Semiconductor ion etching cleaning method

The two-step ion etching cleaning method is used to process particles of different particle sizes step by step, which solves the problem that traditional methods are difficult to clean and control the corrosion rate, and achieves efficient particle removal and semiconductor surface cleaning.

CN112447496BActive Publication Date: 2024-10-18SAE TECH DELEVOPMENT DONGGUAN
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN201910800497.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-08-28
Publication Date
2024-10-18
Estimated Expiration
2039-08-28

AI Technical Summary

Technical Problem

In the semiconductor processing process, traditional particle removal methods are difficult to meet the cleaning conditions, and the corrosion rate of hydroxide ions is difficult to control at different temperatures and concentrations, affecting the cleaning effect.

Method used

A two-step ion etching cleaning method is adopted. The first step uses 30mT chamber pressure, 1000W~1200W power, argon or nitrogen gas for particles with a particle size of ≥30nm. The second step uses 20mT chamber pressure for particles of 10-30nm. , 1000W power, oxygen or nitrogen gas, gradually remove particles through step-by-step ion etching, and remove the oxide layer if necessary.

Benefits of technology

It effectively removes particles on the semiconductor surface and achieves a cleaning effect of more than 95%. It also controls the corrosion rate and ensures cleanliness and no damage to the semiconductor surface.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a semiconductor ion etching cleaning method, including a first ion etching cleaning and a second ion etching cleaning; the process parameters of the first ion etching cleaning are: the chamber pressure is 30mT, the power is 1000W-1200W, the gas introduced is argon or nitrogen, when argon is used, the gas flow rate is 600sccm, when nitrogen is used, the gas flow rate is 500sccm, and the time is 35-55 seconds; the process parameters of the second ion etching cleaning are: the chamber pressure is 20mT, the power is 1000W, the gas introduced is oxygen or nitrogen, when oxygen is used, the gas flow rate is 50sccm, when nitrogen is used, the gas flow rate is 100-120sccm, and the time is 60-80 seconds. The method of the present invention can effectively remove the particles on the surface of the semiconductor by using ion etching step by step for particles of different particle sizes to achieve the expected effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to semiconductor surface treatment, in particular to a semiconductor ion etching cleaning method. Background Art

[0002] In semiconductor processing, there are usually many particles attached. The traditional way to remove particles is to use a mixture of deionized water, hydrogen peroxide and ammonia to separate the particles from the silicon wafer. However, due to the uneven size of the particles, it is difficult to meet the cleaning conditions. In addition, the corrosion rate of hydroxide ions varies under different temperature and concentration conditions, making it difficult to control. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a semiconductor ion etching cleaning method.

[0004] To achieve the above object, the technical solution adopted by the present invention is: a semiconductor ion etching cleaning method, comprising the following steps:

[0005] (1) First ion etching cleaning;

[0006] (2) Second ion etching cleaning;

[0007] The process parameters of the first ion etching cleaning are: chamber pressure of 30mT, power of 1000W-1200W, gas of argon or nitrogen, when argon is used, gas flow rate of 600sccm, when nitrogen is used, gas flow rate of 500sccm, time of 35-55 seconds;

[0008] The process parameters of the second ion etching cleaning are: chamber pressure is 20mT, power is 1000W, the gas introduced is oxygen or nitrogen, when using oxygen, the gas flow rate is 50sccm, when using nitrogen, the gas flow rate is 100-120sccm, and the time is 60-80 seconds.

[0009] Usually, the particles on the surface of the semiconductor are mainly composed of inorganic materials, composed of silicon dioxide, and their particle sizes can also be divided into two types, one with a particle size of ≥30nm and the other with a particle size of ≤30nm. The first ion etching is mainly used to remove particles of 30-100nm, and the second ion etching is mainly used to remove particles of 10-30nm. The method of the present invention uses ion etching to gradually clean particles of different particle sizes in steps, and can effectively remove particles on the surface of the semiconductor under the cleaning conditions of the present invention, achieving the expected effect.

[0010] As a preferred embodiment of the semiconductor ion etching cleaning method of the present invention, when the size of the semiconductor surface particles is ≥30nm and the proportion is ≤20%, the first ion etching cleaning time is 35 seconds;

[0011] When the size of the particles on the surface of the semiconductor is ≥30 nm, the proportion is 20-50%, the first ion etching cleaning time is 40 seconds;

[0012] When the size of the particles on the surface of the semiconductor is ≥30 nm, the proportion is 50-70%, the first ion etching cleaning time is 50 seconds;

[0013] When the proportion of particles on the surface of the semiconductor with a size of ≥30 nm is 70-80%, the time for the first ion etching cleaning is 55 seconds.

[0014] As a preferred embodiment of the semiconductor ion etching cleaning method of the present invention, when the proportion of particles on the surface of the semiconductor with a size of ≤30 nm is 20-30%, the second ion etching cleaning time is 60 seconds;

[0015] When the size of the particles on the surface of the semiconductor is ≤30 nm, the proportion is 30-50%, and the second ion etching cleaning time is 65 seconds;

[0016] When the size of the particles on the surface of the semiconductor is ≤30 nm, the proportion is 50-70%, the second ion etching cleaning time is 70 seconds;

[0017] When the proportion of particles with a size of ≤30 nm on the surface of the semiconductor is 70-80%, the time for the second ion etching cleaning is 80 seconds.

[0018] When the contents of particles of different particle sizes are different, the cleaning time needs to be changed accordingly. The above cleaning time is preferably used for each particle size range and content, which has a better cleaning effect and does not damage the semiconductor surface.

[0019] As a preferred embodiment of the semiconductor ion etching cleaning method of the present invention, the first ion etching cleaning further includes step (1a): using ion etching cleaning to remove the oxide layer on the semiconductor surface, and the process parameters are: chamber pressure of 5mT, power of 300W, CF4 gas, gas flow rate of 50sccm, and time of 5 seconds. The above conditions can effectively clean the oxide layer on the semiconductor surface.

[0020] As a preferred embodiment of the semiconductor ion etching cleaning method of the present invention, the gas used for the second ion etching cleaning is nitrogen, and the cleaning effect of nitrogen is better than that of oxygen.

[0021] The beneficial effects of the present invention are as follows: the present invention provides a semiconductor ion etching cleaning method, which gradually cleans particles of different particle sizes by ion etching in steps, and can effectively remove particles on the semiconductor surface under the cleaning conditions of the present invention, thereby achieving the expected effect. DETAILED DESCRIPTION

[0022] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0023] Example 1

[0024] An embodiment of the semiconductor ion etching cleaning method of the present invention comprises the following steps:

[0025] (1) Ion etching was used to remove the oxide layer on the semiconductor surface. The process parameters were: chamber pressure 5 mT, power 300 W, CF4 gas, gas flow rate 50 sccm, and time 5 seconds.

[0026] (2) Ion etching of a semiconductor containing 70-80% of particles with a size of ≥30 nm, with the following process parameters: chamber pressure of 30 mT, power of 1200 W, argon gas, gas flow of 600 sccm, and time of 55 seconds;

[0027] (3) Ion etching of a semiconductor containing 20-30% of particles with a size of ≤30 nm, with the following process parameters: chamber pressure of 20 mT, power of 1000 W, oxygen gas, gas flow rate of 50 sccm, and time of 60 seconds.

[0028] Example 2

[0029] An embodiment of the semiconductor ion etching cleaning method of the present invention comprises the following steps:

[0030] (1) Ion etching was used to remove the oxide layer on the semiconductor surface. The process parameters were: chamber pressure 5 mT, power 300 W, CF4 gas, gas flow rate 50 sccm, and time 5 seconds.

[0031] (2) Ion etching a semiconductor containing 50-70% of particles with a size of ≥30 nm, with the following process parameters: chamber pressure of 30 mT, power of 1000 W, nitrogen gas, gas flow rate of 500 sccm, and time of 50 seconds;

[0032] (3) Ion etching of a semiconductor containing 30-50% of particles with a size of ≤30 nm, with the following process parameters: chamber pressure of 20 mT, power of 1000 W, nitrogen gas, gas flow of 120 sccm, and time of 65 seconds.

[0033] Example 3

[0034] An embodiment of the semiconductor ion etching cleaning method of the present invention comprises the following steps:

[0035] (1) Ion etching was used to remove the oxide layer on the semiconductor surface. The process parameters were: chamber pressure 5 mT, power 300 W, CF4 gas, gas flow rate 50 sccm, and time 5 seconds.

[0036] (2) Ion etching of a semiconductor containing 20-50% of particles with a size of ≥30 nm, with the following process parameters: chamber pressure of 30 mT, power of 1100 W, argon gas, gas flow of 600 sccm, and time of 40 seconds;

[0037] (3) Ion etching of a semiconductor containing 50-80% of particles with a size of ≤30 nm, with the following process parameters: chamber pressure of 20 mT, power of 1000 W, nitrogen gas, gas flow rate of 110 sccm, and time of 70 seconds.

[0038] Example 4

[0039] An embodiment of the semiconductor ion etching cleaning method of the present invention comprises the following steps:

[0040] (1) Ion etching was used to remove the oxide layer on the semiconductor surface. The process parameters were: chamber pressure 5 mT, power 300 W, CF4 gas, gas flow rate 50 sccm, and time 5 seconds.

[0041] (2) Ion etching of a semiconductor containing particles with a size of ≥30 nm and a proportion of ≤20% is performed, with the process parameters being: chamber pressure of 30 mT, power of 1000 W, nitrogen gas, gas flow of 500 sccm, and time of 35 seconds;

[0042] (3) Ion etching is performed on a semiconductor containing particles with a size of ≤30 nm and a proportion of ≥80%. The process parameters are: chamber pressure of 20 mT, power of 1000 W, nitrogen gas, gas flow rate of 120 sccm, and time of 80 seconds.

[0043] The particles on the semiconductor surface after cleaning by the semiconductor ion etching cleaning method described in Examples 1 to 4 are reduced by more than 95% compared with those before cleaning.

[0044] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A semiconductor ion etching cleaning method, characterized in that: The following steps are involved: (1) First ion etching cleaning; (2) Second ion etching cleaning; The process parameters of the first ion etching cleaning are: chamber pressure of 30mT, power of 1000W-1200W, gas of argon or nitrogen, when argon is used, gas flow rate of 600sccm, when nitrogen is used, gas flow rate of 500sccm, time of 35-55 seconds; The process parameters of the second ion etching cleaning are: chamber pressure of 20mT, power of 1000W, gas of oxygen or nitrogen, when oxygen is used, gas flow rate of 50sccm, when nitrogen is used, gas flow rate of 100-120sccm, time of 60-80 seconds; When the size of the particles on the semiconductor surface is ≥30 nm and the proportion is ≤20%, the first ion etching cleaning time is 35 seconds; When the size of the particles on the surface of the semiconductor is ≥30 nm, the proportion is 20-50%, the first ion etching cleaning time is 40 seconds; When the size of the particles on the surface of the semiconductor is ≥30 nm, the proportion is 50-70%, the first ion etching cleaning time is 50 seconds; When the size of the particles on the surface of the semiconductor is ≥30 nm, the proportion is 70-80%, and the first ion etching cleaning time is 55 seconds; When the proportion of particles on the surface of the semiconductor with a size of ≤30 nm is 20-30%, the second ion etching cleaning time is 60 seconds; When the size of the particles on the surface of the semiconductor is ≤30 nm, the proportion is 30-50%, and the second ion etching cleaning time is 65 seconds; When the size of the particles on the surface of the semiconductor is ≤30 nm, the proportion is 50-70%, the second ion etching cleaning time is 70 seconds; When the proportion of particles with a size of ≤30 nm on the surface of the semiconductor is 70-80%, the time for the second ion etching cleaning is 80 seconds.

2. The semiconductor ion etching cleaning method according to claim 1, characterized in that: Before the first ion etching cleaning, the process also includes step (1a): using ion etching cleaning to remove the oxide layer on the surface of the semiconductor, and the process parameters are: chamber pressure is 5mT, power is 300W, the gas introduced is CF4, the gas flow rate is 50sccm, and the time is 5 seconds.

3. The semiconductor ion etching cleaning method according to claim 1, characterized in that: The gas used for the second ion etching cleaning is nitrogen.

Citation Information

Patent Citations

  • Cleaning method, processing device, and storage medium

    CN103650117A

  • Method of removing contamination layer from optical surface, method of producing cleaning gas, and corresponding structure of cleaning and producing cleaning gas

    JP2012256944A

  • Method of reducing defects in anti-reflective coatings and semiconductor structures fabricated thereby

    US6144083A