed at a solid content mass ratio of 90.5 / 6 / 1 / 1 / 0.5 / 1.

[0073] The performance of each of the test batteries was evaluated by the following method. The evaluation results are shown in Table 1 together with the structure of the negative electrode.

[0074] [Evaluation of initial charge and discharge efficiency]

[0075] Under a temperature environment of 25°C, the test battery was charged at a constant current of 0.5 It until the battery voltage reached 4.3 V, and then charged at a constant voltage at 4.3 V until the current value reached 1 / 50 It. After that, the constant current was discharged at a constant current of 0.5 It until the battery voltage reached 2.5 V. The initial charge and discharge efficiency was calculated from the charge capacity and discharge capacity. The initial charge and discharge efficiency shown in Table 1 is a relative value based on the charge and discharge efficiency of the test battery of Comparative Example 1 as a reference (100).

[0076] [Evaluation of capacity maintenance rate]

[0077] Under a temperature environment of 25°C, the test battery was charged at a constant current of 0.5It until the battery voltage reached 4.3V, and then charged at a constant voltage at 4.3V until the current value reached 1 / 50It. After that, the constant current was discharged at a constant current of 0.5It until the battery voltage reached 3.0V. In addition, the charge and discharge were cycled 200 times, and the capacity retention rate in the charge and discharge cycle was calculated based on the following formula. The capacity retention rate shown in Table 1 is a relative value based on the capacity retention rate of the test battery of Comparative Example 1 (100).

[0078] Capacity retention rate = (discharge capacity at the 200th cycle / discharge capacity at the 1st cycle) × 100

[0079] [Evaluation of input characteristics]

[0080] Under the temperature environment of 25℃ and -30℃, the test battery was charged to half of the initial capacity at a constant current of 0.5It, then the charging was stopped and left for 15 minutes. Then the voltage was measured after charging for 10 seconds at a current value of 0.1It. The amount of charging capacity for 10 seconds was discharged, and the voltage after charging for 10 seconds at the next current value was measured. The amount of charging capacity for 10 seconds was discharged, and the above operation was repeated at a current value of 0.1It to 2It. The current value at which the battery voltage reaches 4.3V after 10 seconds of charging was calculated from the measured voltage values, and the required power (input characteristics) at this time was obtained. The input characteristics shown in Table 1 are relative values ​​based on the above-mentioned required power of the test battery of Comparative Example 1 as the reference (100). Values ​​higher than 100 indicate that the input characteristics are better than those of the test battery of Comparative Example 1.

[0081] [Evaluation of high temperature storage characteristics]

[0082] Under a temperature environment of 25°C, the test battery was charged at a constant current of 0.5It until the battery voltage reached 4.3V, and then charged at a constant voltage at 4.3V until the current value reached 1 / 50It. Thereafter, constant current discharge was performed at a constant current of 0.5It until the battery voltage reached 2.5V(i). Thereafter, under a temperature environment of 25°C, the test battery was charged at a constant current of 0.5It until the battery voltage reached 4.3V, and then charged at a constant voltage at 4.3V until the current value reached 1 / 50It. A storage test was performed for 20 days in this charged state at a temperature environment of 60°C. Thereafter, constant current discharge was performed at a constant current of 0.5It until the battery voltage reached 2.5V(ii). Thereafter, under a temperature environment of 25°C, the test battery was charged at a constant current of 0.5It until the battery voltage reached 4.3V, and then charged at a constant voltage at 4.3V until the current value reached 1 / 50It. Thereafter, constant current discharge was performed at a constant current of 0.5 It until the battery voltage reached 2.5 V (iii).

[0083] The remaining capacity and the recovered capacity were calculated based on the following formula.

[0084] The remaining capacity and recovered capacity shown in Table 1 are relative values ​​with the remaining capacity and recovered capacity of the test battery of Comparative Example 1 as a reference (100).

[0085] Remaining capacity = (discharge capacity of (ii) / discharge capacity of (i)) × 100

[0086] Recovery capacity = (discharge capacity of (iii) / discharge capacity of (i)) × 100

[0087] [Table 1]

[0088]

[0089] As can be understood from the evaluation results shown in Table 1, the test battery of the embodiment is superior to the test battery of Comparative Example 1 in initial charge and discharge efficiency, input characteristics, cycle characteristics, and storage characteristics. The test battery of Comparative Example 2 is superior to the test battery of Comparative Example 1 in input characteristics, but the storage characteristics are particularly significantly reduced. That is, even if fibrous carbon is added to the negative electrode composite material layer of the single-layer structure, both the input characteristics and the storage characteristics cannot be achieved.

[0090] Description of Reference Numerals

[0091] 10 Non-aqueous electrolyte secondary battery

[0092] 11 Electrode body

[0093] 12 Positive terminal

[0094] 13 Negative terminal

[0095] 14 Battery housing

[0096] 15 Housing body

[0097] 16 Sealing body

[0098] 17 Insulation components

[0099] 20 Negative electrode

[0100] 30 Negative electrode collector

[0101] 31. Negative electrode composite material layer

[0102] 32 Layer 1

[0103] 33 Layer 2

Claims

1. A negative electrode for a non-aqueous electrolyte secondary battery, comprising a negative electrode current collector and a negative electrode composite material layer formed on the negative electrode current collector, The negative electrode composite material layer comprises: a first layer comprising a first carbon-based active material, a Si-based active material, polyacrylic acid or a salt thereof, and fibrous carbon, and formed on the negative electrode current collector; and a second layer comprising a second carbon-based active material having a larger tap density than the first carbon-based active material and formed on the first layer, The second layer does not contain the fibrous carbon, The mass of the first layer is 50 mass % or more and less than 90 mass % of the mass of the negative electrode mixture layer, and the mass of the second layer is more than 10 mass % and less than 50 mass % of the mass of the negative electrode mixture layer.

2. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein The BET specific surface area of ​​the first carbon-based active material is 0.9 m 2 / g~6.5m 2 / g, and the BET specific surface area of ​​the second carbon-based active material is 2.5 m 2 / g~8.0m 2 / g.

3. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein The tap density of the first carbon-based active material is 0.85 g / cm 3 ~1.00g / cm 3 .

4. The negative electrode for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 3, wherein The fibrous carbon is carbon nanotube.

5. The negative electrode for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 4, wherein The packing density of the negative electrode composite material layer is 1.65 g / cm 3 above. 6 . A non-aqueous electrolyte secondary battery comprising the negative electrode for a non-aqueous electrolyte secondary battery according to claim 1 , a positive electrode, and a non-aqueous electrolyte.

7. The nonaqueous electrolyte secondary battery according to claim 6, wherein The nonaqueous electrolyte contains 15 mass % or more of fluoroethylene carbonate.