Method for producing carbonate ester and catalyst structure for producing carbonate ester

By using an inorganic binder of alumina and silica to fix the cerium oxide catalyst on the substrate to form a multi-layer structure, the problem of catalyst powdering and detachment is solved, and the carbonate generation reaction efficiency and the long-term use ability of the catalyst are improved. .

CN112424155BActive Publication Date: 2024-10-29NIPPON STEEL CORPORATION +2
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN201980045509.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-07-08
Publication Date
2024-10-29
Estimated Expiration
2039-07-08

AI Technical Summary

Technical Problem

Cerium oxide powder is easily pulverized and detached during the reaction, resulting in low efficiency of the carbonate generation reaction, and it is difficult to effectively fix a large number of catalysts with existing technology, which limits the reaction efficiency and the long-term use of the catalyst.

Method used

An inorganic binder containing alumina and/or silica is used to fix the cerium oxide solid catalyst on the substrate to form a multi-layer structure, including the substrate, catalyst layer and intermediate layer, ensuring the firm fixation and efficient activity of the catalyst. maintain.

Benefits of technology

The catalyst is stably fixed, the carbonate generation reaction efficiency is improved, the service life of the catalyst is extended, the catalytic activity is restored through heat treatment, and the frequency of regeneration treatment is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002885307510000291
    Figure BDA0002885307510000291
  • Figure BDA0002885307510000301
    Figure BDA0002885307510000301
  • Figure BDA0002885307510000311
    Figure BDA0002885307510000311
Patent Text Reader

Abstract

The present invention provides a method for producing carbonate and a catalyst structure for producing carbonate, which can suppress the pulverization and detachment of the solid catalyst when a catalyst structure containing a sufficient amount of cerium oxide is supported on a substrate, and has excellent carbonate reaction efficiency. The method for producing carbonate of the present invention includes a step of producing carbonate by reacting a monohydric alcohol with carbon dioxide in the presence of a catalyst structure and a hydrating agent, wherein the catalyst structure includes a substrate and a catalyst layer formed on at least a portion of the surface of the substrate and containing a solid catalyst and an inorganic binder, wherein the solid catalyst contains cerium oxide, and the supported amount of the solid catalyst is 15 g / m 2 Above 200g / m 2 Hereinafter, the inorganic binder contains silica and / or alumina.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing carbonate esters and a catalyst structure for producing carbonate esters. Background Art

[0002] In recent years, the concern about global warming has increased. In the COP (Conference of the Parties), an international framework for agreeing to reduce greenhouse gas emissions, as a common long-term global goal, the purpose is to keep the average temperature rise from before the industrial revolution to a level sufficiently lower than 2°C, and to be able to suppress the emission peak as soon as possible and reduce it sharply based on the latest technology. In the COP21 Paris Agreement, it is stipulated that all countries should be committed to formulating and proposing a long-term low-emission development strategy for greenhouse gases. Japan's long-term goal is to achieve an 80% reduction in greenhouse gas emissions by 2050. Among the greenhouse gases emitted by humans, carbon dioxide is considered to have the greatest impact, and various places are committed to developing countermeasure technologies for reducing carbon dioxide. As one of the countermeasure technologies, several attempts have been proposed to convert emitted carbon dioxide into useful substances. However, in order to convert carbon dioxide into other substances, a large amount of energy is required, and it is hoped that an effective catalyst for promoting the reaction will be developed. In addition, in order to make it a technology that helps reduce carbon dioxide, it is necessary to manufacture useful substances with great demand.

[0003] Among them, carbonates are very useful compounds as additives such as gasoline additives for improving octane numbers and diesel fuel additives for reducing particulates in exhaust gas. They are also used as alkylating agents, carbonylating agents, solvents, etc. in the synthesis of polycarbonate or polyurethane, resins for medicines, pesticides, etc., organic compounds, or as raw materials for lithium battery electrolytes, lubricating oil raw materials, and deoxidizers for rust prevention of boiler piping.

[0004] Carbonate is a general term for compounds obtained by replacing one or two atoms of hydrogen in two atoms of carbonic acid CO(OH)2 with an alkyl or aryl group, and has a structure of RO-C(=O)-OR' (R, R' represents a saturated hydrocarbon group or an unsaturated hydrocarbon group). Therefore, if such a compound can be efficiently produced from carbon dioxide, a compound equivalent to carbonic acid, it can be a useful solution for reducing carbon dioxide.

[0005] When directly synthesizing carbonate from carbonic acid esters of carbonic acid gas and liquid alcohol, it is known that solid catalysts such as cerium oxide (CeO ) powder, zinc oxide (ZrO ) powder and the coexistence of hydrating agents of nitrile react rapidly. It is known that when cerium oxide powder is used as solid catalyst, reaction is carried out faster (for example, with reference to patent documentation 1).

[0006] Regarding fixing the catalyst on a catalyst supporting structure and using it in a solution reaction system, several examples are known for the purpose of increasing the supply rate of the raw material liquid and preventing the catalyst from eluting into the raw material (e.g., Patent Documents 2 to 5). In these examples, the catalyst is fixed on the catalyst supporting structure by plating, spraying, vapor deposition, and coating with a coating liquid.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2012-162523

[0010] Patent Document 2: Japanese Patent Application Laid-Open No. 6-145113

[0011] Patent Document 3: International Publication No. 2016 / 093329

[0012] Patent Document 4: Japanese Patent Application Laid-Open No. 2013-646

[0013] Patent Document 5: Japanese Patent Application Publication No. 2016-59901 Summary of the invention

[0014] Technical problem to be solved by the invention

[0015] However, the inventors of the present invention have found that the cerium oxide powder is easily pulverized during the reaction. Therefore, when the cerium oxide powder is directly used for the reaction, the powders are pulverized due to contact with each other or with the reactor wall, and thus it is difficult to separate it from the product such as carbonate. In addition, when the cerium oxide powder is directly filled into the reactor, the fluid of the reaction matrix causes a bias flow in the reaction vessel, and as a result, it is difficult to obtain a high reaction efficiency in the reaction at a fast liquid flow rate pursued in the industrial process.

[0016] Therefore, in order to suppress the pulverization of cerium oxide powder during the reaction, the inventors of the present invention have studied a method of fixing a catalyst containing cerium oxide on a substrate (catalyst supporting structure) such as a honeycomb and using it as a catalyst structure in a reaction system. However, in the methods disclosed in Patent Documents 2 to 5, the catalyst can only be fixed on the substrate to a thickness of 5 to 10 μm at most.

[0017] Furthermore, it was found that when cerium oxide powder is supported on a substrate by the methods disclosed in Patent Documents 2 to 5, the amount of catalyst fixed per unit area on the substrate surface becomes the rate-limiting factor of the reaction, making it difficult to improve the reaction efficiency. Furthermore, when a large amount of catalyst is supported on a substrate, there is a problem of the catalyst peeling off and detaching from the substrate.

[0018] Therefore, the present invention is to complete in view of the problems referred to above, the object of the present invention is to, a kind of manufacture method of carbonate is provided, this method can suppress pulverization and the breakaway of solid catalyst when using the solid catalyst that contains sufficient amount of cerium oxide on the catalyst structure on the substrate, and, even through a long time, the efficiency of the formation reaction of carbonate is also excellent.In addition, as object of the present invention, can also enumerate and provide a kind of carbonate manufacturing catalyst structure, it when long-term continuous reaction, even catalytic activity reduces, also can implement the regeneration process that makes function recovery by thermal treatment etc., easily continue long-term continuous use.

[0019] Technical solutions for solving technical problems

[0020] In the process of conducting in-depth research to solve the above-mentioned technical problems, the inventors of the present invention studied the method of fixing the solid catalyst on the substrate, and found that when the solid catalyst is fixed on the substrate together with an inorganic binder containing aluminum oxide and / or silicon dioxide, a relatively large amount of solid catalyst can be fixed on the substrate more firmly. In addition, it is also found that when the solid catalyst is fixed using such an inorganic binder, the activity of the solid catalyst can be fully maintained. Summarizing the above-mentioned insights obtained through research and the results of further research, the inventors of the present invention have completed the present invention.

[0021] The gist of the present invention is as follows.

[0022] (1) A method for producing a carbonate ester, comprising the step of reacting a monohydric alcohol with carbon dioxide in the presence of a catalyst structure and a hydrating agent to produce a carbonate ester,

[0023] The catalyst structure includes a substrate and a catalyst layer formed on at least a portion of the surface of the substrate and containing a solid catalyst and an inorganic binder.

[0024] The solid catalyst contains cerium oxide.

[0025] The solid catalyst loading is 15 g / m 2 Above 200g / m 2 the following,

[0026] The inorganic binder contains silica and / or alumina.

[0027] (2) The method for producing a carbonate ester according to (1), wherein the inorganic binder contains silicon dioxide.

[0028] (3) The method for producing a carbonate ester according to (1) or (2), further comprising an intermediate layer formed between the catalyst layer and the substrate and composed of the inorganic binder.

[0029] (4) The method for producing a carbonate ester according to any one of (1) to (3), wherein the solid catalyst is supported in an amount of 15 g / m 2 Above 150g / m 2 the following.

[0030] (5) The method for producing a carbonate ester according to any one of (1) to (3), wherein the solid catalyst is supported in an amount of 15 g / m 2 Above 70g / m 2 the following.

[0031] (6) The method for producing a carbonate ester according to any one of (1) to (5), wherein the substrate has a continuous hole that serves as a flow path for the monohydric alcohol and the carbon dioxide.

[0032] The catalyst layer is formed on the surface of the communicating hole.

[0033] (7) The method for producing a carbonate ester according to any one of (1) to (6), wherein the solid catalyst further contains an oxide of a rare earth element.

[0034] (8) The method for producing a carbonate ester according to (7), wherein the solid catalyst contains lanthanum oxide.

[0035] (9) The method for producing a carbonate ester according to any one of (1) to (8), wherein the catalyst layer has an average thickness of 12 μm to 150 μm.

[0036] (10) The method for producing a carbonate ester according to any one of (1) to (9), wherein the substrate is a metal honeycomb.

[0037] (11) The method for producing a carbonate ester according to any one of (1) to (10), wherein the hydrating agent contains a nitrile compound.

[0038] (12) The method for producing a carbonate ester according to any one of (1) to (11), wherein the hydrating agent contains 2-cyanopyridine.

[0039] (13) A catalyst structure for producing carbonate esters, comprising:

[0040] substrate; and

[0041] a catalyst layer formed on at least a portion of the surface of the substrate and containing a solid catalyst and an inorganic binder,

[0042] The solid catalyst contains cerium oxide.

[0043] The solid catalyst loading is 15 g / m2 Above 200g / m 2 the following,

[0044] The inorganic binder contains silica and / or alumina.

[0045] (14) The catalyst structure for carbonate production as described in (13), wherein the solid catalyst loading is 15 g / m 2 Above 150g / m 2 the following.

[0046] (15) A carbonate production device comprising:

[0047] The catalyst structure for producing carbonate esters according to (13) or (14) above; and

[0048] A supply passage for supplying at least a monohydric alcohol and carbon dioxide to the catalyst structure.

[0049] (16) The carbonate production apparatus according to (16), further comprising a discharge passage through which carbonate produced from the monohydric alcohol and carbon dioxide passes.

[0050] (17) The carbonate production apparatus according to (15) or (16) above, wherein a plurality of the catalyst structures are arranged in series.

[0051] (18) The carbonate production apparatus according to (15) or (16) above, comprising an integrated structure in which a plurality of the catalyst structures are arranged in parallel.

[0052] (19) A method for producing carbonate esters, comprising: in the carbonate ester production apparatus described in any one of (15) to (18), a step of circulating a reaction substrate containing the monohydric alcohol and carbon dioxide at a space velocity (per minute) of not less than 0.005 and not more than 5000.

[0053] Effects of the Invention

[0054] According to the present invention, a method for producing carbonate and a catalyst structure for producing carbonate can be provided, in which the pulverization and detachment of the solid catalyst can be suppressed when a catalyst structure containing a sufficient amount of cerium oxide is supported on a substrate, and the efficiency of the formation reaction of the carbonate is excellent. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 This is a partially enlarged cross-sectional view of a catalyst structure for producing carbonate esters according to one embodiment of the present invention.

[0056] Figure 2It is a partially enlarged cross-sectional view of a catalyst structure for producing carbonate esters according to another embodiment of the present invention.

[0057] Figure 3 This is a graph showing the results (changes in the catalytic activity retention rate) of carbonate production reactions using the carbonate production catalyst structure according to one embodiment of the present invention and a comparative catalyst structure.

[0058] Figure 4 It is a side view showing a specific example of the carbonate production apparatus including the catalyst structure.

[0059] Figure 5 The figures are a top view (A) and a bottom view (B) showing a specific example of an apparatus for producing carbonate esters including a catalyst structure.

[0060] Figure 6 This is a schematic diagram showing an example of the shape of an apparatus for producing carbonate esters including a catalyst structure suitable for use on a factory scale.

[0061] Figure 7 This is a specific example of a honeycomb substrate (metal honeycomb) used in a carbonate production device, and shows an example of a cylindrical outer shape ( Figure 7 (A)) and a diagram of an example of a rectangular shape ( Figure 7 (B)).

[0062] Figure 8 This is a diagram schematically showing a specific example of a carbonate production facility including various devices such as a carbonate production device. DETAILED DESCRIPTION

[0063] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In addition, in this specification and the accompanying drawings, for components having substantially the same functional configuration, repeated descriptions are omitted by using the same symbols. Furthermore, each component in the drawings is appropriately emphasized for ease of description, and the ratios and sizes of each component in the drawings do not represent the actual ratios and sizes of each component.

[0064] <1. Catalyst structure for carbonate production>

[0065] First, a preferred embodiment of the catalyst structure for producing carbonate esters of the present invention will be described. Figure 1 This is a partially enlarged cross-sectional view of the carbonate producing catalyst structure of the present embodiment. The carbonate producing catalyst structure 1 of the present embodiment (hereinafter also simply referred to as "catalyst structure") catalyzes the production of carbonate from carbon dioxide and monohydric alcohol in the presence of a hydrating agent.

[0066] The carbonate production catalyst structure 1 of the present embodiment includes a substrate 10 and a catalyst layer 20 formed on at least a portion of the surface of the substrate 10 and containing a solid catalyst 40 and an inorganic binder 50. The solid catalyst 40 contains cerium oxide. In the catalyst layer 20, the solid catalyst 40 is supported in an amount of 15 g / m 2 Above 200g / m 2 Hereinafter, the inorganic binder 50 contains silica and / or alumina. In addition, in the present embodiment, the catalyst structure 1 for carbonate production has an intermediate layer 30 composed of the inorganic binder 50 between the catalyst layer 20 and the substrate 10 .

[0067] (1.1. Base material)

[0068] The substrate 10 is a catalyst supporting structure for supporting the solid catalyst 40. By supporting the solid catalyst 40 on the surface of the substrate 10 in this way, compared with the case of directly using a powdered catalyst, the local presence of the solid catalyst 40 in the reaction container during the reaction is suppressed, and the local temperature unevenness in the reaction container caused by the generated reaction heat can be reduced. Therefore, according to this embodiment, the product can be synthesized with high efficiency.

[0069] Furthermore, even if the activity of the solid catalyst 40 decreases when the reaction is continued for a long time, it can be regenerated by heat treatment or the like after being taken out of the reaction vessel to restore the function, making it easy to continue to use it for a long time. In addition, as described in detail later, by adjusting the composition of the solid catalyst 40, the catalyst function can be well maintained for a long time, and the frequency of the regeneration treatment can be reduced.

[0070] As substrate 10, as long as catalyst layer 20 containing solid catalyst 40 can be formed, there is no particular limitation, and substrates of arbitrary shape and size can be used. In particular, substrate 10 preferably has a connected hole that becomes the flow path of monohydric alcohol and carbon dioxide. By substrate 10 having such a connected hole, the diffusion efficiency of monohydric alcohol and carbon dioxide as raw materials is improved, and the recovery of the product of water of carbonate and by-product etc. becomes easy. In addition, by forming catalyst layer 20 on the surface of connected hole, catalyst layer 20 becomes large with the contact area of ​​monohydric alcohol and carbon dioxide as raw materials, and the efficiency of the formation reaction of carbonate is improved.

[0071] As the substrate 10, for example, it can have a porous shape such as foam, a corrugate shape, a honeycomb shape, a mesh shape, a cylindrical shape, a cylindrical shape, etc. The substrate 10 is particularly preferably porous, foamy, honeycomb or mesh. Since these are shapes with connected holes, the above-mentioned effect of having connected holes can be well obtained. In particular, when the substrate 10 is a honeycomb shape, the physical strength of the substrate 10 can be excellent, the shape stability of the substrate 10 can be excellent, and the specific surface area of ​​the connected holes can be large.

[0072] The cross-sectional shape of the communicating cells of the honeycomb is not particularly limited, and may be a polygon such as a triangle, a quadrilateral, or a hexagon, or various wave shapes (fin shapes) such as a sine wave.

[0073] The pore diameter of the connecting pores of the substrate 10 is not particularly limited, and is, for example, 0.3 to 6 mm, preferably 0.5 to 5 mm. In addition, the number of connecting pores (cell number) in the substrate 10 is not particularly limited, and is, for example, 25 to 1200 cells / inch. 2 (3.9~186 cells / cm 2 ), preferably 100 to 600 cells / inch 2 (15.5~93 cells / cm 2 ).

[0074] The material constituting the substrate 10 is not particularly limited, and may be a metal material such as stainless steel or aluminum steel, or various ceramic materials such as cordierite, mullite, silicon carbide, alumina, silicon dioxide, titania, zirconia, and cerium oxide.

[0075] As the substrate 10, a honeycomb substrate composed of a metal material or ceramic, that is, a ceramic honeycomb or a metal honeycomb (metal honeycomb), is preferred, and a metal honeycomb is particularly preferred. By using a metal material such as stainless steel (martensitic, ferritic, austenitic, austenite-ferrite dual-phase, and precipitation-strengthened steel) as the material of the substrate 10, the thermal conductivity of the substrate 10 can be improved. Therefore, the heat generated during the reaction can be easily removed to the outside of the reaction container along with the movement of the raw materials, and the temperature in the catalyst tank can be maintained uniformly and stably, so that the high catalytic activity of the catalyst layer 20 can be stably exerted for a long time. On the other hand, when the substrate 10 is formed of ceramic, the adhesion of the catalyst layer 20 to the substrate 10 can be further improved. In addition, in Figure 6 A specific example of a metal honeycomb in a state where no catalyst layer is included is shown.

[0076] (1.2. Catalyst layer)

[0077] The catalyst layer 20 is formed on at least a portion of the surface of the substrate 10 via an intermediate layer 30 described later. However, as described in detail later, the catalyst layer 20 may be directly laminated on the surface of the substrate 10.

[0078] Typically, the catalyst layer 20 is formed on the inner wall surface of the through-hole of the substrate 10. The catalyst layer 20 includes a solid catalyst 40 containing cerium oxide, and catalyzes a formation reaction of carbonic acid ester from carbon dioxide and monohydric alcohol.

[0079] In the catalyst layer 20, the solid catalyst 40 contains at least cerium oxide. Cerium oxide has excellent catalytic activity in the formation reaction of carbonate from carbon dioxide and monohydric alcohol. On the other hand, cerium oxide is usually easy to pulverize, but in this embodiment, since it is firmly fixed to the substrate 10 by the inorganic binder 50 described later, it can be suppressed from detaching and prevented from pulverizing.

[0080] In addition, the solid catalyst 40 may contain one or more catalysts other than cerium oxide. As such a catalyst, as long as it can catalyze the reaction of carbon dioxide and a monohydric alcohol, for example, tin compounds, thallium compounds, nickel compounds, vanadium compounds, copper compounds, alkali metal carbonates, zirconium oxide, titanium oxide, rare earth elements other than cerium (especially oxides thereof), etc. can be listed. Among these, zirconium oxide is preferred due to its high catalytic activity. In this case, the proportion of cerium oxide in the solid catalyst 40 is, for example, more than 5 atomic weight %, preferably more than 20 atomic weight %. In addition, the proportion of cerium oxide in the solid catalyst 40 can be 100 atomic weight %.

[0081] When the catalyst of cerium oxide is continuously used in the direct synthesis reaction of carbonate, the catalytic activity decreases over time, and sometimes it is necessary to regenerate the catalyst with a relatively high frequency, yet, by adjusting the catalyst component, it is possible to maintain high catalytic activity. For example, when rare earth elements other than cerium are added as a co-catalyst component, the catalytic activity of the solid catalyst 40 can maintain a high trend in the formation reaction of carbonate for a long time.

[0082] As rare earth elements other than cerium, scandium, yttrium, lanthanum, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium can be listed. Among these rare earth elements, lanthanum, praseodymium, and gadolinium are preferably added to the solid catalyst 40, and lanthanum is particularly preferably used. In addition, these metal elements are mainly contained in the solid catalyst 40 in the form of oxides, or exist in the surface layer of the solid catalyst 40.

[0083] The proportion of the promoter component, such as the oxide of a rare earth element, in the solid catalyst 40 is preferably 0.01 to 10 mass %, more preferably 0.05 to 5.0 mass %, further preferably 0.1 to 2.5 mass %, particularly preferably 0.2 to 2.0 mass %, for example 1 mass %, based on the weight of the entire solid catalyst.

[0084] In addition, the solid catalyst 40 is supported in the catalyst layer 20 at a weight of 15 g / m 2 Above 200g / m 2 As a result, the reaction efficiency of the catalytic reaction using the catalyst structure 1 can be improved. In contrast, the supported amount of the solid catalyst 40 is less than 15 g / m 2 When the amount of the solid catalyst 40 supported exceeds 200 g / m 2 When the raw material matrix is ​​too large to diffuse into the deep part of the catalyst layer 20, the reaction efficiency may be reduced. The inventors of the present invention have found that the amount of solid catalyst 40 supported and the reaction efficiency are not simply positively correlated, but there is a range of the amount of solid catalyst 40 supported that is suitable for achieving high reaction efficiency. By allowing the catalyst structure 1 to support such a relatively large amount of solid catalyst 40, high reactivity can be maintained even at a high raw material supply rate, and the reactor can be made relatively small, which can suppress equipment costs.

[0085] From the viewpoint of improving the reaction efficiency of the catalytic reaction using the catalyst structure 1, the supported amount of the solid catalyst 40 in the catalyst layer 20 is, for example, 10 g / m 2 Above 200g / m 2 Below, preferably 15g / m 2 Above 150g / m 2 Below, more preferably 15g / m 2 Above 70g / m 2 Below, more preferably 15g / m 2 Above 30g / m 2 the following.

[0086] Similarly, from the viewpoint of improving the reaction efficiency of the catalytic reaction using the catalyst structure 1, the amount of cerium oxide supported in the catalyst layer 20 is, for example, 10 g / m 2 Above 200g / m 2 Below, preferably 15g / m 2 Above 150g / m 2 Below, more preferably 15g / m 2 Above 70g / m 2 Below, more preferably 15g / m 2Above 30g / m 2 the following.

[0087] In addition, when the solid catalyst 40 is loaded in the above-mentioned range, the thickness of the catalyst layer 20 is approximately 12 μm to 150 μm on average, which is significantly improved compared to the thickness of the catalyst layer formed by the method used in Patent Documents 2 to 5 (maximum 5 μm). At present, it is difficult to load such a large amount of solid catalyst 40 without hindering its reaction activity, but in this embodiment, this problem is solved by the inorganic binder 50 described later. The average thickness of the catalyst layer 20 can be about 12 μm to 180 μm, preferably about 15 μm to 150 μm.

[0088] Furthermore, the thickness of the catalyst layer 20 formed in the through hole of the substrate 10 is not necessarily uniform due to the shape of the through hole. However, by forming a uniform catalyst layer on a plate-like substrate using a scraper method or the like, a correlation between the amount of solid catalyst in the catalyst layer and the thickness is obtained, and thus, even when a through hole is formed, the average thickness of the catalyst layer 20 of the substrate 10 can be obtained as an apparent thickness based on the weight of the supported solid catalyst 40. Furthermore, in this specification, the (average) thickness of the catalyst layer 20 is obtained by the above method.

[0089] In addition, the average particle size of the solid catalyst 40 used in the manufacture is not particularly limited, and is, for example, 0.001 μm to 100 μm, preferably 0.005 μm to 100 μm, more preferably 0.01 μm to 80 μm, further preferably 0.1 μm to 60 μm, particularly preferably 1.0 μm to 30 μm, and further preferably 3.0 μm to 15 μm. Thus, the specific surface area of ​​the solid catalyst 40 can be made relatively large, thereby improving the efficiency of the catalytic reaction, and preventing the solid catalyst 40 from detaching from the inorganic binder 50.

[0090] Here, in this specification, "average particle size" refers to the volume-based 50% particle size (D50) obtained by a wet laser diffraction scattering method. In addition, when it is difficult to measure using the laser diffraction scattering method due to poor dispersibility, calculations based on scanning electron microscopy, X-ray diffraction measurement, image imaging methods, etc. can be applied.

[0091] In addition, the catalyst layer 20 includes the above-mentioned solid catalyst 40 and an inorganic binder 50 for fixing the solid catalyst 40. In addition, the inorganic binder 50 contains silica and / or alumina. As a result of in-depth research conducted by the inventors of the present invention, it was found that when silica and / or alumina are used as the inorganic binder 50, a relatively large amount of solid catalyst 40 can be carried without hindering the catalytic activity of the solid catalyst 40. Moreover, by such an inorganic binder 50, the solid catalyst 40 containing cerium oxide can be firmly fixed to the substrate 10, and the detachment and peeling of the solid catalyst 40 during the reaction can be suppressed. As a result, the catalyst structure 1 can be used for a long time while maintaining high activity. In addition, when an inorganic binder is used, even if the reaction temperature or the regeneration treatment temperature becomes a relatively high temperature, the catalyst layer 20 will not deteriorate, and the high adhesion between the catalyst layer 20 and the substrate 10 can be maintained.

[0092] There are no particular limitations on the silica and alumina that may be contained in the inorganic binder 50, and any silica and alumina formed using any compound as a precursor may be used. In addition, these silica and alumina may be amorphous or crystalline.

[0093] In addition, the inorganic binder 50 may also contain components other than silicon dioxide and aluminum oxide. Such components include magnesium, calcium, etc., or impurities that may be mixed in the production of the inorganic binder 50. In addition, in the inorganic binder 50, the total amount of silicon dioxide and aluminum oxide is preferably 20% by mass or more, and more preferably 50% by mass or more. The inorganic binder 50 is further preferably essentially composed of silicon dioxide and / or aluminum oxide, and particularly preferably composed of silicon dioxide and / or aluminum oxide.

[0094] In addition, in the inorganic binder 50, silicon dioxide and aluminum oxide are usually present in the form of a collection (agglomerate) of tiny particles, so the inorganic binder 50 is porous. By making the inorganic binder 50 porous, carbon dioxide and monohydric alcohol as raw materials can reach the surface of the solid catalyst 40 that is not exposed on the surface in the catalyst layer 20.

[0095] The specific surface area of ​​the solid particles in the inorganic binder 50 is not particularly limited, and may be, for example, 1 m 2 / g above 1000m 2 / g or less, preferably 10m 2 / g above 500m 2By making the specific surface area of ​​the inorganic binder 50 within the above range, the diffusion rate of carbon dioxide and monohydric alcohol in the inorganic binder 50 can reach a sufficient rate, the reaction on the surface of the solid catalyst 40 can be promoted, and the solid catalyst 40 can be further firmly fixed to the catalyst layer 20. The specific surface area can be measured by the BET method.

[0096] In addition, the supported amount of the solid content in the inorganic binder 50 of the catalyst layer 20 is, for example, 1 g / m 2 Above 100g / m 2 Less than 1 g / m 2 Above 40g / m 2 As a result, the exposed area of ​​the solid catalyst 40 can be increased to improve the reaction efficiency, and the solid catalyst 40 can be firmly fixed to the substrate 10 .

[0097] In addition, in the catalyst layer 20, the solid content in the inorganic binder 50 is contained in a ratio of, for example, 0.01 g to 5 g, preferably 0.10 g to 1.0 g, relative to 1 g of the solid catalyst. This can increase the exposed area of ​​the solid catalyst 40 to improve the reaction efficiency, and can firmly fix the solid catalyst 40 to the substrate 10.

[0098] Here, the solid content in the inorganic adhesive 50 refers to the inorganic oxide particles and adhesive solidified material intentionally introduced into the adhesive. The mass ratio of the solid content in the inorganic adhesive is obtained by dividing the mass of the residue after only drying and curing the inorganic adhesive by the mass of the inorganic adhesive before drying and curing. Therefore, the mass of the solid content in the inorganic adhesive can be calculated by (mass ratio of the solid content)×(mass of the inorganic adhesive coating).

[0099] (1.3. Middle layer)

[0100] The intermediate layer 30 is a layer composed of an inorganic binder 50, and is disposed between the substrate 10 and the catalyst layer 20. In this way, by forming the intermediate layer 30 composed of the inorganic binder 50 between the catalyst layer 20 containing the solid catalyst 40 and the substrate 10, the adhesion between the catalyst layer 20 and the substrate 10 is further improved, and the solid catalyst 40 is prevented from detaching from the catalyst structure 1. In addition, by having such an intermediate layer 30, even when using a substrate 10 of a material having low adhesion to the catalyst layer 20, the adhesion between the catalyst layer 20 and the substrate 10 can be made sufficient.

[0101] The inorganic binder 50 may have the same structure as the catalyst layer 20 , and thus its description is omitted. The inorganic binder 50 of the catalyst layer 20 and the inorganic binder of the intermediate layer 30 may have different structures or may have the same structure.

[0102] In the intermediate layer 30, the solid content of the inorganic binder 50 is, for example, 1 g / m 2 Above 100g / m 2 Less than 10 g / m 2 Above 50g / m 2 Within the above range, cohesive failure of the intermediate layer 30 can be prevented, and the adhesion between the catalyst layer 20 and the substrate 10 can be further improved.

[0103] In the carbonate manufacturing catalyst structure 1 of the present embodiment described above, utilize the inorganic binder 50 that contains silicon dioxide and / or aluminum oxide, a large amount of solid catalysts 40 are firmly fixed to catalyst layer 20.And, inorganic binder 50 can not hinder the catalytic reaction that utilizes solid catalyst 40 to carry out.As a result, when using carbonate manufacturing catalyst structure 1 to manufacture carbonate, the efficiency of the formation reaction of carbonate is excellent.And, because solid catalyst 40 is firmly fixed to substrate 10 by inorganic binder 50, so can prevent from carbonate manufacturing catalyst structure 1 to break away from, the result can also prevent pulverization.

[0104] Even such carbonate manufacturing can obtain high reaction efficiency with catalyst structure 1 in the reaction under the fast liquid flow rate required in industrial process.And the disengagement, pulverization of solid catalyst 40 are prevented, therefore, even under the harsh environment required in industrial process, also can reuse, excellent durability.

[0105] The catalyst structure 1 for producing carbonate esters according to the present embodiment has been described above. In addition, the present invention is not limited to the above-described embodiment. Figure 2 It is a partially enlarged cross-sectional view of a catalyst structure for producing carbonate esters according to another embodiment of the present invention. Figure 2 The carbonate manufacturing catalyst structure 1A shown has a catalyst layer 20 on a substrate 10. And, unlike the above-mentioned carbonate manufacturing catalyst structure 1, the intermediate layer composed of the inorganic binder 50 is omitted. Thus, even when the intermediate layer is omitted, the solid catalyst 40 in the catalyst layer 20 is sufficiently fixed by the inorganic binder 50 containing silica and / or alumina, preventing the separation from the carbonate manufacturing catalyst structure 1A and the subsequent pulverization.

[0106] The boundary between the catalyst layer 20 and the intermediate layer 30 can be observed by an optical microscope, a scanning electron microscope, elemental analysis using EDS (energy dispersive X-ray spectrometer), or the like.

[0107] In addition, the amount of solid catalyst 40 carried in the catalyst layer 20 can be calculated based on the catalyst layer area and the overall carrying mass of the catalyst layer 20 by identifying the proportion of metal components (e.g., cerium) in the catalyst layer 20 by elemental analysis. Specifically, when the component of the solid catalyst 40 is cerium oxide, it can be calculated by the following formula.

[0108] (Solid catalyst supported amount) = [(mass of catalyst layer) × (mass ratio of cerium in catalyst layer) × ((mass of cerium oxide) / (mass of cerium))] / (area of ​​catalyst layer)

[0109] This value has the same meaning as the mass of the solid catalyst 40 per unit area of ​​the substrate 10 where the solid catalyst 40 is present, and can be obtained regardless of the presence or absence of the intermediate layer 30 .

[0110] As an elemental analysis method for identifying metal components, a scanning high-frequency inductively coupled plasma method (ICP) can be used. Regarding the amount of inorganic binder 50 carried in the catalyst layer 20 and the intermediate layer 30, the solid component ratio in the inorganic binder used to form the catalyst layer 20 and the intermediate layer 30 can be calculated from the metal component ratio obtained by the above-mentioned elemental analysis. Among them, the catalyst layer area refers to the area of ​​the portion coated (formed) with the solid catalyst 40 (catalyst layer 20). For example, when the substrate 10 is a honeycomb shape and the outer periphery is not coated with the catalyst layer 20, it is set to form the internal connecting pores and the surface area of ​​the entire substrate 10 coated with the catalyst layer 20. Among them, when the intermediate layer 30 is present, the amount of solid catalyst 40 carried is also calculated by the same method.

[0111] <2. Method for producing catalyst structure for producing carbonate ester>

[0112] Next, the method for producing the catalyst structure for producing carbonate esters according to the present embodiment will be described mainly with respect to the method for producing the catalyst structure 1 for producing carbonate esters.

[0113] First, a binder stock solution is prepared for forming the intermediate layer 30. The binder stock solution can be obtained by dissolving or dispersing a material of the inorganic binder 50, such as alumina, silica, or a precursor thereof, in an appropriate liquid medium, such as water or alcohol. In addition, the concentration of the material of the inorganic binder 50 in the binder stock solution is not particularly limited and can be appropriately set according to the method of applying the binder stock solution to the substrate 10.

[0114] Next, a substrate 10 is prepared, and an intermediate layer 30 is formed on the substrate 10. Specifically, it can be performed by applying an adhesive stock solution to the substrate 10, and drying and solidifying it. The application of the adhesive stock solution can be performed by any method, for example, it can be performed by coating using a rod coater, a scraper, a roll coater, a notch wheel coater, a die coater, a gravure coater, a spin coater, a slit coater, etc., inkjet, spray, immersion, etc. In particular, when the substrate 10 has a through hole, it is preferred to immerse the substrate 10 in the adhesive stock solution. In addition, in order to increase the film thickness of the intermediate layer 30, the application of the adhesive solution can also be repeated multiple times.

[0115] Next, the adhesive stock solution applied to the substrate 10 is dried and cured to form the intermediate layer 30. The drying temperature can be any temperature that can remove the liquid medium, and can be appropriately set according to the boiling point of the medium. When the medium is water, for example, it can be 60°C to 100°C. In addition, the drying time can be appropriately set according to the drying state. The curing temperature can be appropriately set according to the curing temperature of the curing component in the adhesive. When it is a siloxane system, for example, it can be 120°C to 200°C. In addition, the curing time is not particularly limited and can be appropriately set.

[0116] Next, a catalyst layer forming mixed solution is prepared for forming the catalyst layer 20. The catalyst layer forming mixed solution can be obtained by dissolving or dispersing the solid catalyst 40 and the material of the inorganic binder 50, such as alumina, silica, or their precursors, in an appropriate liquid medium, such as water or alcohol.

[0117] Next, a catalyst layer 20 is formed on the intermediate layer 30 stacked on the substrate 10 or on the substrate 10. Specifically, a catalyst layer forming mixed solution is imparted on the surface of the intermediate layer 30 or on the surface of the substrate 10, and it is dried and solidified. The imparting of the catalyst layer forming mixed solution can be carried out by any method, for example, it can be carried out by coating, inkjet, spraying, dipping, etc. using a rod coater, a scraper, a roller coating, a notch wheel coater, a die coating, a gravure coating, a spin coating, a slit coating, etc. In particular, when the substrate 10 has a through hole, it is preferred to immerse the substrate 10 in the catalyst layer forming mixed solution. In addition, in order to increase the film thickness of the catalyst layer 20, the imparting of the catalyst layer forming mixed solution can also be repeated multiple times.

[0118] Next, the catalyst layer forming mixed liquid applied to the substrate 10 is dried and cured to form the catalyst layer 20. Thus, the catalyst structure 1 of the present embodiment is obtained. The drying temperature can be any temperature at which the liquid medium can be removed, and can be appropriately set according to the boiling point of the medium. When the medium is water, for example, it can be 60°C to 100°C. In addition, the drying time can be appropriately set according to the drying state. The curing temperature can be appropriately set according to the curing temperature of the curing-expressing component in the adhesive. When it is a siloxane system, for example, it can be 120°C to 200°C. In addition, the curing time is not particularly limited and can be appropriately set.

[0119] In addition, before coating (forming) the intermediate layer 30 on the substrate 10, or directly coating (forming) the catalyst layer 20, the adhesion between the surface of the substrate 10 and the interface between the intermediate layer 30 or the catalyst layer 20 is sometimes insufficient. Therefore, it is preferred to perform the following pretreatment process. Specifically, first, in order to remove the oil on the surface of the substrate 10, it is cleaned and dried with a volatile organic solvent such as alcohol, acetone, etc. Thereafter, the substrate 10 is immersed in an alkaline aqueous solution for washing and drying. Thereafter, the metal substrate is immersed in an acidic aqueous solution for washing and drying. Alternatively, the substrate 10 is treated with a liquid medicine, a heat treatment, or a plasma treatment, a UV treatment, or a corona discharge treatment.

[0120] <3. Method for producing carbonate ester>

[0121] Next, a method for producing carbonate using the carbonate producing catalyst structure is described based on a preferred embodiment. The method for producing carbonate of this embodiment includes a step of producing carbonate by reacting a monohydric alcohol with carbon dioxide in the presence of the catalyst structure 1 and a hydrating agent.

[0122] First, before describing the method for producing a carbonate ester according to the present embodiment, the mechanism of the reaction occurring in the present method will be described. First, the catalyst structure 1 catalyzes the reaction of a monohydric alcohol represented by the following formula (1) and carbon dioxide.

[0123]

[0124] Among them, the catalytic mechanism of the solid catalyst 40 serving as the catalyst structure 1 can be considered to be the following mechanism: at the alkaline point, alcohol in the form of R-O-M (M is the solid catalyst 40) undergoes dissociative adsorption to form RO-C(=O)-O...M with CO2; on the other hand, alcohol in the form of HO-R...M undergoes adsorption at the acidic point to generate RO-C(=O)-OR between the two adsorbed species.

[0125] On the other hand, the reaction shown in the above-mentioned formula (1) is a reversible reaction. Therefore, when there is by-product water, it reacts again with the generated carbonate to return monohydric alcohol and carbonic acid gas. Therefore, in order to remove the by-product water, a hydrating agent is used to carry out the hydration reaction shown in the following formula (2).

[0126]

[0127] By the result of the reaction shown in the above formula (2) removing water, the reverse reaction in the formula (1) is suppressed, and promotes the formation reaction of carbonate. In addition, although the reason is still unclear, it can be believed that the solid catalyst 40 also has catalytic activity for the hydration reaction of the above-mentioned formula (2). Above, the mechanism of the reaction occurring in this method has been described.

[0128] As described above, the method for producing carbonate esters according to the present embodiment includes the step of producing carbonate esters by reacting a monohydric alcohol with carbon dioxide in the presence of the catalyst structure 1 described above and a hydrating agent.

[0129] Specifically, the catalyst structure 1 is placed in a reaction container, and a hydrating agent, a monohydric alcohol, and carbon dioxide are introduced into the reaction container, thereby causing a carbonate reaction to proceed.

[0130] As the monohydric alcohol, one or more compounds selected from primary alcohols, secondary alcohols and tertiary alcohols can be used.

[0131] Specific examples of the monohydric alcohol include methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, n-pentanol, n-hexanol, 2-hexanol, 3-hexanol, heptanol, hexanol, and phenol.

[0132] The type of the monohydric alcohol can be appropriately selected depending on the chemical structure of the target carbonate and the method of use of the carbonate to be obtained.

[0133] As a hydrating agent, as long as it can react with water to remove water, there is no particular limitation. As shown in the above formula (2), compounds containing cyano groups can be listed, and one or more of them can be used alone or in combination. Specifically, for example, acetonitrile, cyanoethane, 1-cyano-propane, 2-cyano-propane, cyanoethylene, phenylacetonitrile, benzonitrile, 2-cyanopyridine, 2-cyanopyrazine, 2-cyanopyrimidine, thiophene-2-carbonitrile, 2-furancarbonitrile (2-cyanofuran) and the like can be listed. In particular, from the viewpoint of water removal efficiency, that is, hydration reaction speed, 2-cyanopyridine is preferred.

[0134] The amount of the hydrating agent used can be set according to the amount of the monohydric alcohol used. For example, the amount of the hydrating agent is 0.01 mol to 2 mol, preferably 0.1 mol to 0.5 mol, based on 1 mol of the monohydric alcohol used.

[0135] As the temperature of the formation reaction of carbonate, it is not particularly limited, preferably set to more than 50 ℃ and less than 300 ℃.When the reaction temperature is lower than 50 ℃, according to the kind of its reaction substrate, the reaction speed is low sometimes, and the carbonate synthesis reaction and the hydration reaction utilizing hydrating agent are almost not carried out, and the productivity of carbonate is low.In addition, when the reaction temperature exceeds 300 ℃, although the reaction speed of each reaction becomes high, according to the kind of its reaction substrate, the monomer modification of carbonate, the amide obtained by hydration reaction is other monomers sometimes, or polymerization occurs easily, so the yield of carbonate reduces.The reaction temperature is further preferably more than 100 ℃ and less than 200 ℃.But it is believed that the reaction temperature is different according to the amount and ratio of the type and amount of solid catalyst 40, raw material (monohydric alcohol, hydrating agent), so it is desired to appropriately set the optimum conditions.

[0136] As reaction pressure, it is not particularly limited, and is preferably set to below 20MPa (absolute pressure) above 0.1MPa. When reaction pressure is lower than 0.1MPa (absolute pressure), pressure reducer is needed, not only equipment is complicated and cost becomes high, but also the power energy for forming decompression is needed, and there is a trend of energy efficiency variation. In addition, when reaction pressure exceeds 20MPa, according to the kind of hydrating agent, the hydration reaction utilizing hydrating agent sometimes becomes difficult to carry out, causes the yield variation of carbonate, not only that, but also the power energy required for boosting is needed, and energy efficiency variation is needed. In addition, from the viewpoint of improving the yield of carbonate, reaction pressure is more preferably below 10MPa (absolute pressure) above 0.1MPa.

[0137] As reaction time, it is not particularly limited, and can be appropriately set according to the kind of reaction substrate (raw material), the kind of hydrate and the generation rate of by-product, for example, more than 5 minutes and less than 24 hours, preferably more than 15 minutes and less than 8 hours, more preferably more than 30 minutes and less than 6 hours. In addition, when using the reaction apparatus of continuous type, considering the flow velocity of raw material, the total of the time of being introduced into the reaction vessel from raw material to being discharged from the reaction vessel can be set as reaction time (retention time). In addition, when making the reaction substrate circulate for the catalyst structure to react, the circulation flow is defined with the space velocity shown in the following formula (3).

[0138] Space velocity (per minute) = circulation flow (m 3 / min)÷volume of catalyst structure (m 3 )(3)

[0139] As the value of space velocity, it is not particularly limited, for example, per minute 0.005 above 5000 below, preferably per minute 0.05 above 500 below, more preferably per minute 0.5 above 50 below. When the space velocity is too small, there is a possibility that CO2 is consumed before passing through the catalyst structure and the reaction efficiency deteriorates, and the side reaction increases. On the other hand, the larger the space velocity, the larger the size of the pump, and the energy efficiency is likely to deteriorate. By circulating the reaction substrate containing raw materials in a carbonate manufacturing device with a space velocity (per minute) of the above-mentioned scope, for example, 0.005 above 5000 below, it is possible to efficiently manufacture carbonate.

[0140] According to the above, carbonate can be efficiently produced. And, in the present embodiment, due to the use of the catalyst structure 1 of the present embodiment, the solid catalyst 40 can be prevented from being separated and pulverized from the catalyst structure 1. Therefore, even under the harsh environment required in the industrial process, the catalyst structure 1 can be reused. In addition, the activity of the solid catalyst 40 can be better maintained for a long time by adjusting the catalyst component.

[0141] <4. Carbonate production equipment>

[0142] Next, the carbonate production device is described based on a preferred embodiment. The carbonate production device includes the above-mentioned carbonate production catalyst structure. Figure 4 and Figure 5 In this way, the carbonate manufacturing device 60 has a housing (housing) 62. The housing 62 is formed of, for example, a SUS pipe, and the carbonate manufacturing catalyst structure 1 is accommodated inside the housing 62. The carbonate manufacturing device 60 preferably has a plurality of carbonate manufacturing catalyst structures 1, and these carbonate manufacturing catalyst structures 1 can be arranged in series, for example.

[0143] The carbonate production device 60 has a supply passage 64 that can supply monohydric alcohol and carbon dioxide, which are raw materials for producing carbonate, to the carbonate production catalyst structure 1. Figure 4 As shown by arrow A, when the above raw materials are supplied to the carbonate manufacturing device 60 via the supply passage 64, a carbonate forming reaction is performed inside the carbonate manufacturing catalyst structure 1. And, the carbonate formed by the carbonate forming reaction is as follows. Figure 4 As shown by arrow B, the reactant passes through the discharge passage 70 together with unreacted raw materials and the like, and is discharged to the outside of the carbonate producing apparatus 60 .

[0144] In order to adjust the temperature of the carbonate production reaction, a heat medium fluid (not shown) is supplied to the carbonate production device 60. The temperature rise and reaction temperature of the carbonate production catalyst structure 1 can be adjusted by the heat medium fluid. Therefore, in the carbonate production device 60, a heat medium supply pipe 66 for supplying the heat medium fluid is provided. Figure 4 As shown by arrow C, the heat medium fluid supplied from the inlet 66A of the heat medium supply pipe 66 to the carbonate manufacturing device 60 is as follows: Figure 4 As shown by the arrow D, the heat medium is discharged to the outside of the carbonate production device 60 through the outlet 66B. Thereafter, the heat medium fluid is adjusted to a predetermined temperature and then supplied to the carbonate production device 60 again through the inlet 66A of the heat medium supply pipe 66.

[0145] Furthermore, the form of the carbonate manufacturing apparatus 60 is not limited to the above-mentioned apparatus. For example, in order to increase the flow rate of the fluid containing the raw material supplied through the above-mentioned supply passage, the carbonate manufacturing apparatus may be designed into a shape suitable for large-scale. In this way, when the size of the carbonate manufacturing apparatus becomes larger, Figure 6 As illustrated, sometimes the catalyst structures 1 for carbonate manufacturing are arranged in parallel and arranged in series in the height direction as a one-piece structure 2. In the carbonate manufacturing device 60A having such a structure, after long-term operation, it is easy to replace only the one-piece structure 2 configured with the catalyst structure 1 that is considered to have deteriorated, which can minimize the operating cost of the device configured with the catalyst. In the structure 2 in which the catalyst structures 1 for carbonate manufacturing are arranged in parallel and are integrated, it is preferably provided with a sealing structure for allowing the fluid to inevitably pass through the catalyst structure 1. In addition, in order to ensure the uniformity of the fluid flow in the carbonate manufacturing device 60A, when the catalyst structures 1 for carbonate manufacturing are arranged in parallel and are arranged in series in the height direction as a one-piece structure 2, it is preferably ensured that space is ensured in each section. In order to minimize the device by closely configuring the catalyst structure 1 in the cross section of the carbonate manufacturing device, it is possible to adopt the following method: Figure 7 (B) The catalyst structure 1B of the rectangular shape shown. In this way, when the catalyst structure 1B of the rectangular shape is used, a plurality of catalyst structures 1B can be densely packed in the cross section of the carbonate manufacturing device, and the loss of the storage space can be minimized. Among them, the shape of the catalyst structure 1B is not particularly limited, and the catalyst structure 1B can also be a shape other than the rectangular shape. In addition, the catalyst structure 1B preferably has a porous, foamy, honeycomb or sieve-shaped structure.

[0146] The integrated structure 2 preferably includes a fixing plate 62A as a part of the housing 62 for supporting a plurality of catalyst structures 1B. A frame 62B corresponding to the outer shape of the catalyst structure 1B is formed on the fixing plate 62A. Figure 6As shown by the arrow, the frame 62B is embedded and can be fixed in a freely attachable and detachable manner. In addition, a rectangular honeycomb structure 1C that does not carry a catalyst can be added to the integral structure 2 instead of the catalyst structure 1B. In this way, the structure 1C that has a rectangular honeycomb structure but does not carry a catalyst can be used to prevent the total amount of catalyst contained in the carbonate manufacturing device 60A from becoming excessive. By containing dozens of catalyst structures 1B, such as Figure 6 By disposing one or two or more catalyst-free structures 1C in the illustrated integrated structure 2 containing about 30 to 40 catalyst structures 1B, the distribution amount of the catalyst can be adjusted to an appropriate level, thereby suppressing the amount of by-products generated.

[0147] In addition, as described above, the carbonate production apparatus 60A has a structure in which the catalyst structures 1 are not only arranged in series but also arranged in parallel, that is, a structure in which a plurality of integrated structures 2 in which a plurality of catalyst structures 1 are arranged in parallel are arranged in series, and can be used when the flow rate of the fluid containing the raw material is, for example, 500m 3 / h or more, preferably 550m 3 When a fluid with a flow rate lower than these values ​​is supplied, for example, the carbonate production apparatus 60 in which only 10 or less catalyst structures 1 are arranged in series can be used.

[0148] <5. Carbonate manufacturing equipment>

[0149] Next, a carbonate production facility including a carbonate production device and the like will be described based on preferred embodiments. Figure 7 As shown, the carbonate production facility 100 includes a carbonate production device 60, a raw material supply system for supplying raw materials to the carbonate production device 60, and a recovery system for recovering the produced carbonate.

[0150] When the internal pressure of the CO2 storage device 72 as a supply system is increased by the CO2 boosting pump 73, the carbon dioxide in the CO2 storage device 72 is supplied to the buffer tank 74. On the other hand, the monohydric alcohol and 2-cyanopyridine as liquid raw materials stored in the raw material tank 76 are supplied from the raw material tank 76 to the buffer tank 74 by the raw material input pump 78. In this way, the carbon dioxide and monohydric alcohol etc. supplied to the buffer tank 74 by the respective systems are mixed in the buffer tank 74. The mixed liquid is supplied to the carbonate manufacturing device 60 via the first filter 80.

[0151] In the carbonate manufacturing device 60, the carbonate manufacturing catalyst structure 1 is used to promote the carbonate formation reaction to generate carbonate corresponding to the type of monohydric alcohol as a raw material. The carbonate generated in this way is supplied to the recovery system via the second filter 82. In the recovery system, the liquid containing carbonate is separated from the liquid containing the monohydric alcohol and 2-cyanopyridine as unreacted raw materials, and the liquid containing carbonate is sent to the pump 86 for liquid extraction by the action of the reaction liquid circulation pump 84, and the liquid containing the monohydric alcohol is returned to the buffer tank 74. In the pump 86 for liquid extraction, the liquid other than the carbonate is removed, thereby manufacturing a high-purity carbonate.

[0152] Example

[0153] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples and Comparative Examples.

[0154] (Example 1)

[0155] 1. Preparation of catalyst structure

[0156] Cerium oxide (HSA-20SP manufactured by Solvay Special Chem Japan, average particle size of about 10 μm, impurity concentration of less than 0.02%) was fired at 873K in an air atmosphere for 3 hours to obtain a powdered solid catalyst. Specifically, 20 g of cerium oxide was placed in a crucible in a muffle furnace (FO310 manufactured by Yamato Scientific co., ltd.), heated to 873K at a heating rate of 10°C / min, and then fired. The solid catalyst, silica binder (SUMICERAM, P-750 manufactured by Asahi Chemical Industries (mainly a mixture of siloxane-based binder and water)) and water obtained in this way were weighed in a weight ratio of 2.05:1:1 to prepare 50 g of a mixed solution for catalyst layer preparation, which was filled in a 50cc beaker.

[0157] In addition, in order to prepare an intermediate layer between the catalyst layer and the catalyst-coated substrate, 50 g of the silica binder stock solution was filled into a 50 cc beaker. Length 20mm, 100 cells / inch 2 A cylindrical metal honeycomb (steel type: YUS205M1, plate thickness: 50μm, fin (corrugated foil) shape: sine wave, made by Nippon Steel & Sumitomo Metal Materials). The metal honeycomb was placed in a beaker containing the above-mentioned silica binder stock solution. After confirming that the entire honeycomb was immersed in the liquid, it was lifted up and the excess liquid was blown away with nitrogen. The honeycomb coating obtained in this way was dried at 80°C and cured at 150°C to obtain about 30g / m2 of silica with the binder component attached. 2The thickness of the intermediate layer at this time is estimated to be about 20 μm.

[0158] After that, the honeycomb was placed in a beaker containing the mixed liquid of the cerium oxide and the binder. After confirming that the entire honeycomb was immersed in the liquid, it was lifted up and the excess liquid was blown away with nitrogen. The honeycomb coated product obtained in this way was dried at 80°C and then cured at 150°C. Thus, the silicon dioxide and cerium oxide of the binder components were coated on the surface of the intermediate layer, and finally a honeycomb with about 15 g / m2 of cerium oxide attached was obtained. 2 The catalyst structure of the embodiment. The catalyst layer thickness at this time was estimated to be about 14 μm. In addition, the silica as the binder component was dried and solidified in the same manner as above, and the specific surface area was measured by the BET method. The result was 59 m 2 / g.

[0159] 2. Manufacture of carbonates

[0160] Five catalyst structures thus obtained (0.3 g per structure in terms of cerium oxide adhesion) were used and fixed at the center of a 1-inch SUS tube serving as a fixed bed reactor (see Figure 4 and Figure 5 ). 323 g of 1-propanol and 93 g of 2-cyanopyridine were weighed and mixed in a molar ratio of 6:1 to obtain a mixed solution. The mixed solution was supplied to the fixed bed reactor at a rate of 150 ml / min by a circulation pump while CO2 was introduced into the piping for purging. After that, the pressure was increased so that the total absolute pressure reached 1.0 MPa. In addition, the temperature was raised to 132°C by a heater, and the time to reach the target temperature was taken as the reaction start time, and the reaction was carried out for 6 hours. After reacting at 132°C for 6 hours, the reactor was cooled, cooled to room temperature, and then reduced to normal pressure. The internal standard substance 1-hexanol was added, and the product was collected and analyzed by GC (gas chromatography).

[0161] Regarding the reaction degree of the synthesis reaction, the yield of dipropyl carbonate (hereinafter also referred to as "DPrC") as a product, the yield of DPrC, and the molar ratio of by-products to DPrC when products other than water and 2-cyanopyridine (hereinafter also referred to as "2-CP") hydrate 2-pyridinecarboxamide (hereinafter also referred to as "2-PA") produced as by-products with DPrC are calculated from the concentrations of each component using the following formula. Among them, the by-products are propyl carbamate, propyl picolinate, propyl pyridine-2-carboximidate, etc.

[0162] When alcohol (mol) / nitrile group (mol) ≥ 2:

[0163] DPrC yield (mol%) = ((DPrC molar amount) / (nitrile group feed molar amount)) × 100

[0164] When alcohol (mol) / nitrile group (mol) < 2:

[0165] DPrC yield (mol%) = (2×(DPrC molar amount) / (1-propanol feed molar amount))×100

[0166] Byproduct / DPrC (mol%) = (the sum of the molar amounts of each component of the byproduct) / (the molar amount of DPrC) × 100

[0167] As a result, under the present conditions, the DPrC yield reached a high yield of 55 mol%, while the byproduct / DPrC was suppressed to 1.0 mol%. Moreover, even after the reaction, the cerium oxide powder did not peel off from the substrate, and had high adhesion. It was also confirmed that after the present structure was sintered and used repeatedly under the above reaction conditions, the reaction results were almost unchanged, and the cerium oxide powder did not peel off from the substrate.

[0168] Specifically, whether the catalyst is re-fired and reused causes a decrease in reaction efficiency and whether the catalyst is peeled off was evaluated according to the following criteria. As a result, these situations were not confirmed in Example 1. In addition, the re-firing of the catalyst was carried out by washing the used catalyst structure with an alcohol of the same type as the alcohol used in the synthesis of dialkyl carbonate, placing it on a heat-resistant dish, mixing nitrogen in the air in a muffle furnace to adjust the oxygen concentration in the air to below the explosion limit of the alcohol, and firing it at 300° C. for 3 hours. The re-firing of the catalyst can also be carried out by using a muffle furnace without taking the catalyst structure out of the reactor and keeping it fixed to the reactor, except for this.

[0169] (Whether the reaction efficiency is reduced)

[0170] When the carbonate yield was lowered by 5 mol% or more compared with the initial use, the reaction efficiency was evaluated as "yes", and when it was lower than 5 mol%, the reaction efficiency was evaluated as "no".

[0171] (Presence or absence of peeling)

[0172] When the weight of the catalyst structure after the reaction was reduced by 0.2 g or more compared with the weight of about 8.80 g before the reaction, the catalyst peeling was evaluated as "yes", and when it was less than 0.2 g, the catalyst peeling was evaluated as "no".

[0173] Furthermore, whether the reaction efficiency is reduced and whether the catalyst is peeled off due to the reaction and firing are also evaluated by the same method in each of the examples and comparative examples described later.

[0174] (Examples 2 to 4)

[0175] The metal honeycomb was repeatedly immersed in the coating solution with cerium oxide powder added, and the cerium oxide was attached to about 30 g / m 2 , 70g / m 2 , 150g / m 2 Except for this, the catalyst structures of Examples 2 to 4 were prepared in the same manner as in Example 1. The catalyst layer thicknesses of the structures thus obtained were estimated to be about 20 μm, about 50 μm, and about 100 μm, respectively.

[0176] The results of reaction evaluation using each catalyst structure showed that the adhesion of Example 2 was 30 g / m 2 In the catalyst structure of Example 3, the DPrC yield reached a high yield of 57 mol%, while the by-product / DPrC was suppressed to 1.2 mol%. 2 In the catalyst structure of Example 4, the DPrC yield reached a high yield of 52 mol%, while the by-product / DPrC was suppressed to 1.4 mol%. 2 In the catalyst structure of Example 1, the DPrC yield reached a high yield of 42 mol%, and the byproduct / DPrC was suppressed to 2.7 mol%. Moreover, in any structure, the cerium oxide powder did not peel off from the substrate even after the reaction, and all had high adhesion. It was also confirmed that when each structure was repeatedly used after being re-fired in the same manner as in Example 1, the reaction results were almost unchanged, and the cerium oxide powder did not peel off from the substrate.

[0177] (Example 5)

[0178] The same cerium oxide powder, silica binder (SUMICERAM, P-700-D manufactured by Asahi Chemical Industries, Ltd. (mainly a mixture of silica powder with an average particle size of about 5 μm, a siloxane-based binder and water)) and water as in Example 1 were weighed in a weight ratio of 2:0.95:1.5 to prepare 50 g of a mixed solution for preparing a catalyst layer, which was filled in a 50 cc beaker. Except for this, all other operations were carried out in the same manner as in Example 2 to prepare a 30 g / m2 adhesive layer of Example 5. 2The catalyst structure. The catalyst layer thickness at this time was estimated to be about 20 μm. As a result of the reaction evaluation using this structure, the DPrC yield reached a high yield of 54 mol%, and the by-product / DPrC was suppressed to 0.9 mol%. In addition, even after the reaction, the cerium oxide powder did not peel off from the substrate and had high adhesion.

[0179] It was also confirmed that when each structure was repeatedly used after being subjected to the same re-firing treatment as in Example 1, the reaction results were almost unchanged and the cerium oxide powder did not peel off from the substrate. Specifically, for the catalyst structure of Example 5, after the above-mentioned reactivity evaluation, it was fired at 573K in an air atmosphere for 3 hours to perform a regeneration treatment, and then the reaction evaluation was performed again. As a result, the DPrC yield was 54 mol%, and the by-product / DPrC was 0.9 mol%, showing the same result as the initial evaluation of Example 5. Moreover, even after the reaction, the cerium oxide powder did not peel off from the substrate, and had high adhesion.

[0180] (Examples 6 and 7)

[0181] As metal honeycomb substrate, diameter Length 20mm, 200 cells / inch 2 and 300 cells / inch 2 The cylindrical metal honeycomb (steel type: YUS205M1, plate thickness: 50μm, fin (corrugated foil) shape: sine wave, made by Nippon Steel & Sumitomo Metal Materials) was made with a cerium oxide adhesion amount of 30g / m 2 , except for this, all operations were carried out in the same manner as in Example 1 to prepare catalyst structures of Examples 6 and 7. The catalyst layer thickness at this time was estimated to be about 11 μm. The results of reaction evaluation using each structure showed that the 200 cells / inch of Example 6 2 In the catalyst structure of Example 7, the DPrC yield reached a high yield of 58 mol%, while the by-product / DPrC was suppressed to 1.1 mol%. 2 In the catalyst structure of Example 1, the DPrC yield reached a high yield of 59 mol%, and the byproduct / DPrC was suppressed to 1.0 mol%. Moreover, in any structure, the cerium oxide powder did not peel off from the substrate even after the reaction, and all had high adhesion. It was also confirmed that when each structure was repeatedly used after being re-fired in the same way as in Example 1, the reaction results were almost unchanged, and the cerium oxide powder did not peel off from the substrate.

[0182] (Example 8)

[0183] The same cerium oxide powder, silica binder (SUMICERAM, P-700-D manufactured by Asahi Chemical Industries, Ltd. (mainly a mixture of silica powder with an average particle size of about 5 μm, a siloxane-based binder and water)) and water as in Example 1 were weighed in a weight ratio of 2:0.95:1.5 to prepare 50 g of a mixed solution for preparing a catalyst layer, which was filled in a 50 cc beaker. The silica binder, which would become an intermediate layer between the catalyst layer and the catalyst-coated substrate, was not applied in advance, and all other operations were performed in the same manner as in Example 2 to prepare a 30 g / m2-attached catalyst layer. 2 The catalyst structure of Example 8. The catalyst layer thickness at this time is estimated to be about 20 μm. As a result of the reaction evaluation using this structure, the DPrC yield reached a high yield of 54 mol%, while the byproduct / DPrC was suppressed to 0.9 mol%. Even after the reaction, the cerium oxide powder did not peel off from the substrate, and had high adhesion. However, it was confirmed that when the present structure was repeatedly used after being re-fired in the same way as Example 1, although the reaction results were almost unchanged, a part of the cerium oxide powder peeled off from the substrate. However, this peeling was not a problem.

[0184] (Example 9)

[0185] As described below, catalyst components different from those in the above-described embodiments were used.

[0186] That is, sodium hydroxide was introduced into a solution in which cerium nitrate and zirconium nitrate were dissolved so that cerium accounted for 20 atomic weight % to generate a precipitate, which was then filtered and washed with water, and then fired at 1273K for 3 hours in an air atmosphere. Thereafter, the precipitate was sized with a sieve to obtain a cerium zirconium oxide powder having an average particle size of about 10 μm and an impurity concentration of less than 0.1%. Except for this, all operations were carried out in the same manner as in Example 2 to prepare a cerium zirconium oxide powder having an average particle size of about 10 μm and an impurity concentration of less than 0.1%. 2 The catalyst structure. The catalyst layer thickness at this time is estimated to be about 20 μm. As a result of the reaction evaluation using this structure, the DPrC yield reached a high yield of 48 mol%, and the by-product / DPrC was suppressed to 0.8 mol%. Even the cerium zirconium oxide powder used for the reaction did not peel off from the substrate, and had high adhesion. It was also confirmed that when this structure was repeatedly used after being re-fired in the same way as Example 1, the reaction results were almost unchanged, and the cerium zirconium oxide powder did not peel off from the substrate.

[0187] (Examples 10 to 14)

[0188] The catalyst structure was manufactured in the same manner as in Example 1. When the catalyst structure was used for reaction evaluation, methanol, ethanol, n-butanol as primary alcohol, isopropanol as secondary alcohol, and tert-butanol as tertiary alcohol were used instead of 1-propanol. The evaluation was carried out in the same manner as in Example 1. As a result, the yields of dimethyl carbonate, diethyl carbonate, dibutyl carbonate, diisopropyl carbonate, and di-tert-butyl carbonate were 56 mol%, 55 mol%, 52 mol%, 48 mol%, and 42 mol%, respectively, and the by-products / carbonates were suppressed to 0.8 mol%, 0.9 mol%, 1.0 mol%, 1.4 mol%, and 1.8 mol%, respectively. Moreover, in any case, the cerium oxide powder did not peel off from the substrate after the reaction, and all had high adhesion. It was also confirmed that when the structure was repeatedly used multiple times under any conditions after being re-fired in the same manner as in Example 1, the reaction results were almost unchanged, and the cerium oxide powder did not peel off from the substrate.

[0189] (Examples 15 to 17)

[0190] The catalyst structure of Example 5 was used, and the reaction pressure was set to 2.0 MPa, 4.0 MPa, and 8.0 MPa. The reaction evaluation was carried out in the same manner as in Example 3 except that the reaction pressure was 2.0 MPa, 4.0 MPa, and 8.0 MPa. As a result, the DPrC yields reached high yields of 55 mol%, 55 mol%, and 54 mol%, respectively, and the byproduct / DPrC was suppressed to 0.7 mol%, 0.6 mol%, and 0.5 mol%, respectively. Moreover, the cerium oxide powder did not peel off from the substrate even after the reaction, and had high adhesion. It was also confirmed that after the re-firing treatment as in Example 1, when the present structure was repeatedly used multiple times under any conditions, the reaction results were almost unchanged, and the cerium oxide powder did not peel off from the substrate.

[0191] (Example 18)

[0192] Cerium oxide (produced by Daiichi Kizenso Co., Ltd., HS, average particle size of about 5 μm, impurity concentration of 0.02% or less) was calcined at 873K in an air atmosphere for 3 hours to obtain a powdered solid catalyst. This powder was used to prepare a cerium oxide coating with a weight of 200 g / m 2 , except for this, all operations were performed in the same manner as in Example 1 to prepare a catalyst structure. The catalyst layer thickness at this time was estimated to be about 140 μm. As a result of the reaction evaluation using this structure, under this condition, the DPrC yield reached 40 mol%. On the other hand, the byproduct / DPrC was suppressed to 2.9 mol%. Moreover, even after the reaction, the cerium oxide powder did not peel off from the substrate, and had high adhesion. It was also confirmed that when this structure was repeatedly used after being re-fired in the same manner as in Example 1, the reaction results were almost unchanged, and the cerium oxide powder did not peel off from the substrate.

[0193] (Example 19)

[0194] Except for using SUS304 as the honeycomb substrate, all operations were carried out in the same manner as in Example 1 to prepare a catalyst structure and conduct reaction evaluation. As a result, under the present conditions, the DPrC yield reached 51 mol%. On the other hand, the byproduct / DPrC was suppressed to 1.2 mol%. Moreover, even after the reaction, the cerium oxide powder did not peel off from the substrate, and had high adhesion. It was also confirmed that when the present structure was repeatedly used after being subjected to the same re-firing treatment as in Example 1, the reaction results were almost unchanged, and the cerium oxide powder did not peel off from the substrate.

[0195] (Example 20)

[0196] In addition to using ceramics (manufactured by Nippon Insulators Co., Ltd., 400 cells / inch) as the honeycomb substrate 2 Except for the cylindrical shape of the catalyst, trade name: HONEYCERAM, all operations were carried out in the same manner as in Example 1 to prepare a catalyst structure and conduct reaction evaluation. As a result, under the present conditions, the DPrC yield reached 50 mol%. On the other hand, the byproduct / DPrC was suppressed to 1.2 mol%. Moreover, even after the reaction, the cerium oxide powder did not peel off from the substrate, and had high adhesion. It was also confirmed that when the present structure was repeatedly used after being subjected to the same re-firing treatment as in Example 1, the reaction results were almost unchanged, and the cerium oxide powder did not peel off from the substrate.

[0197] (Example 21)

[0198] As an inorganic binder, silica sol (manufactured by Nikko Catalysts & Chemicals Co., Ltd.) was used. Except for this, all operations were carried out in the same manner as in Example 1 to prepare a catalyst structure and to conduct reaction evaluation. As a result, under the present conditions, the DPrC yield reached 54 mol%. On the other hand, the byproduct / DPrC was suppressed to 1.1 mol%. Moreover, even after the reaction, the cerium oxide powder did not peel off from the substrate, and had high adhesion. It was also confirmed that when the present structure was repeatedly used after being subjected to the same re-firing treatment as in Example 1, the reaction results were almost unchanged, and the cerium oxide powder did not peel off from the substrate.

[0199] (Example 22)

[0200] As an inorganic binder, alumina sol (manufactured by Nissan Chemical Co., Ltd.) was used. In addition, all operations were performed in the same manner as in Example 1 to prepare a catalyst structure and to perform reaction evaluation. As a result, under the present conditions, the DPrC yield reached 51 mol%. On the other hand, byproduct / DPrC was suppressed to 1.2 mol%. Moreover, even after the reaction, the cerium oxide powder did not peel off from the substrate, and had high adhesion. It was also confirmed that when the present structure was repeatedly used after being subjected to the same re-firing treatment as in Example 1, the reaction results were almost unchanged, and the cerium oxide powder did not peel off from the substrate.

[0201] (Example 23)

[0202] Except that benzonitrile was used as a hydrating agent, all operations were performed in the same manner as in Example 1 to prepare a catalyst structure and to conduct reaction evaluation. As a result, under the present conditions, the DPrC yield reached 40 mol%. On the other hand, the byproduct / DPrC was suppressed to 2.8 mol%. Moreover, even after the reaction, the cerium oxide powder did not peel off from the substrate, and had high adhesion. It was also confirmed that after the structure was subjected to the same re-firing treatment as in Example 1, when it was repeatedly used under the present conditions, the reaction results were almost unchanged, and the cerium oxide powder did not peel off from the substrate.

[0203] (Comparative Example 1)

[0204] Increase the nitrogen blowing pressure after coating the cerium oxide powder, and finally make the cerium oxide adhesion amount reach 8g / m 2 , except for this, all operations were performed in the same manner as in Example 1 to prepare a catalyst structure. The catalyst layer thickness of the structure obtained by this operation was estimated to be about 6 μm. The results of the reaction evaluation using this structure showed that the DPrC yield was limited to 30 mol% under this condition, while the byproduct / DPrC increased to 3.6 mol%. In addition, after the reaction, the cerium oxide powder was not peeled off from the substrate and had high adhesion.

[0205] (Comparative Example 2)

[0206] The adhesion amount of cerium oxide is 250g / m 2 , except for this, all the same operations as in Example 1 were performed to prepare a catalyst structure. The catalyst layer thickness of the structure obtained by this operation was estimated to be about 180 μm. The results of the reaction evaluation using this structure showed that the DPrC yield was limited to 22 mol% under this condition, while the byproduct / DPrC increased to 4.5 mol%. In addition, after the reaction, it was observed that the cerium oxide powder was partially peeled off from the substrate, and the adhesion was insufficient.

[0207] The above results are summarized in Tables 1 to 4.

[0208] In each table, "Metal Honeycomb 1" means 100 cells / inch 2 Cylindrical metal honeycomb (steel type: YUS205M1, plate thickness: 50μm, fin (corrugated foil) shape: sine wave, made by Nippon Steel & Sumitomo Metal Materials), "Metal Honeycomb 2" means 200 cells / inch 2 Cylindrical metal honeycomb (steel type: YUS205M1, plate thickness: 50μm, fin (corrugated foil) shape: sine wave, made by Nippon Steel & Sumitomo Metal Materials), "Metal Honeycomb 3" means 300 cells / inch 2 Cylindrical metal honeycomb (steel type: YUS205M1, plate thickness: 50μm, fin (corrugated foil) shape: sine wave, made by Nippon Steel & Sumitomo Metal Materials), "Metal Honeycomb 4" means 100 cells / inch 2 Cylindrical metal honeycomb (steel type: SUS304, plate thickness: 50μm, fin (corrugated foil) shape: sine wave, made by Nippon Steel & Sumitomo Metal Materials), "ceramic honeycomb" means 400 cells / inch 2 A cylindrical ceramic honeycomb (manufactured by Nippon Insulator Co., Ltd., trade name: HONEYCERAM).

[0209] In addition, in each table, "Silica 1" represents silica from SUMICERAM P-750 (produced by Asahi Chemical Industries, Ltd.), "Silica 2" represents silica from SUMICERAM P-700-D (produced by Asahi Chemical Industries, Ltd.), "Silica 3" represents silica from silica sol (produced by Nikko Catalysts & Chemicals Co., Ltd.), and "Alumina" represents alumina from alumina sol (produced by Nissan Chemical Industries, Ltd.).

[0210] [Table 1]

[0211]

[0212] [Table 2]

[0213]

[0214] [Table 3]

[0215]

[0216] [Table 4]

[0217]

[0218] Above, in embodiment 1~23, yield is good to produce carbonate, also suppressed the generation of by-product.And, the catalyst structure of embodiment 1~23 is in repeated use, and the reduction of reaction efficiency (catalytic activity) is also suppressed, and, the disengagement of solid catalyst is also suppressed.

[0219] In contrast, in Comparative Example 1,2, the solid catalyst amount carried is too much or too little, and as a result, the yield of carbonate is low, and by product also generates in a large number. And, in the Comparative Example 2 that carries solid catalyst in a large number, observe the peeling of solid catalyst, the reduction of reaction efficiency that causes of departure.

[0220] In addition, when the reaction was carried out in the same manner as in Example 1 without supporting the solid catalyst on the substrate, the powdered solid catalyst was further pulverized and clogged the filter, making it impossible to continue the operation.

[0221] (Example 24)

[0222] The adhesive of Example 2 was 30 g / m 2 The catalyst structure of cerium oxide was evaluated by continuous flow reaction. A buffer tank was prepared and filled with 445 g of liquid of the same composition as used in the reaction. Then, the reaction liquid was transported to the reactor at a rate of 111 g / h, and the same amount of liquid was taken out from the reactor. Here, the residence time of the reaction liquid in the reactor was 240 minutes, which was 2 / 3 of the case of Examples 1 to 7.

[0223] As a result, the yields of DPrC after 6 hours, 12 hours, 18 hours and 22 hours of reaction time were all basically stable at 29 mol%. It was confirmed that the byproduct / DPrC at each moment was 0.8 mol%, 1.0 mol%, 1.0 mol% and 1.0 mol% respectively, becoming a saturated and stable state. Moreover, even after the reaction, the cerium oxide powder did not peel off from the substrate and had high adhesion. It was also confirmed that when the present structure was repeatedly used, the reaction results were almost unchanged and the cerium oxide powder did not peel off from the substrate. Based on the above, it is known that the catalyst structure of the present invention can also be used in a continuous reactor with a fast flow rate of raw materials.

[0224] (Example 25)

[0225] Catalyst components different from those in the above examples were prepared as follows.

[0226] First, lanthanum oxide (LaO3·6H2O) as a catalyst precursor was dissolved in 2 g of ultrapure water in a 20 mL sample bottle.

[0227] Furthermore, 2.5 g of CeO2 fired at 600° C. for 3 hours was added to a 50 mL glass beaker, and the solution containing the precursor was added to the CeO2 in the beaker in a uniform manner, and stirred and mixed with a glass rod. The beaker was placed on a heating stirrer set at about 80° C. in advance, and the solution in the beaker was stirred and mixed with a glass rod. Furthermore, the water was evaporated while being stirred and mixed with a glass rod to make the metal component uniform, and stirring was continued until the water evaporated.

[0228] Separately, 2 g of ultrapure water was added to the sample bottle containing the precursor solution, and the mixture was co-washed and added to the beaker containing CeO2. Similarly, the mixture was stirred and mixed with a glass rod while evaporating the water, and the co-washing and subsequent operations were performed again. Thereafter, the mixture was dried on a heating stirrer for about 2 hours in order to completely evaporate the water in the beaker.

[0229] The catalyst precursor components in the beaker were transferred to a crucible and fired in a muffle furnace. The firing program was set to increase the temperature at a rate of 2°C / min and fire at 400°C for 4 hours.

[0230] Using the catalyst of Example 25 obtained in this manner and a comparative catalyst as a reference example prepared in the same manner as in Example 25 except that lanthanum oxide was not contained, carbonate was produced under the same conditions as described below.

[0231] (Conditions for Carbonate Formation Reaction)

[0232] Feeding molar ratio:

[0233] (PrOH) / (2-CP) / (catalyst (CeO2+LaO3 or CeO2))=300 / 50 / 1

[0234] Catalyst: Foil-immobilized sample (about 150 g / m 2 )

[0235] Reaction liquid volume: 325g

[0236] ·Liquid delivery and liquid withdrawal volume: 162.5g / h

[0237] ·Residence time: 2h

[0238] Reaction pressure: 0.9MPa

[0239] Reaction temperature: 132℃

[0240] These results are shown in Figure 3 . As from Figure 3 As can be seen from the curve graph, in Example 25, it was confirmed that by adjusting the composition of the catalyst, a high catalytic activity can be maintained for a long time without the need for regeneration treatment such as re-firing as described in Example 1. Figure 3 As shown in the curve diagram, when using the comparison catalyst of reference example, although the yield of carbonate after the reaction just started is high, it is confirmed that the activity decreases. On the contrary, when using the catalyst of embodiment 25, even after 50 hours of reaction, the catalytic activity is also not substantially reduced and is maintained at a good level.

[0241] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited to the above examples. A person skilled in the art with common knowledge in the technical field to which the present invention belongs can know that various variations or modifications can be thought of within the scope of the technical ideas described in the scope of the present invention, and these should also belong to the technical scope of the present invention.

[0242] Explanation of symbols

[0243] 1. 1A: Catalyst structure for carbonate production; 10: substrate; 20: catalyst layer; 30: intermediate layer; 40: solid catalyst; 50: inorganic binder; 60: carbonate production device; 100: carbonate production equipment.

Claims

1. A method for producing a carbonate, Features: The method comprises the steps of reacting a monohydric alcohol with carbon dioxide in the presence of a catalyst structure and a hydrating agent to produce a carbonate ester. The catalyst structure includes a substrate and a catalyst layer formed on at least a portion of a surface of the substrate and containing a solid catalyst and an inorganic binder. The solid catalyst contains cerium oxide, The solid catalyst loading is 15 g / m 2 Above 200g / m 2 the following, The inorganic binder contains silicon dioxide and / or aluminum oxide, The catalyst structure further comprises an intermediate layer formed between the catalyst layer and the substrate and composed of the inorganic binder. The solid content of the inorganic binder in each of the catalyst layer and the intermediate layer is 1 g / m 2 Above 100g / m 2 the following, The average thickness of the catalyst layer is 12 μm to 180 μm.

2. The method for producing a carbonate according to claim 1, Features: The inorganic binder contains silicon dioxide.

3. The method for producing a carbonate according to claim 1 or 2, Features: The solid catalyst loading is 15 g / m 2 Above 150g / m 2 the following.

4. The method for producing a carbonate according to claim 1 or 2, Features: The solid catalyst loading is 15 g / m 2 Above 70g / m 2 the following.

5. The method for producing a carbonate according to claim 1 or 2, Features: The substrate has a through hole that serves as a flow path for the monohydric alcohol and the carbon dioxide. The catalyst layer is formed on the surface of the communicating hole.

6. The method for producing a carbonate according to claim 1 or 2, Features: The solid catalyst also contains oxides of rare earth elements.

7. The method for producing a carbonate according to claim 6, Features: The solid catalyst contains lanthanum oxide.

8. The method for producing a carbonate according to claim 1 or 2, Features: The average thickness of the catalyst layer is 15 μm to 150 μm.

9. The method for producing a carbonate according to claim 1 or 2, Features: The substrate is a metal honeycomb.

10. The method for producing a carbonate according to claim 1 or 2, Features: The hydrating agent contains a nitrile compound.

11. The method for producing a carbonate according to claim 1 or 2, Features: The hydrating agent contains 2-cyanopyridine.

12. A catalyst structure for producing carbonate esters, It is characterized in that include: Base material; and a catalyst layer formed on at least a portion of the surface of the substrate and containing a solid catalyst and an inorganic binder, The solid catalyst contains cerium oxide, The solid catalyst loading is 15 g / m 2 Above 200g / m 2 the following, The inorganic binder contains silicon dioxide and / or aluminum oxide, The catalyst structure further comprises an intermediate layer formed between the catalyst layer and the substrate and composed of the inorganic binder. The solid content of the inorganic binder in each of the catalyst layer and the intermediate layer is 1 g / m 2 Above 100g / m 2 the following, The average thickness of the catalyst layer is 12 μm to 180 μm.

13. The catalyst structure for producing carbonate according to claim 12, Features: The solid catalyst loading is 15 g / m 2 Above 150g / m 2 the following.

14. A carbonate production device, It is characterized in that include: The catalyst structure for producing carbonate according to claim 12 or 13; and A supply passage for supplying at least a monohydric alcohol and carbon dioxide to the catalyst structure.

15. The carbonate production device according to claim 14, Features: The carbonate production apparatus further includes a discharge passage through which carbonate produced from the monohydric alcohol and carbon dioxide passes.

16. The carbonate production device according to claim 14, Features: A plurality of the catalyst structures are arranged in series.

17. The carbonate production device according to claim 14, Features: An integrated structure having a plurality of the catalyst structures arranged in parallel.

18. A method for producing a carbonate ester, It is characterized in that include: In the carbonate production apparatus according to claim 14, the step of circulating the reaction substrate containing the monohydric alcohol and carbon dioxide at a space velocity of 0.005 to 5000 per minute is included.

Citation Information

Patent Citations

  • Production of carbonate diester

    JP1994145113A

  • Method for producing carbonic acid ester

    JP2012162523A

  • Method for accelerating decomposition of hydrogen peroxide

    JP2013000646A

  • Catalyst cartridge and peroxide-containing aqueous solution treatment apparatus equipped with the same

    JP2016059901A

  • Catalyst for hydrogen peroxide decomposition, method for producing same, and method for decomposing hydrogen peroxide using said catalyst

    WO2016093329A1