Negative electrode active material, method for preparing negative electrode active material, negative electrode and secondary battery comprising the negative electrode
By using artificial graphite cores and carbon coatings in the negative electrode active material, the specific surface area of the edge surface is controlled, solving the problem of side reactions between the negative electrode and the electrolyte during high-temperature storage and improving the performance of the secondary battery.
Patent Information
- Application Number
- CN201980050952.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-08-17
- Filing Date
- 2019-08-16
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2039-08-16
AI Technical Summary
Existing technologies result in numerous side reaction sites between the negative electrode and the electrolyte during high-temperature storage, leading to significant lithium loss and impacting the capacity and lifespan of secondary batteries.
The negative electrode active material is prepared by using an artificial graphite core and a carbon coating, and by controlling the specific surface area of the edge surface within the range of 1.0 m2/g to 1.9 m2/g to reduce side reactions with the electrolyte, combined with appropriate heat treatment and pulverization processes.
It effectively suppresses side reactions between the negative electrode and the electrolyte during high-temperature storage, reduces lithium loss, and improves the initial efficiency of the secondary battery and the capacity retention rate during high-temperature storage.
Smart Images

Figure CN112514111B_ABST
Abstract
Description
Technical Field
[0002] CROSS-REFERENCE TO RELATED APPLICATIONS
[0003] This application claims the benefit of Korean Patent Application No. 10-2018-0096155 filed on August 17, 2018, in the Korean Intellectual Property Office, the disclosure of which is incorporated herein by reference in its entirety. Technical Field
[0004] The present invention relates to a negative electrode active material, a method for preparing the negative electrode active material, a negative electrode and a secondary battery comprising the negative electrode, wherein the negative electrode active material comprises: a core comprising artificial graphite; and a carbon coating disposed on the core, wherein the edge surface has a thickness of 1.0 m 2 / g to 1.9m 2 / g specific surface area. Background Art
[0005] With the recent technological development and increased demand for mobile devices, the demand for batteries as energy sources has increased significantly, and therefore various studies have been conducted on batteries that can meet various needs. In particular, as a power source for such devices, lithium secondary batteries with excellent life and cycle characteristics and high energy density have been actively studied.
[0006] A lithium secondary battery refers to a battery in which a nonaqueous electrolyte containing lithium ions is contained in an electrode assembly, the electrode assembly containing a positive electrode containing a positive electrode active material capable of inserting / deinserting lithium ions, a negative electrode containing a negative electrode active material capable of inserting / deinserting lithium ions, and a microporous separator disposed between the positive electrode and the negative electrode. As the negative electrode active material, lithium metal, lithium alloy, carbon-based active material, and silicon-based active material are used.
[0007] As carbon-based active materials, various carbon-based materials such as artificial graphite, natural graphite, and hard carbon are used, among which graphite-based active materials that can ensure the life characteristics of lithium secondary batteries due to excellent reversibility have been most widely used. Regarding graphite-based active materials, since the discharge voltage to lithium is as low as -0.2V, a battery using graphite-based active materials can exhibit a high discharge voltage of 3.6V, and thus, graphite-based active materials provide many advantages in terms of energy density of lithium batteries.
[0008] The temperature of the secondary battery increases during its use, and therefore, functional degradation of the secondary battery may occur during high-temperature storage. In particular, since a side reaction occurs between the negative electrode and the electrolyte during high-temperature storage and lithium is lost in a reversible reaction, there is a limitation that the remaining capacity after high-temperature storage is small.
[0009] Conventionally, in order to suppress functional degradation of secondary batteries during high temperature storage, a technique for preparing a negative electrode by mixing artificial graphites of different particle sizes has been proposed. However, this technique is undesirable in that the low capacity of artificial graphites with relatively small diameters reduces the energy density of the negative electrode and the side reaction between the negative electrode and the electrolyte is not smoothly resolved.
[0010] Therefore, a new technology is needed that can minimize the side reaction sites between the anode and the electrolyte during high-temperature storage and can minimize the loss of lithium participating in the reversible reaction. Summary of the invention
[0011] Technical issues
[0012] One aspect of the present invention provides a negative electrode active material, a method for preparing the negative electrode active material, a negative electrode, and a secondary battery comprising the negative electrode, wherein the negative electrode active material can minimize the side reaction sites between the negative electrode and the electrolyte during high temperature storage and can minimize the loss of lithium participating in the reversible reaction.
[0013] Technical Solution
[0014] According to one aspect of the present invention, there is provided a negative electrode active material, comprising: a core comprising artificial graphite; and a carbon coating disposed on the core, wherein the edge surface of the negative electrode active material has a thickness of 1.0 m 2 / g to 1.9m 2 / g specific surface area.
[0015] According to another aspect of the present invention, there is provided a method for preparing a negative electrode active material, the method comprising: preparing needle coke; pulverizing the needle coke at a pressure of 10 MPa to 20 MPa; preparing a core by heat treating the pulverized needle coke at a temperature of 3,000° C. or above after mixing the pulverized needle coke with a carbonaceous precursor; and forming a carbon coating on the core.
[0016] According to another aspect of the present invention, there is provided a negative electrode, the negative electrode comprising a current collector and a negative electrode active material layer disposed on the current collector, wherein the negative electrode active material layer comprises a negative electrode active material, wherein the negative electrode active material contains a core comprising artificial graphite; and a carbon coating disposed on the core, wherein the edge surface has a thickness of 0.5 m 2 / g to 1.1m 2 / g specific surface area.
[0017] According to another aspect of the present invention, there is provided a secondary battery including a negative electrode; a positive electrode; a separator disposed between the positive electrode and the negative electrode; and an electrolyte.
[0018] Beneficial Effects
[0019] According to the present invention, by using a negative electrode active material containing artificial graphite and having a small specific surface area of an edge surface causing a side reaction with an electrolyte, the side reaction between the negative electrode and the electrolyte during high temperature storage can be suppressed, and as a result, the loss of lithium participating in the reversible reaction can be reduced. Therefore, the initial efficiency of the prepared battery and the capacity retention rate during high temperature storage can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 : is a schematic diagram showing artificial graphite contained in the negative electrode active material of the present invention. DETAILED DESCRIPTION
[0021] Hereinafter, the present invention will be described in more detail to enable a clearer understanding of the present invention. In this case, it should be understood that the words or terms used in the specification and claims should not be interpreted as the meanings defined in the commonly used dictionaries, and it should be further understood that, based on the principle that the inventor can appropriately define the meanings of words or terms to best explain the present invention, these words or terms should be interpreted as having a meaning consistent with their meanings in the context of the relevant fields and technical ideas of the present invention.
[0022] The expression "average particle size (D 50 )” can be defined as the particle size when the cumulative volume in the particle size distribution curve is 50%. The average particle size (D 50 ) can be measured, for example, by using laser diffraction. Laser diffraction can generally measure particle sizes ranging from submicron to several millimeters, and can obtain highly reproducible and high-resolution results.
[0023] <Negative Electrode Active Material>
[0024] The negative electrode active material according to one embodiment of the present invention includes: a core including artificial graphite; and a carbon coating layer disposed on the core, wherein the edge surface of the negative electrode active material may have a thickness of 1.0 m 2 / g to 1.9m 2 / g specific surface area.
[0025] The core may include artificial graphite, and specifically may consist of artificial graphite.
[0026] Since the artificial graphite has excellent lithium absorption capacity, when the negative electrode active material includes the artificial graphite, the energy density of the negative electrode is improved, and thus, the charge and discharge characteristics of the secondary battery, especially the efficiency of the secondary battery, can be improved.
[0027] The artificial graphite may be a secondary particle in the form of a plurality of primary particles. Since the artificial graphite in the form of secondary particles has fewer sites causing side reactions with the electrolyte than a single particle, the side reactions between the electrolyte and the negative electrode can be suppressed. The primary particles may also correspond to artificial graphite.
[0028] The primary particles may have an average particle size (D) of 7 μm to 10 μm, specifically 8 μm to 9 μm, and more specifically 8.5 μm to 8.7 μm. 50 ). In the case where the average particle size satisfies the above range, the rapid charging performance of the secondary battery can be improved.
[0029] The secondary particles may be formed by gathering a plurality of primary particles. Specifically, the artificial graphite may be formed by combining at least two primary particles together, and more specifically, the primary particles may be combined with each other through a material formed by graphitization of a carbonaceous precursor such as an asphalt binder as a medium. The artificial graphite may have a curved surface, for example, in the form of a flake or a spike. The artificial graphite (secondary particles) may have an average particle size (D) of 15 μm to 20 μm, particularly 16 μm to 17 μm, and more particularly 16.2 μm to 17 μm. 50 ). In the case where the above range is satisfied, a high capacity and efficiency level of the secondary battery can be achieved, and the fast charging performance of the secondary battery can be improved.
[0030] Figure 1 This is a schematic diagram of artificial graphite. Figure 1 , the artificial graphite comprises layers in which hexagonal rings consisting of six carbon atoms are connected by planes. These layers are stacked in parallel, specifically, these layers are stacked in the
[0001] direction. The plane perpendicular to the stacking direction, that is, the plane of each layer is the basal plane ( Figure 1 (a)), and the basal plane may correspond to the (0001) plane. In addition, in the artificial graphite in particle form, the edges of each basal plane gather to form an edge plane ( Figure 1 (b)). The edge face is not composed of carbon atoms in the same face only, but multiple faces may exist in a zigzag shape. The edge face exists in a direction that is almost perpendicular to or nearly perpendicular to the base face.
[0031] The edge face contains carbon atoms that are not present on the same face and corresponds to the position where the site causing the side reaction with the electrolyte is most abundant. Thus, the present invention is characterized in that the side reaction with the electrolyte is controlled by using artificial graphite having a low specific surface area of the edge face as a negative electrode active material. In addition, since the amount of the carbon coating is small, the edge face specific surface area of the artificial graphite is similar to the edge face specific surface area of the negative electrode active material despite the presence of the carbon coating.
[0032] The carbon coating layer may be disposed on the core. Specifically, the carbon coating layer may cover at least a portion of the core, and more specifically, the carbon coating layer may cover the entire core.
[0033] Since the carbon coating can promote the embedding and release of lithium ions in artificial graphite, or can reduce the diffusion resistance of lithium ions, the carbon coating can contribute to the improvement of fast charging performance. In addition, the carbon coating can improve the hardness of the negative electrode active material, and thus, the carbon coating can improve the structural stability of the negative electrode active material and minimize the structural change during rolling.
[0034] The carbon coating layer may include soft carbon, and may specifically consist of soft carbon. In the case of using soft carbon instead of hard carbon, the high temperature storage performance of the battery may be improved.
[0035] In the negative electrode active material, the carbon coating may be present in an amount of 3 to 5 wt %, for example, 3.5 to 4.5 wt %. When the above range is satisfied, fast charging performance may be improved while achieving sufficiently high discharge capacity and initial efficiency.
[0036] The edge surface of the negative electrode active material may have a 1.0 m 2 / g to 1.9m 2 / g, especially 1.3m 2 / g to 1.9m 2 / g, more particularly 1.5m 2 / g to 1.7m 2 / g specific surface area. When the specific surface area is less than 1.0m 2 / g, the fast charging performance of the battery may be reduced due to excessive increase in charge transfer resistance. On the contrary, when the specific surface area is greater than 1.9m 2 / g, the reactivity between the negative electrode and the electrolyte is too high, so the durability of the battery in high-temperature storage and high-temperature cycling is reduced. Therefore, when the above range is met, a battery with a high level of fast charging performance and capable of maintaining high-temperature performance can be obtained.
[0037] The specific surface area of the edge surface of the negative electrode active material can be measured by the following method. After obtaining the nitrogen adsorption specific surface area (Brunauer-Emmett-Teller (BET)) of the negative electrode active material by a nitrogen adsorption method, the defect edge surface, the basal plane and the prismatic edge plane can be quantified by the nitrogen adsorption specific surface area by density functional theory. This is because the carbon atom density of the defect edge surface, the basal plane and the prismatic edge plane is different, and the higher the carbon atom density, the greater the adsorption energy. In this case, the sum of the specific surface areas of the defect edge surface and the prismatic edge surface is considered to be the specific surface area of the edge surface. The instrument used for measurement can be ASAP2000 (Accelerated Surface Area and Porosity Measurement System).
[0038] <Method for preparing negative electrode active material>
[0039] A method for preparing a negative electrode active material according to another embodiment of the present invention may include: preparing needle coke; pulverizing the needle coke at a pressure of 10 MPa to 20 MPa; preparing a core by heat-treating at a temperature of 3,000° C. or more after mixing the pulverized needle coke with a carbonaceous precursor; and forming a carbon coating on the core. According to the above preparation method, the negative electrode active material according to the above embodiment may be prepared.
[0040] In the preparation of needle coke, needle coke is classified into coal-based needle coke and petroleum-based needle coke, and preferably, the needle coke used in the present invention is petroleum-based needle coke. Since needle coke includes a needle-like structure and the crystallite arrangement is somewhat irregular, when the negative electrode active material is prepared by using needle coke, it is more favorable for the diffusion of lithium ions.
[0041] The effect of the negative electrode active material of the present invention may not be achieved by using mosaic coke. Since mosaic coke has a round shape, in which the amount of needle-like structures is less than that of needle coke, and the crystallites are arranged more regularly, when the negative electrode active material is prepared by using mosaic coke, the diffusion of lithium ions is difficult.
[0042] The needle coke may have an average particle size (D) of 4 μm to 6 μm, specifically 4.5 μm to 5.5 μm, and more specifically 4.8 μm to 5.2 μm. 50 ). When the above range is satisfied, the needle coke can be easily pulverized by an appropriate pulverizing pressure.
[0043] When the needle coke is pulverized under a pressure of 10 MPa to 20 MPa, the pulverization may be performed by at least one method selected from the group consisting of a pulverization process, a pulverization mixing process, a heat-treated coal pulverization process, and a pulverized coal process. Specifically, the pulverization mixing process is most preferred because it can more easily pulverize the needle coke by applying uniform pressure and heat.
[0044] The pressure used in the pulverization may be in the range of 10 MPa to 20 MPa, particularly 12 MPa to 18 MPa, and more particularly 14 MPa to 16 MPa. In the case where the pressure is lower than 10 MPa, since the needle coke is not pulverized to the desired extent, it is difficult to obtain uniform and consistent pulverized needle coke. In contrast, in the case where the pressure is greater than 20 MPa, the needle coke is excessively pulverized, and there is a limitation in that it is difficult to control the specific surface area of the edge surface of the negative electrode active material.
[0045] A jaw crusher, a gyratory crusher, a roller mill or a wheel mill can be used for the crushing.
[0046] In the process of preparing the core by heat treating at a temperature above 3,000°C after mixing crushed needle coke with a carbonaceous precursor, the carbonaceous precursor can be at least one material selected from the group consisting of asphalt binders such as coal tar pitch, rayon and polyacrylonitrile resin, or a precursor of the material.
[0047] The heat treatment may be performed in a reactor into which pulverized needle coke is added, and the heat treatment temperature may be the temperature of the reactor. The heat treatment may prepare a core including artificial graphite.
[0048] The heat treatment temperature may be 3,000° C. or more, particularly 3,000° C. to 3,500° C., and more particularly 3,200° C. to 3,400° C. In the case where the temperature is lower than 3,000° C., the capacity of the negative electrode active material may be low due to the low graphitization degree and crystallinity of the prepared artificial graphite. That is, since artificial graphite having a high degree of graphitization and high crystallinity can be prepared only when heat treatment is performed at a temperature of 3,000° C. or more, sufficient discharge capacity and efficiency can be achieved.
[0049] The heat treatment may be performed for 8 to 12 hours, particularly 9 to 11 hours, and more particularly 10 to 11 hours. When the above time is met, since artificial graphite with a high degree of graphitization and high crystallinity can be prepared, sufficient discharge capacity and efficiency can be achieved.
[0050] In the process of forming the carbon coating on the core, the carbon coating may be soft carbon. After providing at least one material selected from the group consisting of a pitch binder such as coal tar pitch, rayon, and polyacrylonitrile resin or a precursor of the material to the surface of the core, the carbon coating may be formed by heat treating the material or the precursor of the material. From the perspective of promoting uniform formation of the coating, the heat treatment process for forming the carbon coating may be performed at a temperature range of 1,000° C. to 4,000° C.
[0051] As described above, in order to prepare the negative electrode active material according to one embodiment of the present invention, that is, wherein the edge surface has 1.0 m 2 / g to 1.9m 2 / g of negative electrode active material with a specific surface area of 1000 g / cm2, the coke used to prepare the artificial graphite may be needle coke, the needle coke may be pulverized at a pulverization pressure of 10 MPa to 20 MPa, and the heat treatment may be performed at a temperature of 3,000° C. or higher. In addition, in the case where the amount of the carbon coating is maintained at a low level, the low specific surface area of the edge face of the artificial graphite may result in a low specific surface area of the edge face of the negative electrode active material.
[0052] <Negative electrode>
[0053] According to another embodiment of the present invention, the negative electrode comprises a current collector and a negative electrode active material layer disposed on the current collector, wherein the negative electrode active material layer comprises a negative electrode active material, wherein the negative electrode active material contains: a core comprising artificial graphite; and a carbon coating disposed on the core, wherein the edge surface of the negative electrode may have a thickness of 0.5 m 2 / g to 1.1m 2 / g specific surface area. The negative electrode can be prepared by using the negative electrode active material of the above embodiment. Specifically, the negative electrode active material mentioned in this embodiment (negative electrode) refers to a form in which the negative electrode active material of the above embodiment is used in the preparation process and is finally contained in the negative electrode.
[0054] The negative electrode may include a current collector. The current collector is not particularly limited as long as it has conductivity without causing adverse chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, aluminum or stainless steel whose surface is treated with one of carbon, nickel, titanium, silver, etc. may be used. Specifically, transition metals such as copper and nickel that fully adsorb carbon may be used as the current collector. The current collector may have a thickness of 6 μm to 20 μm, but the thickness of the current collector is not limited thereto.
[0055] The negative electrode active material layer may be disposed on the current collector. The negative electrode active material layer may cover one surface or both surfaces of the current collector. The negative electrode active material layer may include a negative electrode active material and a binder. Specifically, the negative electrode active material layer may include a negative electrode active material, a conductive agent, and a binder.
[0056] The negative electrode active material may be in a form in which the negative electrode active material of the above embodiment is used in a preparation process and finally contained in the negative electrode. Therefore, the properties of the negative electrode active material contained in the negative electrode of this embodiment may include all the properties of the negative electrode active material of the above embodiment.
[0057] The content of the negative electrode active material in the negative electrode active material layer may be 92 wt % to 97 wt %, for example 95.6 wt % to 95.9 wt %. When the above range is satisfied, the energy density of the prepared negative electrode may be at a sufficient level.
[0058] The binder may include various types of binder polymers, such as polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, polyacrylic acid, and polymers whose hydrogen is substituted by lithium (Li), sodium (Na) or calcium (Ca), or various copolymers.
[0059] Any conductive agent can be used without particular limitation as long as it has conductivity without causing adverse chemical changes in the battery, for example, conductive materials such as: carbon black, such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers, such as carbon fibers and metal fibers; conductive tubes, such as carbon nanotubes; metal powders, such as fluorocarbon powders, aluminum powders, and nickel powders; conductive whiskers, such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides, such as titanium oxide; or polyphenylene derivatives. The conductive agent may preferably be carbon black, and may more specifically be carbon black having an average particle size of several tens of nanometers.
[0060] The negative electrode active material layer may have a porosity of 10% to 20%, particularly 12% to 16%, and more particularly 13% to 15%. When the porosity satisfies the above range, the fast charging performance and high temperature durability of the battery can be improved. The porosity can be measured and calculated by the following method. Specifically, after measuring the specific surface area of the negative electrode by a nitrogen adsorption method using ASAP2000 (accelerated surface area and porosity determination system), the porosity is derived by using a BJT mapping program.
[0061] The edge surface of the negative electrode may have a thickness of 0.5 m 2 / g to 1.1m 2 / g, especially 0.5m 2 / g to 0.85m 2 / g, more particularly 0.5m 2 / g to 0.80m 2 / g, for example 0.70m 2 / g to 0.80m 2 / g specific surface area. When the specific surface area is less than 0.5m 2 / g, the fast charging performance of the battery may be reduced due to excessive increase in charge transfer resistance. On the contrary, when the specific surface area is greater than 1.1m 2 / g, the loss of lithium ions increases due to the excessive reactivity between the negative electrode and the electrolyte. Therefore, the durability of the battery decreases during high-temperature storage and high-temperature cycling. Thus, when the above range is met, a battery having a high level of fast charging performance and capable of maintaining high-temperature performance can be obtained.
[0062] In addition, when the negative electrode active material according to the embodiment of the present invention is used, the above range can be achieved. That is, by including a negative electrode having 1.0 m 2 / g to 1.9m 2 / g of edge surface specific surface area of the negative electrode active material of the above embodiment, and subjecting it to the subsequent negative electrode preparation process, the edge surface of the negative electrode may have 0.5m 2 / g to 1.1m 2 / g specific surface area.
[0063] The specific surface area of the edge face of the negative electrode can be measured by the following method. The sample is prepared by punching the prepared negative electrode into a size of 8 mm × 8 mm, and 60 samples are placed in a tube to measure the specific surface area by a nitrogen adsorption method. Then, the specific surface area of each of the defect edge face, the base face, and the prismatic edge face is obtained by density functional theory, and the sum of the specific surface areas of the defect edge face and the prismatic edge face is defined as the specific surface area of the edge face of the negative electrode.
[0064] <Secondary Battery>
[0065] The present invention provides a secondary battery including a positive electrode, a negative electrode, an electrolyte, and a separator, wherein the negative electrode is the same as the above-described negative electrode according to the embodiment, and the secondary battery may be a lithium secondary battery.
[0066] The secondary battery may be prepared according to a typical method known in the art. For example, the secondary battery may be prepared by disposing a separator between a positive electrode and a negative electrode and injecting an electrolyte in which a lithium salt is dissolved.
[0067] The positive electrode may include a positive electrode active material. A lithium transition metal oxide may be preferably used as the positive electrode active material, for example, the positive electrode active material may be a mixture of at least one selected from the group consisting of: Li x1 CoO 2 (0.5<x1<1.3), Li x2 NiO 2 (0.5<x2<1.3), Li x3 MnO 2 (0.5<x3<1.3), Li x4 Mn 2 O 4 (0.5<x4<1.3), Li x5 (Ni a1 Co b1 Mn c1 ) 2 (0.5<x5<1.3, 0<a1<1, 0<b1<1, 0<c1<1, a1+b1+c1=1), Li x6 Ni 1-y1 Co y1 O 2 (0.5<x6<1.3, 0<y1<1), Li x7 Co 1-y2 Mn y2 O 2 (0.5<x7<1.3, 0≤y2<1), Li x8 Ni 1-y3 Mn y3 O 2 (0.5<x8<1.3, 0≤y3<1), Li x9 (Ni a2 Co b2 Mn c2 ) 4 (0.5<x9<1.3, 0<a2<2, 0<b2<2, 0<c2<2, a2+b2+c2=2), Li x10 Mn 2-z1 Niz1 O 4 (0.5<x10<1.3, 0<z1<2), Li x11 Mn 2-z2 Co z2 O 4 (0.5<x11<1.3, 0<z2<2), Li x12 CoPO 4 (0.5<x12<1.3) and Li x13 FePO 4 (0.5<x13<1.3).
[0068] Typical porous polymer films, for example, porous polymer films prepared from polyolefin-based polymers such as ethylene homopolymers, propylene homopolymers, ethylene / butene copolymers, ethylene / hexene copolymers, and ethylene / methacrylate copolymers can be used alone or in the form of their laminates as separators included in the lithium secondary battery according to the present invention. In addition, typical porous nonwoven fabrics, such as nonwoven fabrics formed from high melting point glass fibers or polyethylene terephthalate fibers, can be used, but the separator is not limited thereto.
[0069] The electrolyte contained in the lithium secondary battery according to the present invention may be a mixed organic solvent of at least one selected from the group consisting of propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), γ-butyrolactone (GBL), fluoroethylene carbonate (FEC), methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, amyl acetate, methyl propionate, ethyl propionate and butyl propionate.
[0070] In addition, the electrolyte according to the present invention may further include a lithium salt, and the anion of the lithium salt may be at least one selected from the group consisting of: - , Cl - Br - ,I - 、NO 3 - 、N(CN) 2 - , BF 4 - , ClO 4 - PF 6 - ,(CF 3 ) 2 PF 4 -, (CF 3 ) 3 PF 3 - , (CF 3 ) 4 PF 2 - , (CF 3 ) 5 PF - , (CF 3 ) 6 P - , F 3 SO 3 - , CF 3 CF 2 SO 3 - , (CF 3 SO 2 ) 2 N - , (FSO 2 ) 2 N - , CF 3 CF 2 (CF 3 ) 2 CO - , (CF 3 SO 2 ) 2 CH - , (SF 5 ) 3 C - , (CF 3 SO 2 ) 3 C - , CF 3 (CF 2 ) 7 SO 3 - , CF 3 CO 2 - , CH 3 CO 2 - , SCN - and (CF 3 CF 2 SO 2 ) 2 N - .
[0071] The lithium secondary battery according to the present invention may be a cylindrical type secondary battery, a prismatic type secondary battery, and a pouch type secondary battery, but the lithium secondary battery is not limited thereto as long as it corresponds to a charging and discharging device.
[0072] Furthermore, the present invention provides a battery module including a lithium secondary battery as a unit cell; and a battery pack including the battery module.
[0073] The battery pack can be used as a power source for at least one medium and large device selected from the group consisting of power tools; electric vehicles including electric vehicles (EV), hybrid electric vehicles (HEV) and plug-in hybrid electric vehicles (PHEV); or power storage systems.
[0074] Hereinafter, embodiments of the present invention will be described in detail in a manner that can be easily implemented by a person skilled in the art to which the present invention belongs. However, the present invention can be embodied in many different forms and should not be construed as being limited to the embodiments set forth herein.
[0075] Example 1: Preparation of negative electrode active material
[0076] The average particle size (D 50 ) of 5 μm. Then, the pulverized needle coke was mixed with a pitch binder and then heat-treated at a temperature of 3,300° C. to prepare a pulverized needle coke having an average particle size (D 50 ) is artificial graphite in the form of secondary particles of 17 μm.
[0077] Thereafter, after 800 g of the pitch binder was mixed and stirred with 20 kg of artificial graphite, heat treatment was performed at 2,000° C. for 3 hours to form a carbon coating on the artificial graphite. The amount of the carbon coating in the negative electrode active material thus prepared was 4 wt %.
[0078] Example 2: Preparation of negative electrode active material
[0079] A negative electrode active material of Example 2 was prepared in the same manner as in Example 1 except that the pulverization pressure was set to 12 MPa.
[0080] Example 3: Preparation of negative electrode active material
[0081] A negative active material of Example 3 was prepared in the same manner as in Example 1, except that the heat treatment temperature applied to the pulverized needle coke was 3,100°C.
[0082] Example 4: Preparation of negative electrode active material
[0083] In addition to controlling the pulverization conditions to make the average particle size (D50 ) is 7 μm and the average particle size of the secondary particles of artificial graphite (D 50 ) was 15 μm, a negative electrode active material of Example 4 was prepared in the same manner as Example 1.
[0084] Comparative Example 1: Preparation of negative electrode active material
[0085] In addition to using the average particle size (D 50 A negative electrode active material of Comparative Example 1 was prepared in the same manner as in Example 1, except that natural graphite in the form of secondary particles with a diameter of 15 μm was used instead of the artificial graphite in Example 1.
[0086] Comparative Example 2: Preparation of negative electrode active material
[0087] A negative electrode active material of Comparative Example 2 was prepared in the same manner as in Example 1, except that mosaic coke was used instead of needle coke.
[0088] Comparative Example 3: Preparation of negative electrode active material
[0089] A negative electrode active material of Comparative Example 3 was prepared in the same manner as in Example 1 except that the pulverization pressure was set to 28 MPa.
[0090] Comparative Example 4: Preparation of negative electrode active material
[0091] A negative electrode active material of Comparative Example 4 was prepared in the same manner as in Example 1, except that the pulverization pressure was set to 36 MPa.
[0092] Comparative Example 5: Preparation of negative electrode active material
[0093] A negative electrode active material of Comparative Example 5 was prepared in the same manner as in Example 1, except that the heat treatment temperature applied to the pulverized needle coke was 2,800°C.
[0094] [Table 1]
[0095]
[0096] The specific surface area of the edge face of the negative electrode active material is measured by the following method. After obtaining the nitrogen adsorption specific surface area (BET) of the negative electrode active material by a nitrogen adsorption method, the defect edge face, the base face and the prismatic edge face are quantified by the nitrogen adsorption specific surface area by density functional theory. In this case, the sum of the specific surface areas of the defect edge face and the prismatic edge face is defined as the specific surface area of the edge face. The instrument used for measurement is ASAP2000 (Accelerated Surface Area and Porosity Measurement System). The average particle size (D 50 ) was measured by using laser diffraction.
[0097] Example 5: Preparation of negative electrode and battery
[0098] (1) Preparation of negative electrode
[0099] The negative electrode active material of Example 1, styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC) as a binder, and Super C65 as a conductive agent were added to distilled water in a weight ratio of 95.6:1:2.3:1.1 and mixed to prepare a negative electrode slurry having a solid content of 47% of the mixture. The negative electrode slurry was coated on a 20 μm thick copper collector and dried to prepare a preliminary electrode. In this case, the temperature of the circulating air was 80°C. Subsequently, the preliminary electrode was rolled under a pressure of Gap20, dried in a vacuum oven at 130°C for 10 hours, and then punched into 1.4875 cm 2 The negative electrode containing the negative electrode active material layer is prepared by using a coin cell size of 3.61 mAh / cm 2 .
[0100] (2) Preparation of batteries
[0101] Cut into pieces with an area of 1.7671cm 2 A lithium coin half-cell was prepared by providing a porous polyethylene separator between the positive electrode and the negative electrode prepared as described above, and injecting an electrolyte in which 1M LiPF was dissolved in a solvent in which ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed at a volume ratio of 1:4 and 0.5 wt% of vinylene carbonate was mixed. 6 .
[0102] Example 6: Preparation of negative electrode and battery
[0103] A negative electrode and a battery were prepared in the same manner as in Example 5, except that roll pressing was performed at a pressure of Gap10 during the preparation of the negative electrode.
[0104] Examples 7 to 9: Preparation of negative electrode and battery
[0105] A negative electrode and a battery were prepared in the same manner as in Example 5, except that each of the negative electrode active materials of Examples 2 to 4 was used instead of the negative electrode active material of Example 1.
[0106] Comparative Examples 6 to 10: Preparation of negative electrodes and secondary batteries
[0107] A negative electrode and a battery were prepared in the same manner as in Example 5, except that each of the negative electrode active materials of Comparative Examples 1 to 5 was used instead of the negative electrode active material of Example 1.
[0108] Comparative Example 11: Preparation of negative electrode and secondary battery
[0109] A negative electrode and a secondary battery were prepared in the same manner as in Example 5, except that the negative electrode active material of Comparative Example 3 was used instead of the negative electrode active material of Example 1 and roll pressing was performed at a pressure of Gap5 during preparation of the negative electrode.
[0110] [Table 2]
[0111]
[0112] The specific surface area of the edge face of the negative electrode is obtained by the following method. The sample is prepared by punching the negative electrode into a size of 8mm×8mm, and 60 samples are placed in a tube to measure the specific surface area by a nitrogen adsorption method. Then, the specific surface area of each of the defect edge face, the base face and the prismatic edge face is obtained by density functional theory, and the sum of the specific surface areas of the defect edge face and the prismatic edge face is defined as the specific surface area of the edge face of the negative electrode. The instrument used for measurement is ASAP2000 (Accelerated Surface Area and Porosity Measurement System). After measuring the specific surface area of the negative electrode by using the nitrogen adsorption method using ASAP2000 (Accelerated Surface Area and Porosity Measurement System), the porosity (%) of the negative electrode is deduced by using a BJT plotting program.
[0113] Experimental Example 1: Evaluation of initial efficiency and capacity retention after high-temperature storage
[0114] For each of the batteries of Examples 5 to 9 and Comparative Examples 6 to 11, the initial capacity and the capacity retention rate after high-temperature storage were evaluated.
[0115] Specifically, each battery was left to stand for 24 hours from the time of injection of the electrolyte, and then each battery was charged at a constant current rate of 0.1C, and then charged at a constant voltage (CV) at 0.005V. Thereafter, each battery was discharged to 1.5V at a rate of 0.1C. The initial efficiency was evaluated during the first charge and discharge cycle as described above. Thereafter, after two additional charge and discharge cycles, the battery at 90% state of charge (SOC) was stored in a reactor at 60°C for 4 weeks. Thereafter, the capacity retention rate was evaluated by checking the remaining capacity while discharging the battery at 0.1C.
[0116] Capacity retention rate (%) = (discharge capacity after high temperature storage / initial discharge capacity) × 100
[0117] [Table 3]
[0118]
[0119] Referring to Table 3, for the use of edge surface specific surface area of 0.5 m 2 / g to 1.1m2 / g range of negative electrode (Examples 5 to 9), it can be understood that the initial efficiency and the capacity retention rate during high temperature storage are higher than those of the battery using the negative electrode in which the edge surface specific surface area is not less than 0.5m 2 / g to 1.1m 2 / g range of negative electrodes (Comparative Examples 6 to 11).
Claims
1. A negative electrode active material comprising: a core comprising artificial graphite; and A carbon coating is disposed on the core, The edge surface of the negative electrode active material has a 1.0 m 2 / g to 1.9m 2 / g specific surface area, wherein the artificial graphite is a secondary particle in the form of an aggregate of primary particles, The specific surface area of the edge surface of the negative electrode active material is measured by the following method: After the nitrogen adsorption specific surface area of the negative electrode active material is obtained by the nitrogen adsorption method, the defect edge surface, the base surface and the prismatic edge surface are quantified by the nitrogen adsorption specific surface area through density functional theory, and the sum of the specific surface areas of the defect edge surface and the prismatic edge surface is considered to be the specific surface area of the edge surface of the negative electrode active material.
2. The negative electrode active material according to claim 1, wherein the primary particles have an average particle size D of 7 μm to 10 μm. 50 .
3. The negative electrode active material according to claim 1, wherein the artificial graphite has an average particle size D of 15 μm to 20 μm. 50 . The negative electrode active material according to claim 1 , wherein the carbon coating layer comprises soft carbon. 5 . The negative electrode active material according to claim 1 , wherein the carbon coating layer has a content of 3 wt % to 5 wt % in the negative electrode active material.
6. A method for preparing the negative electrode active material according to any one of claims 1 to 5, the method comprising: Prepare needle coke; crushing the needle coke at a pressure of 10 MPa to 20 MPa; After mixing the pulverized needle coke with a carbonaceous precursor, preparing a core by heat-treating at a temperature of 3,000° C. or more; as well as A carbon coating is formed on the core.
7. The method according to claim 6, wherein the needle coke has an average particle size D of 4 μm to 6 μm. 50 . The method according to claim 6 , wherein the heat treatment is performed for 8 to 12 hours.
9. A negative electrode comprising a current collector and a negative electrode active material layer disposed on the current collector, wherein the negative electrode active material layer comprises a negative electrode active material, wherein the negative electrode active material comprises a core comprising artificial graphite; and a carbon coating layer disposed on the core, The edge surface has a 0.5m 2 / g to 1.1m 2 / g specific surface area, wherein the artificial graphite is a secondary particle in the form of an aggregate of primary particles, The specific surface area of the edge surface of the negative electrode is measured by the following method: The samples were prepared by punching the prepared negative electrode into a size of 8 mm × 8 mm, and 60 samples were placed in a tube to measure the specific surface area by a nitrogen adsorption method, and then, the specific surface areas of the defect edge face, the base face and the prismatic edge face were obtained by density functional theory, and the sum of the specific surface areas of the defect edge face and the prismatic edge face was defined as the specific surface area of the edge face of the negative electrode. 10 . The negative electrode according to claim 9 , wherein the negative electrode active material is the negative electrode active material according to claim 1 . 11 . The negative electrode according to claim 9 , wherein the negative electrode active material layer has a porosity of 10% to 20%.
12. A secondary battery comprising: The negative electrode according to any one of claims 9 to 11; positive electrode; A separator disposed between the positive electrode and the negative electrode; and Electrolytes.