Electrode additives and coatings for minimizing cathode transition metal dissolution
By embedding or coating ceramic hydrofluoric acid scavengers in lithium-ion battery electrodes, the problem of transition metal ion release caused by HF release at high temperatures is solved, and the cycle stability and capacity retention rate of the battery are improved.
Patent Information
- Application Number
- CN202010978927.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-17
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-09-17
AI Technical Summary
Lithium-ion batteries generate HF due to the reaction between water and electrolyte at high temperatures, resulting in the release of transition metal ions, resulting in the loss of cathode active materials and capacity attenuation. The hydrolysis of existing ceramic materials at high temperatures leads to the release of HF.
Use ceramic hydrofluoric acid (HF) scavengers containing lithium (Li) or sodium (Na), such as Li2SiO3, LiAlO2, Na2SiO3, NaAlO2, etc., embedded or coated in the electrode active material to capture protons without forming releasable Hydrates to prevent transition metals from dissolving.
It effectively prevents the release of transition metal ions, improves the high-temperature cycle stability and capacity retention rate of lithium-ion batteries, and reduces the loss of electrode materials.
Smart Images

Figure CN112531138B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to an electrode comprising an electrode active material and a ceramic hydrofluoric acid (HF) scavenger and a method for manufacturing the electrode. Background Art
[0002] This section provides background information related to the present disclosure which is not necessarily prior art.
[0003] Electrochemical energy storage devices, such as lithium-ion batteries, can be used in a variety of products, including automotive products, such as start-stop systems (e.g., 12V start-stop systems), battery auxiliary systems ("μBAS"), hybrid electric vehicles ("HEV"), and electric vehicles ("EV"). A typical lithium-ion battery includes two electrodes, a separator, and an electrolyte. The lithium-ion battery may also include various terminals and packaging materials. In electrochemical cells, such as lithium-ion batteries, one of the two electrodes acts as a positive electrode or cathode and the other electrode acts as a negative electrode or anode. Conventional rechargeable lithium-ion batteries operate by reversibly transferring lithium ions back and forth between a negative electrode and a positive electrode. For example, lithium ions may move from a positive electrode to a negative electrode during charging of the battery and move in the opposite direction when the battery is discharged. A separator and / or an electrolyte may be disposed between the negative electrode and the positive electrode. The electrolyte is suitable for conducting lithium ions (or sodium ions in the case of a sodium-ion battery) between the electrodes and may be in solid form, liquid form, or a solid-liquid hybrid form as with the two electrodes. In the case of a solid-state battery comprising a solid electrolyte disposed between solid-state electrodes, the solid electrolyte physically separates the electrodes so that no separate separator is required.
[0004] Lithium-ion batteries generally include a cathode active material and a liquid electrolyte, wherein the cathode active material includes a transition metal (e.g., LiMnO 2 ), wherein the liquid electrolyte comprises, for example, LiPF in a carbonate-based organic solvent 6 However, especially at elevated temperatures from about 40°C to about 60°C, water in the electrolyte can react with LiPF 6 The reaction generates HF, LiF and H 3 PO 4 HF can react with the cathode active material to induce transition metal ions (such as Mn 2+ ) release. This transition metal ion release phenomenon is called transition metal dissolution. As a result of transition metal dissolution, the transition metal ions can precipitate back onto the cathode or migrate to and become deposited on the anode, resulting in loss of cathode active material, capacity decay, damage to the solid electrolyte interface layer and / or blocking lithium insertion into the negative electrode. Therefore, in order to remove HF, ceramic materials SiO 2and Al 2 O 3 Coating the isolation member. The SiO 2 and Al 2 O 3 React with HF to form hydrate SiF 4 ‧XH 2 O and AlF 3 ‧XH 2 O. However, at elevated temperatures, water molecules are released from the hydrate, promoting the 6 Therefore, there is a need for HF scavengers that do not release water at elevated temperatures. Summary of the invention
[0005] This section provides a general summary of the disclosure, and is not a comprehensive disclosure of its full scope or all of its features.
[0006] In various aspects, the technology of the present application provides an electrode comprising an electrode active material and a ceramic hydrofluoric acid (HF) scavenger, wherein the ceramic HF scavenger comprises M 2 SiO 3 、MA10 2 、M 2 O-Al 2 O 3 -SiO 2 or a combination thereof, wherein M is lithium (Li), sodium (Na) or a combination thereof.
[0007] In one aspect, the ceramic HF scavenger comprises Li 2 SiO 3 、LiAlO 2 , Li 2 O-Al 2 O 3 -SiO 2 or a combination thereof.
[0008] In one aspect, the ceramic HF scavenger comprises Na 2 SiO 3 、NaAlO 2 、Na 2 O-Al 2 O 3 -SiO 2 or a combination thereof.
[0009] In one aspect, the electrode active material is a cathode active material.
[0010] In one aspect, the cathode active material is a transition metal oxide or a transition metal polyanion.
[0011] In one aspect, the ceramic HF scavenger is embedded within the electrode active material.
[0012] In one aspect, the ceramic HF scavenger is in the form of a coating that coats at least a portion of the electrode active material.
[0013] In one aspect, the coating has a thickness of greater than or equal to about 1 micron to less than or equal to about 20 microns.
[0014] In one aspect, the electrode is an anode, the electrode active material is an anode active material, and the ceramic HF scavenger is in the form of a coating coating at least a portion of the anode active material.
[0015] In one aspect, the electrode is in a battery that cycles Li or Na ions and contains a liquid electrolyte capable of reacting with water to form HF.
[0016] In various aspects, the technology of the present application further provides a method for manufacturing an electrode for scavenging hydrofluoric acid (HF), the method comprising mixing a ceramic hydrofluoric acid (HF) scavenger powder into a solution comprising a binder dissolved in a solvent to form a slurry having a viscosity of greater than or equal to about 5000 cps to less than or equal to about 6000 cps, wherein the ceramic HF scavenger is 2 SiO 3 、MA1O 2 、M 2 O-Al 2 O 3 -SiO 2 or a combination thereof, wherein M is lithium (Li), sodium (Na) or a combination thereof; casting a continuous layer of the slurry onto a surface of an electrode; removing the solvent from the slurry to form a coating on the electrode, wherein the coating has a first porosity and removes HF.
[0017] In one aspect, the solution comprising the binder dissolved in the solvent comprises 6 wt% polyvinylidene fluoride (PVDF) dissolved in N-methyl-2-pyrrolidone (NMP).
[0018] In one aspect, the continuous layer of the slurry has a thickness of greater than or equal to about 1 micron to less than or equal to about 20 microns.
[0019] In one aspect, the slurry includes the ceramic HF scavenger powder at a concentration of greater than or equal to about 70 wt % to less than or equal to about 95 wt %.
[0020] In one aspect, the method further comprises calendering the coated electrode to create a second porosity in the coating, the second porosity being lower than the first porosity.
[0021] In various aspects, the technology of the present application also provides a method for manufacturing an electrode for scavenging hydrofluoric acid (HF), the method comprising mixing a powder of a ceramic hydrofluoric acid (HF) scavenger into a solution comprising a binder dissolved in a solvent to form a slurry having a viscosity of greater than or equal to about 200 cps to less than or equal to about 1000 cps, wherein the ceramic HF scavenger is 2 SiO 3 、MA10 2 、M 2 O-Al 2 O 3 -SiO 2 or a combination thereof, wherein M is lithium (Li), sodium (Na), or a combination thereof; mixing a cathode active material into the slurry until the slurry has a viscosity of greater than or equal to about 4000 cps to less than or equal to about 6000 cps; casting a continuous layer of the slurry onto a current collector; and removing the solvent from the slurry to produce the electrode for scavenging HF, the electrode having a first porosity, wherein the scavenging HF electrode comprises the ceramic HF scavenger embedded in the cathode active material.
[0022] In one aspect, the solution comprising the binder dissolved in the solvent comprises 6 wt% polyvinylidene fluoride (PVDF) dissolved in N-methyl-2-pyrrolidone (NMP).
[0023] In one aspect, the solution further comprises carbon black.
[0024] In one aspect, the slurry includes the cathode active material at a concentration of greater than or equal to about 70 wt % to less than or equal to about 95 wt %.
[0025] In one aspect, the method further comprises calendering the electrode to create a second porosity in the electrode, the second porosity being lower than the first porosity.
[0026] Further areas of applicability will become apparent from the description provided herein.The description and specific examples in this summary are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The drawings described herein are for illustrative purposes only of selected embodiments and not all possible implementations, and are not intended to limit the scope of the present disclosure.
[0028] Figure 1 is a diagrammatic representation of an electrochemical cell in accordance with various aspects of the technology of the present application.
[0029] Figure 2 is a diagram of an electrode that does not include a ceramic HF scavenger.
[0030] Figure 3 is a diagram of an electrode having a ceramic HF scavenger embedded within the electrode active material in accordance with various aspects of the present technology.
[0031] Figure 4A is an illustration of an electrode having an electrode active material with a coating comprising a ceramic HF scavenger in accordance with various aspects of the present technology.
[0032] Figure 4B The electrode active material is shown to be hidden by the coating. Figure 4A Schematic diagram of the electrodes.
[0033] Figure 4C After removing the layer or plane indicated by arrow 4C Figure 4A A view of an electrode that exposes previously hidden electrode active materials.
[0034] Figure 5 is a diagram of an exemplary battery including a cathode and an anode in accordance with various aspects of the present technology.
[0035] Figure 6 is a graph showing the performance of a button cell battery including an exemplary cathode having a ceramic HF scavenger embedded within the cathode active material.
[0036] Figure 7 is a graph showing the performance of a button cell battery including an exemplary cathode having a cathode active material coated with a composition including a ceramic HF scavenger.
[0037] Corresponding reference numerals indicate corresponding parts throughout the several views of the drawings. DETAILED DESCRIPTION
[0038] Exemplary embodiments are provided so that the present disclosure will be thorough and will fully convey its scope to those skilled in the art. Many specific details, such as examples of specific compositions, components, devices and methods, are set forth to provide a full understanding of the embodiments of the present disclosure. It will be apparent to those skilled in the art that specific details need not be used, that the exemplary embodiments may be embodied in many different forms, and that none of them should be considered to limit the scope of the present disclosure. In some exemplary embodiments, well-known methods, well-known device structures, and well-known technologies are not described in detail.
[0039] The terms used herein are intended only to describe specific exemplary embodiments and are not intended to be limiting. Unless the context clearly indicates otherwise, the singular forms "one", "a kind of" and "the" as used herein may be intended to also include plural forms. The terms "comprise", "include", "contain" and "have" are inclusive, thus illustrating the presence of the described features, elements, compositions, steps, integers, operations and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or their collections. Although the open term "comprise" should be understood as a non-limiting term for describing and claiming the various embodiments described herein, in some aspects, the term may be alternatively understood as a more restrictive and limited term, such as "consisting of" or "consisting essentially of". Thus, for any given embodiment of a narration composition, material, component, element, feature, integer, operation and / or process step, the present disclosure also particularly includes an embodiment consisting of or essentially consisting of such a composition, material, component, element, feature, integer, operation and / or process step. In the case of "consisting of," alternative embodiments exclude any additional compositions, materials, components, elements, features, integers, operations and / or process steps, while in the case of "consisting essentially of," any additional compositions, materials, components, elements, features, integers, operations and / or process steps that materially affect the basic and novel characteristics are excluded from such embodiments, but any compositions, materials, components, elements, features, integers, operations and / or process steps that do not materially affect the basic and novel characteristics may be included in the embodiments.
[0040] Any method steps, processes, and operations described herein are not to be construed as necessarily requiring their performance in the particular order discussed or illustrated, unless specifically identified as a certain order of performance. It is also to be understood that additional or alternative steps may be used unless otherwise stated.
[0041] When a part, element or layer is referred to as being "on," "engaged," "connected," or "coupled" to another element or layer, it may be directly on, engaged, connected, or coupled to another part, element or layer, or there may be intermediate elements or layers. Conversely, when an element is referred to as being directly on, "directly engaged," "directly connected," or "directly coupled" to another element or layer, there may be no intermediate elements or layers. Other words used to describe the relationship between elements should be interpreted in a similar manner (e.g., "between" vs. "directly between," "adjacent" vs. "directly adjacent," etc.). As used herein, the term "and / or" includes any and all combinations of one or more of the associated enumerated items.
[0042] Although the terms first, second, third, etc. can be used to describe various steps, elements, components, regions, layers and / or sections in this article, these steps, elements, components, regions, layers and / or sections should not be limited by these terms unless otherwise specified. These terms can only be used to distinguish a step, element, component, region, layer or section from another step, element, component, region, layer or section. Unless clearly stated in the context, terms such as "first", "second" and other numerical terms do not imply order or sequence when used in this article. Therefore, the first step, element, component, region, layer or section discussed below can be referred to as the second step, element, component, region, layer or section without departing from the teaching of exemplary embodiments.
[0043] For ease of description, spatial or temporal relative terms may be used herein, such as "before", "after", "inside", "outside", "below", "beneath", "lower", "upper", etc. to describe the relationship of one element or feature relative to other elements or features shown in the figures. Spatial or temporal relative terms may be intended to include different orientations of a device or system in use or operation in addition to the orientation shown in the figures.
[0044] Throughout this disclosure, numerical values represent approximate measured values or range limits to include slight deviations from given values and embodiments with roughly listed values and embodiments with exactly listed values.Except in the examples provided at the end of the detailed description part, all numerical values of parameters (such as amounts or conditions) in this specification (including the appended claims) should be understood to be modified by the term "about" in all cases, regardless of whether "about" actually appears before the numerical value. "About" means that the numerical value allows certain slight imprecision (some close to the exact value; roughly or reasonably close to the value; almost). If the imprecision provided by "about" is not understood in this art with this common meaning, then "about" used herein at least refers to the variation that may be caused by the common method of measuring and using such parameters.For example, "about" can include less than or equal to 5%, optionally less than or equal to 4%, optionally less than or equal to 3%, optionally less than or equal to 2%, optionally less than or equal to 1%, optionally less than or equal to 0.5% and optionally less than or equal to 0.1% variation in some aspects.
[0045] Additionally, disclosure of ranges includes disclosure of all values within the entire range and further subdivided ranges, including endpoints and subranges given within those ranges.
[0046] Example embodiments will now be described more fully with reference to the accompanying drawings.
[0047] The technology of the present application provides a ceramic hydrofluoric acid (HF) scavenger that can be embedded in an electrode or included in an electrode coating. The ceramic HF scavenger captures protons, such as from HF, without forming hydrates that can be released at elevated temperatures. As a result, transition metal dissolution is prevented, inhibited, relatively reduced or minimized. The technology of the present application also provides a method for preparing the ceramic HF scavenger and a method for manufacturing an electrode having the ceramic HF scavenger.
[0048] Figure 1 An exemplary schematic illustration of an electrochemical cell 20 (also referred to as a battery, which includes at least one electrochemical cell) that circulates lithium ions is shown in FIG. Unless otherwise specifically noted, the term "ion" used herein refers to lithium ions or sodium ions. For example, an electrochemical cell that circulates sodium ions has components similar to the lithium ion battery 20, but replaces lithium and lithium ions with sodium and sodium ions in the corresponding components. The battery 20 includes a negative electrode (i.e., an anode) 22, a positive electrode (i.e., a cathode) 24, and a separator 30 (e.g., a microporous polymer separator) disposed between the two electrodes 22 and 24. The electrolyte is present throughout the separator 30 and is optionally present in the negative electrode 22 and the positive electrode 24. The negative electrode current collector 32 may be located at or near the negative electrode 22, and the positive electrode current collector 34 may be located at or near the positive electrode 24. Although not shown, as known in the art, the negative electrode current collector 32 and the positive electrode current collector 34 may be coated on one or both sides. In some aspects, the current collectors 32, 34 may be coated with electrode active materials / electrode layers on both sides. The negative electrode current collector 32 and the positive electrode current collector 34 collect and move free electrons to and from the external circuit 40, respectively (as shown by the box arrows). For example, the interruptible external circuit 40 and the load device 42 can connect the negative electrode 22 (through the negative electrode current collector 32) and the positive electrode 24 (through the positive electrode current collector 34). The composite electrode may also include a binder, such as polyvinylidene fluoride (PVDF), and / or conductive carbon, such as carbon black or carbon nanotubes, which are dispersed throughout the material defining the negative electrode 22 and / or the positive electrode 24.
[0049] The battery 20 can generate an electric current (indicated by a box arrow) during discharge through a reversible electrochemical reaction that occurs when the external circuit 40 is closed (to connect the negative electrode 22 and the positive electrode 24) and the negative electrode 22 contains a relatively larger amount of lithium than the positive electrode. The chemical potential difference between the positive electrode 24 and the negative electrode 22 drives the electrons generated by the oxidation of the lithium embedded at the negative electrode 22 to move toward the positive electrode 24 through the external circuit 40. Lithium ions, which are also generated at the negative electrode, are simultaneously transferred to the positive electrode 24 through the electrolyte solution contained in the separator 30. The electrons flow through the external circuit 40 and the lithium ions migrate through the separator 30 containing the electrolyte solution to form embedded lithium at the positive electrode 24. The current through the external circuit 40 can be controlled and directed through the load device 42 until the embedded lithium in the negative electrode 22 is depleted and the capacity of the battery 20 is reduced.
[0050] The battery 20 can be charged or recharged at any time by connecting an external power source to the battery 20 to reverse the electrochemical reactions that occur during the battery discharge. The connection of the external power source to the battery 20 forces the non-spontaneous oxidation of the intercalated lithium at the positive electrode 24 to produce electrons and ions. The electrons, which flow back to the negative electrode 22 through the external circuit 40, and the ions, which are carried by the electrolyte solution through the separator 30 back to the negative electrode 22, recombine at the negative electrode 22 and replenish lithium for use during the next battery discharge event. In this way, each complete discharge event followed by a complete charge event is considered a cycle, in which ions circulate between the positive electrode 24 and the negative electrode 22.
[0051] The external power source that can be used to charge the battery 20 can vary depending on the size, construction, and specific end use of the battery 20. Some notable and exemplary external power sources include, but are not limited to, AC power sources such as AC wall outlets and motor vehicle alternators, and AC-DC converters and motor vehicle alternators connected to the AC grid through a wall outlet.
[0052] In many ion battery configurations, the negative electrode current collector 32, the negative electrode 22, the separator 30, the positive electrode 24, and the positive electrode current collector 34 are each prepared as relatively thin layers (e.g., thicknesses from a few microns to a fraction of a millimeter or less) and assembled in layers connected in an electrically parallel arrangement to provide suitable power and power packaging. In various other cases, the battery 20 may include electrodes 22, 24 connected in series. In addition, the separator 30 operates as an electrical insulator by being sandwiched between the negative electrode 22 and the positive electrode 24 to prevent physical contact and thus prevent the occurrence of a short circuit. In addition to providing a physical barrier between the electrodes 22, 24, the separator 30 also acts as a sponge containing an electrolyte solution in an open pore network during lithium ion cycling to facilitate the operation of the battery 20.
[0053] The battery 20 may include various other components known to those skilled in the art, although not shown here. For example, the battery 20 may include a casing, a gasket, an end cap, a tab, a battery terminal, and any other conventional components or materials that may be located within the battery 20, including between or around the negative electrode 22, the positive electrode 24, and / or the separator 30. As described above, the size and shape of the battery 20 may vary depending on the specific application for which it is designed. For example, battery-powered vehicles and handheld consumer electronic devices are two examples in which the battery 20 will most likely be designed to different sizes, capacities, and power output specifications. If the load device 42 requires, the battery 20 may also be connected in series or in parallel with other similar lithium-ion cells or batteries to produce greater voltage output, energy, and power.
[0054] Thus, the battery 20 can generate current to a load device 42 that is part of the external circuit 40. When the battery 20 is discharged, the load device 42 can be powered by the current through the external circuit 40. Although the electrical load device 42 can be any number of known electrically driven devices, some examples include electric motors for electric vehicles, laptop computers, tablet computers, mobile phones, and cordless power tools or appliances. The load device 42 can also be a power generation device that charges the battery 20 to store electrical energy.
[0055] Any suitable electrolyte capable of conducting lithium ions between the negative electrode 22 and the positive electrode 24, whether in solid form (e.g., in a solid-state electrochemical cell) or in solution, can be used in the lithium-ion battery 20. In certain aspects, the electrolyte solution can be a non-aqueous liquid electrolyte solution that includes a lithium salt dissolved in an organic solvent or an organic solvent mixture. Many conventional non-aqueous liquid electrolyte solutions can be used in the lithium-ion battery 20. A non-limiting list of lithium salts that can be dissolved in an organic solvent to form a non-aqueous liquid electrolyte solution includes LiPF 6 、LiFSi、LiClO 4 、LiAlCl 4 、LiI、LiBr、LiSCN、LiBF 4 、LiB(C 6 H 5 ) 4 、LiAsF 6 、LiCF 3 SO 3 、LiN(CF 3 SO 2 ) 2 、Li(CF 3 SO 2 ) 2N and combinations thereof. These and other similar lithium salts can be dissolved in various organic solvents, including but not limited to various alkyl carbonates, such as cyclic carbonates (ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC)), acyclic carbonates (dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC)), aliphatic carboxylic acid esters (methyl formate, methyl acetate, methyl propionate), γ-lactones (γ-butyrolactone, γ-valerolactone), chain structure ethers (1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane), cyclic ethers (tetrahydrofuran, 2-methyltetrahydrofuran), and mixtures thereof. However, as described above, some lithium salts react with water, i.e., hydrolyze, which results in the formation of hydrofluoric acid (HF). Such lithium salts include LiPF 6 、LiFSi、LiBF 4 、LiAsF 6 、LiCF 3 SO 3 、LiN(CF 3 SO 2 ) 2 、Li(CF 3 SO 2 ) 2 N, and combinations thereof. Thus, as discussed further below, a ceramic HF scavenger is included in or on the negative or positive electrode 22, 24.
[0056] Separator 30 works as both an electrical insulator and a mechanical support. In one embodiment, microporous polymer separator 30 comprises polyolefin. The polyolefin can be a homopolymer (derived from a single monomer component) or a heteropolymer (derived from more than one monomer component), which can be linear or branched. If the heteropolymer is derived from two monomer components, the polyolefin can present any copolymer chain arrangement, including those of block copolymers or random copolymers. Similarly, if the polyolefin is a heteropolymer derived from more than two monomer components, it can also be a block copolymer or a random copolymer. In some aspects, the polyolefin can be a blend of polyethylene (PE), polypropylene (PP) or PE and PP.
[0057] When the separator 30 is a microporous polymer separator, it can be a single layer or a multi-layer laminate, which can be manufactured by a dry process or a wet process. For example, in one embodiment, a single layer of a polyolefin can form the entire microporous polymer separator 30. In other aspects, the separator 30 can be a fiber membrane with a large number of pores extending between relative surfaces, and can have a thickness of, for example, less than 1 mm. As another example, multiple discrete layers of the same or different polyolefins can be assembled to form a microporous polymer separator 30. The polyolefin can be a homopolymer (derived from a single monomer component) or a heteropolymer (derived from more than one monomer component), which can be linear or branched. If the heteropolymer is derived from two monomer components, the polyolefin can present any copolymer chain arrangement, including those of block copolymers or random copolymers. Similarly, if the polyolefin is a heteropolymer derived from more than two monomer components, it can also be a block copolymer or a random copolymer. In some aspects, the polyolefin can be polyethylene (PE), polypropylene (PP), a blend of PE and PP, or a multilayer structured porous film of PE and / or PP. The microporous polymer separator 30 can also include other polymers besides the polyolefin, such as, but not limited to, polyethylene terephthalate (PET), polyvinylidene fluoride (PVDF) and / or polyamide. In addition, the porous separator 30 can be mixed with a ceramic material or its surface can be coated with a ceramic material. For example, the ceramic coating can include aluminum oxide (Al2O3). 2 O 3 ), silicon dioxide (SiO 2 ), titanium dioxide (TiO 2 ) or a combination thereof. Commercially available polyolefin porous membranes include CELGARD ® 2500 (single-layer polypropylene spacer) and CELGARD ® 2320 (three-layer polypropylene / polyethylene / polypropylene separator), both available from Celgard, LLC. The polyolefin layer and any other optional polymer layers may be further included in the microporous polymer separator 30 as fiber layers to help provide the microporous polymer separator 30 with appropriate structural and porosity properties. A variety of conventionally available polymers and commercial products are contemplated for use in forming the separator 30, as well as a number of manufacturing methods that can be used to prepare such a microporous polymer separator 30.
[0058] The negative electrode 22 can be formed of a lithium-based material capable of acting as a negative terminal of a lithium-ion battery. Thus, the negative electrode 22 may include an electrode active material and optionally another conductive material, and one or more polymer binder materials to structurally hold the lithium-based material together. In some variations, the negative electrode active material may include lithium, such as lithium metal. In some variations, the negative electrode 22 is a film or layer formed of lithium metal or a lithium alloy. In some variations, the negative electrode active material includes a carbon-based material such as graphite or silicon and / or a silicon-based alloy.
[0059] This negative electrode active material may optionally be mixed with a conductive material that provides an electron conduction path and / or at least one polymer binder material that improves the structural integrity of the negative electrode 22. As a non-limiting example, the negative electrode 22 may include an active material mixed with a binder material, the active material including lithium metal particles (e.g., lithium foil), the binder material being selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene propylene diene monomer (EPDM) rubber, carboxymethyl cellulose (CMC), nitrile rubber (NBR), lithium polyacrylate (LiPAA), sodium polyacrylate (NaPAA), sodium alginate, lithium alginate, and combinations thereof. Additional suitable conductive materials may include carbon-based materials or conductive polymers. As a non-limiting example, the carbon-based material may include KETCHEN TM Black, DENKA TM The negative electrode current collector 32 may be formed of copper (Cu) or any other suitable conductive material known to those skilled in the art.
[0060] The positive electrode 24 may be formed of a lithium-based or sodium-based active material that can fully undergo lithium / sodium intercalation and deintercalation or alloying and alloy degradation and simultaneously serve as a positive terminal of the battery 20. In various aspects, the positive electrode 24 includes a positive electrode active material in a spinel or layered oxide phase, the positive electrode active material including a lithium / sodium transition metal oxide or a lithium / sodium transition metal polyanion. Non-limiting examples of transition metal oxides include lithium cobalt oxide (LCO, LiCoO 2 ); Lithium manganese oxide (LMO, LiMn 2 O 4 );Li 1+x M 2-x O 2 , wherein 0≤x≤1 and M is a transition metal (e.g., Fe, Ni, Mn, Co, Ti, V, and combinations thereof); lithium nickel cobalt manganese oxide (NMC / NCM, LiNiCoMnO 2 ), including LiNi x Mny Co 1-x-y O 2 , where 0≤x≤1 and 0≤y≤1; lithium nickel cobalt aluminum oxide (NCA, LiNiCoAlO 2 ); lithium nickel manganese spinel (LNMO, LiNi 0.5 Mn 1.5 O 4 ); and LiNi x Mn 1-x O 2 , where 0≤x≤1. Non-limiting examples of transition metal polyanions include phosphates, such as LiMPO 4 , wherein M is Fe, Mn, Co, Ni, Zn, V or a combination thereof, LiV 2 (PO 4 ) 3 and Li 3 Fe 3 (PO 4 ) 4 ; Fluorophosphates, such as Li 2 MPO 4 F, wherein M is Fe, Mn, Co, Ni, Zn, V or a combination thereof, Li 2 FePO 4 F and Li 3 V 2 (PO 4 )F 3 ; Pyrophosphates, such as Li 2 MP 2 O 7 , wherein M is Fe, Mn, Co, Ni, Zn, V or a combination thereof; silicates such as Li 2 MSiO 4 , wherein M is Fe, Mn, Co, Ni, Zn, V or a combination thereof; carbonophosphates, such as Li 3 MCO 3 PO 4 , wherein M is Fe, Mn, Co, Ni, Zn, V or a combination thereof; sulfates such as Li 2 M(SO 4 ) 2 , wherein M is Fe, Mn, Co, Ni, Zn, V or a combination thereof; and borates such as LiMBO 3 , wherein M is Fe, Mn, Co, Ni, Zn, V or a combination thereof. For sodium-ion batteries, the lithium of the foregoing examples may be exchanged for sodium. In certain aspects, the positive solid-state electrode active particles may be coated (e.g., with Al 2 O 3) and / or the positive electrode active material may be doped (eg, with magnesium (Mg)).
[0061] The positive electrode active material can be a powder composition. The positive electrode active material can be mixed with an optional conductive material (e.g., conductive particles) and a polymer binder. The binder can keep the positive electrode active material together and provide ionic conductivity to the positive electrode 24. The polymer binder can include polyvinylidene fluoride (PVDF), poly (vinylidene chloride) (PVC), poly ((dichloro-1,4-phenylene) ethylene), carboxymethoxy cellulose (CMC), nitrile rubber (NBR), fluorinated polyurethane, fluorinated epoxide, fluorinated acrylic resin, copolymer of halogenated hydrocarbon polymers, epoxide, ethylene propylene diene terpolymer rubber (EPDM), hexafluoropropylene (HFP), ethylene acrylic acid copolymer (EAA), ethylene vinyl acetate copolymer (EVA), EAA / EVA copolymer, PVDF / HFP copolymer, polyvinylidene fluoride (PVDF), lithium polyacrylate (LiPAA), sodium polyacrylate (NaPAA), sodium alginate, lithium alginate or a combination thereof.
[0062] The positive electrode active material loading in the binder can be large, for example, greater than about 80 wt %. For example, the binder can be present at a level of greater than or equal to about 1 wt % to less than or equal to about 20 wt %, optionally greater than or equal to about 1 wt % to less than or equal to about 10 wt %, optionally greater than or equal to about 1 wt % to less than or equal to about 8 wt %, optionally greater than or equal to about 1 wt % to less than or equal to about 7 wt %, optionally greater than or equal to about 1 wt % to less than or equal to about 6 wt %, optionally greater than or equal to about 1 wt % to less than or equal to about 5 wt %, or optionally greater than or equal to about 1 wt % to less than or equal to about 3 wt %.
[0063] The conductive material may include graphite, other carbon-based materials, conductive metals, or conductive polymer particles. As a non-limiting example, the carbon-based material may include KETCHEN TM Black, DENKA TM Conductive metal particles may include particles of nickel, gold, silver, copper, aluminum, etc. Examples of conductive polymers include polyaniline, polythiophene, polyacetylene, polypyrrole, etc. In some aspects, a mixture of conductive materials may be used.
[0064] In certain variations, the positive electrode 24 includes the conductive material in an amount of less than or equal to about 15 wt %, optionally less than or equal to about 10 wt %, or optionally greater than or equal to about 0.5 wt % to less than or equal to about 8 wt %. Although the supplemental conductive materials may be described as powders, these materials lose their powder-like characteristics after being added to the electrode, wherein the associated particles of the supplemental conductive material become components of the resulting electrode structure.
[0065] As described above, some liquid electrolytes can react with water to form HF, especially at elevated temperatures. With a cooling system in place, the battery 20 is typically operated within a normal temperature of less than or equal to about 40° C., such as within a range of greater than or equal to about 25° C. to less than about 40° C. As used herein, "elevated temperature" is a temperature greater than or equal to about 40° C., such as within a range of greater than or equal to about 40° C. to less than or equal to about 60° C. As non-limiting examples, such liquid electrolytes that hydrolyze to form HF at elevated temperatures include LiPF 6 、LiFSi、LiBF 4 、LiAsF 6 、LiCF 3 SO 3 、LiN(CF 3 SO 2 ) 2 、Li(CF 3 SO 2 ) 2 As described above, HF can react with the positive electrode active material comprising at least one transition metal and cause the transition metal to dissolve. Although ceramic materials such as SiO 2 and Al 2 O 3 It has been used to scavenge HF and form hydrated SiF 4 ‧XH 2 O and AlF 3 ‧XH 2 O, but at elevated temperatures water molecules are released from the hydrate, which can lead to the formation of additional HF and cause transition metal dissolution. Therefore, the technology of the present application provides an electrode comprising an electrode active material and a ceramic HF scavenger, wherein the ceramic HF scavenger comprises M 2 SiO 3 、MA1O 2 、M 2 O-Al 2 O 3 -SiO 2 or a combination thereof, wherein M is Li, Na or a combination thereof. Thus, for a battery that cycles lithium ions, the ceramic HF scavenger includes Li 2 SiO3 、LiAlO 2 , Li 2 O-Al 2 O 3 -SiO 2 or a combination thereof, and for circulating sodium ion batteries, the ceramic HF scavenger includes Na 2 SiO 3 、NaAlO 2 、Na 2 O-Al 2 O 3 -SiO 2 or a combination thereof. The ceramic HF scavenger (or combination of scavengers) captures protons, for example from HF, without forming hydrates that can be released at elevated temperatures. More specifically, for example, Li 2 SiO 3 Reacts with HF to form LiHAl 2 O 4 , which contains no releasable water molecules. Similarly, LiAlO 2 Reacts with HF to form Li x H 4-x SiO 4 (0≤x<4), which does not contain releasable water molecules, and Li 2 O-Al 2 O 3 -SiO 2 Reacts with HF to form Li x H 7-x SiAlO 7 (0≤x<7), which does not contain releasable water molecules. The ceramic HF scavenger is embedded in the positive electrode, ie, within the positive electrode active material, or contained in the electrode coating of the positive electrode, or in certain embodiments discussed further below, contained in the electrode coating of the negative electrode.
[0066] The method for preparing the ceramic HF scavenger is described in U.S. Patent Application No. 16 / 445,610 filed on June 19, 2019, which is incorporated herein by reference in its entirety. The method includes mixing a precursor zeolite-based powder with a solution, such as an aqueous solution, containing one or more of lithium hydroxide (LiOH) and lithium chloride (LiCl) to form a second zeolite slurry. The weight ratio of the precursor zeolite to the solution can be greater than or equal to about 1 wt % to less than or equal to about 10 wt %, and the weight ratio of lithium hydroxide to the solution can be greater than or equal to about 0.5 wt % to less than or equal to about 5 wt %. The precursor zeolite-based powder may include one or more zeolite materials selected from zeolite A, zeolite X, zeolite Y, zeolite L, ZSM-5, zeolite beta, mordenite, ferrierite, and combinations thereof. For example, the precursor zeolite may include a zeolite material such as zeolite Y. Zeolite Y has a silicon-to-aluminum ratio of greater than or equal to about 1.5 to less than or equal to about 3 and a carbon content of about 453 m 2 In various aspects, the zeolite material can have an average particle size of less than or equal to about 5 microns, and in certain variations, optionally less than or equal to about 1 micron. In certain variations, the precursor zeolite powder further comprises greater than or equal to about 1 wt % to less than or equal to about 20 wt % of sodium oxide (NaO 2 ). When the mixture is exposed to a temperature of greater than or equal to about 30°C to less than or equal to about 100°C, and in some aspects optionally about 60°C, for a time of greater than or equal to about 6 hours to less than or equal to about 24 hours, and in some aspects optionally about 12 hours, the sodium oxide promotes lithium ion exchange between lithium hydroxide and / or lithium chloride in the solution and extra-framework cations and / or free ions in the zeolite material. In various cases, it is desirable that the zeolite material have a cumulative total concentration of sodium and hydrogen that is less than the concentration of lithium hydroxide and / or lithium chloride in the solution in order to drive ion exchange between lithium ions and sodium ions or protons. This lithium ion exchange results in the formation of one or more lithiated oxides, such as a powder comprising one or more lithiated oxides. In some variations, the lithiated oxide, such as Li 2 SiO 3 and LiAlO 2, resulting from this lithium ion exchange between the zeolite material and lithium hydroxide and / or lithium chloride. In various aspects, for example, the formed lithiated oxide powder can be washed to remove residual lithium hydroxide and / or lithium chloride. Residual lithium hydroxide and / or lithium chloride can undesirably increase the moisture content by reacting with carbon dioxide within the battery. The lithiated oxide can be washed with an aqueous liquid such as water. In certain variations, the water can be, for example, distilled water, and in certain aspects, optionally deionized water. In various aspects, the lithiated oxide powder can also be calcined at a temperature of greater than or equal to about 200° C. to less than or equal to about 400° C., and in certain aspects, optionally at about 400° C., for a time of greater than or equal to about 2 hours to less than or equal to about 6 hours, and in certain aspects, optionally for a time of about 2 hours, to remove any adsorbed water.
[0067] Figure 2 An exemplary electrode 50 is shown including a current collector 52 and an electrode active material 54 disposed on opposite sides of the current collector 52, the electrode active material 54 having a thickness T of greater than or equal to about 1 micron to less than or equal to about 100 microns. E , such as a thickness of about 1 micron, about 5 microns, about 10 microns, about 15 microns, about 20 microns, about 25 microns, about 30 microns, about 35 microns, about 40 microns, about 45 microns, about 50 microns, about 55 microns, about 60 microns, about 65 microns, about 70 microns, about 75 microns, about 80 microns, about 85 microns, about 90 microns, about 95 microns, or about 100 microns. Electrode 50 represents both a positive electrode (e.g., a cathode in an electrochemical cell) and a negative electrode (e.g., an anode in an electrochemical cell). Thus, the electrode active material can be a positive electrode active material or a negative electrode active material. Electrode 50 does not include a ceramic HF scavenger according to the technology of the present application.
[0068] Figure 3 An electrode 56 is shown comprising an electrode active material 58 and a ceramic HF scavenger, wherein the ceramic HF scavenger comprises M 2 SiO 3 、MA10 2 、M 2 O-Al 2 O 3 -SiO 2 or a combination thereof, wherein M is Li, Na, or a combination thereof. The electrode active material 58 is disposed on opposite sides of the current collector 60 and has a thickness T as described above. E. Electrode 56 can be a cathode or an anode. Thus, the electrode active material can be a positive electrode (i.e., a cathode in an electrochemical cell) active material or a negative electrode (i.e., an anode in an electrochemical cell) active material. In various embodiments, the electrode active material 58 is a cathode active material comprising a transition metal oxide or a transition metal polyanion as described above. The ceramic HF scavenger is embedded in the electrode active material 58. Therefore, when the electrode 56 is in an electrochemical cell or battery, the electrochemical cell or battery also includes a cathode (which can be the electrode 56 itself) comprising a transition metal oxide or a transition metal polyanion and an electrolyte capable of reacting with water to form HF, and when HF is formed in the electrolyte, the ceramic HF scavenger binds hydrogen atoms from the HF. The HF is then unable to react with the transition metal oxide or transition metal polyanion in the cathode, which results in preventing, inhibiting or minimizing transition metal dissolution at the cathode. When the ceramic HF scavenger is embedded in the cathode active material, the ceramic HF scavenger is included as an additive to the cathode active material during cathode manufacturing. Electrode active material 58 includes a ceramic HF scavenger at a concentration of greater than or equal to about 0.25 wt % to less than or equal to about 10 wt %, greater than or equal to about 0.5 wt % to less than or equal to about 7.5 wt %, or greater than or equal to about 1 wt % to less than or equal to about 5 wt %.
[0069] The technology of the present application also provides a method for manufacturing an electrode for removing HF, such as Figure 3 56, shown in the method of the electrode 56. The method includes dissolving the binder in a solvent to form a binder solution, the binder solution with a concentration of greater than or equal to about 2% by weight to less than or equal to about 10% by weight or greater than or equal to about 4% by weight to less than or equal to about 8% by weight, for example, with a concentration of about 2%, about 2.5%, about 3%, about 3.5%, about 4%, about 4.5%, about 5%, about 5.5%, about 6%, about 6.5%, about 7%, about 7.5%, about 8%, about 8.5%, about 9%, about 9.5% or about 10% by weight. The binder can be non-aqueous or aqueous. Non-limiting examples of non-aqueous binders include polyvinylidene fluoride (PVDF), poly (ethylene oxide) (PEO), poly (tetrafluoroethylene) (PTFE), copolymers of PTFE and perfluoro-3,6-dioxa-4-methyl-7-octene-sulfonic acid (e.g., NAFION ®Tetrafluoroethylene-perfluoro-3,6-dioxa-4-methyl-7-octene sulfonic acid copolymer) and combinations thereof, which can be dissolved in solvents, such as N-methyl-2-pyrrolidone (NMP), tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), methyl ethyl ketone (MEK), N,N-dimethylacetamide (DMAc), acetone, acetonitrile (MeCN) and combinations thereof as non-limiting examples. Non-limiting examples of aqueous binders include sodium carboxymethyl, styrene-butadiene rubber (SBR), sodium alginate, lithium polyacrylate (LiPAA), sodium carboxymethyl cellulose (NaCMC) and combinations thereof, which can be dissolved in solvents, such as water (including distilled water and deionized water), tert-butyl alcohol, propanol, ethanol, methanol, ammonia, acetic acid and combinations thereof as non-limiting examples.
[0070] The method further comprises mixing a powder of a ceramic HF scavenger and optional additional additives into the binder solution comprising a binder dissolved in a solvent to form a slurry having a first viscosity of greater than or equal to about 100 cps to less than or equal to about 1500 cps, greater than or equal to about 200 cps to less than or equal to about 1200 cps, or greater than or equal to about 300 cps to less than or equal to about 1000 cps, such as about 100 cps, about 200 cps, about 300 cps, about 400 cps, about 500 cps, about 600 cps, about 700 cps, about 800 cps, about 900 cps, about 1000 cps, about 1100 cps, about 1200 cps, about 1300 cps, about 1400 cps, or about 1500 cps. The ceramic HF scavenger comprises M 2 SiO 3 、MA1O 2 、M 2 O-Al 2 O 3 -SiO 2 or a combination thereof, wherein M is Li, Na or a combination thereof, as described above. In various embodiments, a ceramic HF scavenger is added to the binder solution until the first viscosity is reached. Optional additional additives include, for example, conductive carbon, such as carbon black, acetylene black or carbon nanotubes.
[0071] The method then includes mixing the electrode active material into the slurry until the slurry has a new second viscosity of greater than or equal to about 2000 cps to less than or equal to about 8000 cps, greater than or equal to about 3000 cps to less than or equal to about 7000 cps, or greater than or equal to about 4000 cps to less than or equal to about 6000 cps, for example, about 2000 cps, about 2500 cps, about 3000 cps, about 3500 cps, about 4000 cps, about 4500 cps, about 5000 cps, about 5500 cps, about 6000 cps, about 6500 cps, about 7000 cps, about 7500 cps, or about 8000 cps. In various embodiments, the electrode active material is added to the slurry at a concentration of greater than or equal to about 70% by weight to less than or equal to about 95% by weight, greater than or equal to about 80% by weight to less than or equal to about 92% by weight, or greater than or equal to about 85% by weight to less than or equal to about 90% by weight, such as at a concentration of about 70%, about 75%, about 80%, about 85%, about 90%, about 91%, about 92%, about 93%, about 94%, or about 95%. The electrode active material can be a cathode active material or an anode active material comprising a transition metal oxide or a transition metal polyanion.
[0072] Next, the method includes forming the slurry with a thickness of T E A continuous layer of (as described above) is cast onto a current collector. Casting may be performed using any method known in the art, such as by doctor blading, spin casting or pipetting, as non-limiting examples.
[0073] The method then includes removing the solvent from the slurry to produce an HF-scavenging electrode. The removal is performed by at least one of: maintaining in an oven at a temperature of greater than or equal to about 30°C to less than or equal to about 80°C or greater than or equal to about 60°C to less than or equal to about 75°C (e.g., a temperature of about 30°C, about 35°C, about 40°C, about 45°C, about 50°C, about 55°C, about 60°C, about 65°C, about 70°C, about 75°C, or about 80°C) or applying negative pressure (i.e., vacuum). The removal is performed for a period of greater than or equal to about 1 hour to less than or equal to about 24 hours, such as about 1 hour, about 2 hours, about 3 hours, about 4 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours, about 9 hours, about 10 hours, about 11 hours, about 12 hours, about 13 hours, about 14 hours, about 15 hours, about 16 hours, about 17 hours, about 18 hours, about 19 hours, about 20 hours, about 21 hours, about 22 hours, about 23 hours, or about 24 hours. The resulting electrode has an electrode active material having a first porosity, and the electrode active material includes a ceramic HF scavenger embedded therein. The first porosity is greater than about 50% and less than or equal to about 75%, or greater than about 50% and less than or equal to about 65%.
[0074] In some embodiments, the method further comprises calendaring the electrode between the flat surface and the roller or between two rollers to produce a second porosity in the electrode. The second porosity is lower than the first porosity and may be greater than or equal to about 20% to less than or equal to about 50%, or greater than or equal to about 35% to less than or equal to about 50%. The calendaring applies a continuous pressure of greater than or equal to about 1 Pa to less than or equal to about 10 MPa to the electrode.
[0075] The method may further comprise disposing the electrode in an electrochemical cell, for example as a cathode when it comprises a cathode active material. The electrochemical cell may further comprise an electrolyte capable of reacting with water to form HF.
[0076] The technology of the present application also provides an electrode having a coating comprising a ceramic HF scavenger. Figure 4A An electrode 70 is shown, Figure 4B An electrode 70 is shown with a buried interior portion (electrode active material) indicated by a dashed line, and Figure 4C After removing the layer or plane indicated by arrow 4C Figure 4A 70, which exposes the interior portion. Electrode 70 includes electrode active material 72 disposed on opposite sides of current collector 74. Electrode active material 72 has a thickness T as described above. Eand may be a cathode active material or an anode active material including a transition metal oxide or a transition metal polyanion. The electrode 70 further includes a ceramic HF scavenger in the form of a coating 76 coating at least a portion of the electrode active material 72, wherein the ceramic HF scavenger includes M 2 SiO 3 、MA10 2 、M 2 O-Al 2 O 3 -SiO 2 or a combination thereof, wherein M is Li, Na, or a combination thereof (as described above). In other words, the electrode 70 includes a coating 76 comprising a ceramic HF scavenger, wherein the coating 76 coats or covers at least a portion of the electrode active material 72. With respect to "at least a portion of the electrode active material", it is meant that the coating 76 completely coats the electrode active material 72 on both sides of the current collector 74, the coating 76 only completely coats the electrode active material 72 on one side of the current collector 74 (and the electrode active material on the other side of the current collector is not coated), or the coating 76 at least partially coats the electrode active material 72 on both sides of the current collector 74, so that the coating 76 can be continuous or discontinuous independently on either side of the current collector 74.
[0077] The coating 76 has a thickness T C , which is greater than or equal to about 1 micron to less than or equal to about 20 microns, greater than or equal to about 2 microns to less than or equal to about 15 microns, or greater than or equal to about 5 microns to less than or equal to about 10 microns, for example, a thickness of about 1 micron, about 2 microns, about 3 microns, about 4 microns, about 5 microns, about 6 microns, about 7 microns, about 8 microns, about 9 microns, about 10 microns, about 11 microns, about 12 microns, about 13 microns, about 14 microns, about 15 microns, about 16 microns, about 17 microns, about 18 microns, about 19 microns or about 20 microns. Coating 76 includes a ceramic HF scavenger at a concentration of greater than or equal to about 70 wt % to less than or equal to about 95 wt %, greater than or equal to about 75 wt % to less than or equal to about 92 wt %, or greater than or equal to about 80 wt % to less than or equal to about 90 wt %, for example, at a concentration of about 70 wt %, about 75 wt %, about 80 wt %, about 85 wt %, about 90 wt %, about 91 wt %, about 92 wt %, about 93 wt %, about 94 wt %, or about 95 wt %.
[0078] In some embodiments, electrode 70 is a cathode (i.e., the electrode active material is a transition metal oxide or transition metal polyanion) that is located within an electrochemical cell or battery that also includes an electrolyte capable of reacting with water to form HF. When HF is formed within the electrolyte, the ceramic HF scavenger scavenge and binds hydrogen atoms from the HF. The HF is then rendered incapable of reacting with the transition metal oxide or transition metal polyanion in the cathode, which results in preventing, inhibiting, or minimizing transition metal dissolution at the cathode.
[0079] In other embodiments, the electrode 70 is an anode (i.e., the electrode active material is an anode active material) that is located within an electrochemical cell or battery that also includes a cathode and an electrolyte capable of reacting with water to form HF. As HF is formed within the electrolyte, the ceramic HF scavenger scavenge and binds hydrogen atoms from the HF. The HF is then rendered incapable of reacting with the transition metal oxide or transition metal polyanion in the cathode, which results in preventing, inhibiting, or minimizing transition metal dissolution at the cathode.
[0080] Figure 5 Yet another embodiment is illustrated in , which shows a portion of a battery 80 that includes alternating anodes 82 and cathodes 84 separated by separators 86, with the anodes 82 located at opposite ends. Each anode 82 includes an anode current collector 88 and an anode active material 90 disposed on opposite sides of the current collector. Each cathode 84 includes a cathode current collector 92 and an anode active material 94 disposed on opposite sides of the current collector. Each cathode 84 includes a cathode active material having at least one of the following: a ceramic HF scavenger according to the technology of the present application embedded therein or a coating containing the ceramic HF scavenger. With respect to the anodes 82, only the anode active material 90 at the opposite end and on the side of the anode current collector 88 that does not face the cathode 84 includes at least one of the following: a ceramic HF scavenger according to the technology of the present application embedded therein or a coating containing the ceramic HF scavenger.
[0081] The technology of the present application also provides a method for manufacturing an electrode for removing HF, such as Figures 4A-4C70, shown in the method of the electrode 70,. The method includes dissolving the binder in a solvent to form a binder solution, the binder solution with a concentration of greater than or equal to about 2% by weight to less than or equal to about 10% by weight or greater than or equal to about 4% by weight to less than or equal to about 8% by weight, for example, at a concentration of about 2%, about 2.5%, about 3%, about 3.5%, about 4%, about 4.5%, about 5%, about 5.5%, about 6%, about 6.5%, about 7%, about 7.5%, about 8%, about 8.5%, about 9%, about 9.5% or about 10% by weight. The binder can be non-aqueous or aqueous. Non-limiting examples of non-aqueous binders include polyvinylidene fluoride (PVDF), poly (ethylene oxide) (PEO), poly (tetrafluoroethylene) (PTFE), copolymers of PTFE and perfluoro-3,6-dioxa-4-methyl-7-octene-sulfonic acid (e.g., NAFION ® Tetrafluoroethylene-perfluoro-3,6-dioxa-4-methyl-7-octene sulfonic acid copolymer) and combinations thereof, which can be dissolved in solvents, such as N-methyl-2-pyrrolidone (NMP), tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), methyl ethyl ketone (MEK), N,N-dimethylacetamide (DMAc), acetone, acetonitrile (MeCN) and combinations thereof as non-limiting examples. Non-limiting examples of aqueous binders include sodium carboxymethyl, styrene-butadiene rubber (SBR), sodium alginate, lithium polyacrylate (LiPAA), sodium carboxymethyl cellulose (NaCMC) and combinations thereof, which can be dissolved in solvents, such as water (including distilled water and deionized water), tert-butyl alcohol, propanol, ethanol, methanol, ammonia, acetic acid and combinations thereof as non-limiting examples.
[0082] The method further includes mixing a powder of a ceramic HF scavenger into the binder solution comprising a binder dissolved in a solvent to form a slurry having a viscosity of greater than or equal to about 3000 cps to less than or equal to about 8000 cps, greater than or equal to about 4000 cps to less than or equal to about 7000 cps, or greater than or equal to about 5000 cps to less than or equal to about 6000 cps, for example, a viscosity of about 3000 cps, about 3500 cps, about 4000 cps, about 4500 cps, about 5000 cps, about 5500 cps, about 6000 cps, about 6500 cps, about 7000 cps, about 7500 cps, or about 8000 cps. The concentration of the ceramic HF scavenger in the slurry is greater than or equal to about 70 wt % to less than or equal to about 95 wt %, greater than or equal to about 75 wt % to less than or equal to about 92 wt %, or greater than or equal to about 80 wt % to less than or equal to about 90 wt %, such as about 70 wt %, about 75 wt %, about 80 wt %, about 85 wt %, about 90 wt %, about 91 wt %, about 92 wt %, about 93 wt %, about 94 wt % or about 95 wt %. The amount of the ceramic HF scavenger can be adjusted to achieve a suitable viscosity.
[0083] Next, the method includes forming the slurry with a thickness of T C A continuous or discontinuous layer (as described above) is cast onto the surface of the electrode active material. Casting can be performed using any method known in the art, such as by doctor blading, spin casting or pipetting as non-limiting examples.
[0084] The method then includes removing the solvent from the slurry to produce an HF-scavenging electrode. The removal is performed by at least one of: maintaining in an oven at a temperature of greater than or equal to about 30°C to less than or equal to about 80°C or greater than or equal to about 60°C to less than or equal to about 75°C (e.g., a temperature of about 30°C, about 35°C, about 40°C, about 45°C, about 50°C, about 55°C, about 60°C, about 65°C, about 70°C, about 75°C, or about 80°C) or applying negative pressure (i.e., vacuum). The removal is performed for a period of greater than or equal to about 1 hour to less than or equal to about 24 hours, such as about 1 hour, about 2 hours, about 3 hours, about 4 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours, about 9 hours, about 10 hours, about 11 hours, about 12 hours, about 13 hours, about 14 hours, about 15 hours, about 16 hours, about 17 hours, about 18 hours, about 19 hours, about 20 hours, about 21 hours, about 22 hours, about 23 hours, or about 24 hours. The resulting electrode has a coating having a first porosity and including a ceramic HF scavenger embedded therein. The first porosity is greater than about 50% and less than or equal to about 75%, or greater than about 50% and less than or equal to about 65%.
[0085] In some embodiments, the method further comprises calendaring the electrode between the flat surface and the roller or between two rollers to produce a second porosity in the coating. The second porosity is lower than the first porosity and may be greater than or equal to about 20% to less than or equal to about 50%, or greater than or equal to about 35% to less than or equal to about 50%. The calendaring applies a continuous pressure of greater than or equal to about 1 Pa to less than or equal to about 10 MPa to the electrode.
[0086] Therefore, the technology of the present application provides a cathode comprising a cathode active material, wherein the cathode active material comprises a transition metal oxide or a transition metal polyanion, wherein the ceramic HF scavenger is at least one of the following: embedded in the cathode active material or contained in a coating coating the cathode active material. The technology of the present application also provides an anode comprising an anode active material, wherein the ceramic HF scavenger is at least one of the following: embedded in the anode active material or contained in a coating coating the anode active material. Methods for making these electrodes are also provided above. The technology of the present application also provides an electrochemical cell and a storage battery for circulating lithium ions or sodium ions, which include any combination of the cathode and anode, and an electrolyte capable of reacting with water to form HF. As non-limiting examples, the electrochemical cells and batteries may include a cathode with at least one ceramic HF scavenger embedded in a cathode active material or contained in a coating coating the cathode active material and an anode without a ceramic HF scavenger; a cathode with at least one ceramic HF scavenger embedded in a cathode active material or contained in a coating coating the cathode active material and an anode with at least one ceramic HF scavenger embedded in an anode active material or contained in a coating coating the anode active material; or a cathode without a ceramic HF scavenger and an anode with at least one ceramic HF scavenger embedded in an anode active material or contained in a coating coating the anode active material.
[0087]
[00136] Embodiments of the present application's technology are further illustrated by the following non-limiting examples.
[0088] Example 1
[0089] According to the method of the present application, a cathode active material (Li 2 MnO 4 ) 2 SiO 3 The cathode comprises 4-5 wt% polyvinylidene fluoride (PVDF), 4-5 wt% carbon black (C65), 1-5 wt% Li 2 SiO 3 and 85-90 wt% Li 2 MnO 4A control cathode was prepared in the same manner but without the inclusion of Li 2 SiO 3 The cathode was incorporated into a button cell with 1 M LiPF in ethylene carbonate (EC) / diethyl carbonate (DEC). 6 The button cells were subjected to two C / 10 formation cycles and then long term testing at C / 3 at an elevated temperature of about 50°C.
[0090] The results are shown in Figure 6 , the figure is a graph having a first y-axis 100 representing capacity retention (0%-150%), a second y-axis 102 representing coulombic efficiency (50%-110%), and an x-axis 104 representing cycle number (0-65 cycles). For capacity retention, triangles 106 form a curve for a coin cell including a control cathode, and squares 108 form a curve for a coin cell including a Li+ cathode embedded in the cathode active material. 2 SiO 3 These results show that the cathode active material includes Li embedded in the cathode active material. 2 SiO 3 The coin cell including the cathode has improved capacity retention relative to the coin cell including the control cathode. For the coulombic efficiency, the triangle 110 forms a curve for the coin cell including the control cathode, and the square 112 forms a curve for the coin cell including the cathode having Li embedded in the cathode active material. 2 SiO 3 These results show that when Li 2 SiO 3 There is no loss in Coulombic efficiency when included in the cathode active material. 2 SiO 3 Improved high temperature cycle stability of button batteries.
[0091] Example 2
[0092] According to the method of the present application, a cathode is manufactured, which comprises a 2 SiO 3 The coating comprises 10-20 wt % polyvinylidene fluoride (PVDF) and 80-90 wt % Li 2 SiO 3 A control cathode was prepared in the same manner, but without the coating. The cathode was incorporated into a button cell with 1 M LiPF in ethylene carbonate (EC) / diethyl carbonate (DEC). 6 The button cells were subjected to two C / 10 formation cycles and then long term testing at C / 3 at an elevated temperature of about 50°C.
[0093] The results are shown in Figure 7 , the figure is a graph having a first y-axis 120 representing capacity retention (0%-150%), a second y-axis 122 representing coulombic efficiency (50%-110%), and an x-axis 124 representing the number of cycles (0-125 cycles). For capacity retention, squares 126 form a curve for a button cell including a control cathode, and triangles 128 form a curve for a button cell including a Li 2 SiO 3 These results show that the cathode with Li 2 SiO 3 The coin cells with the coated cathodes have improved capacity retention relative to the coin cells including the control cathodes. For coulombic efficiency, squares 130 form a curve for the coin cells including the control cathodes, and triangles 132 form a curve for the coin cells including the Li 2 SiO 3 curves for coin cells with coated cathodes. These results show that when Li 2 SiO 3 There is no loss in Coulombic efficiency when coating the cathode active material. 2 SiO 3 Improved high temperature cycle stability of button batteries.
[0094] The present application may include the following embodiments.
[0095] 1. An electrode comprising:
[0096] electrode active materials; and
[0097] Ceramic hydrofluoric acid (HF) scavenger, wherein the ceramic HF scavenger comprises M 2 SiO 3 、MA1O 2 、M 2 O-Al 2 O 3 -SiO 2 or a combination thereof, wherein M is lithium (Li), sodium (Na) or a combination thereof.
[0098] 2. An electrode according to embodiment 1, wherein the ceramic hydrofluoric acid (HF) scavenger comprises Li 2 SiO 3 、LiAlO 2 , Li 2 O-Al 2 O 3 -SiO 2 or a combination thereof.
[0099] 3. An electrode according to embodiment 1, wherein the ceramic hydrofluoric acid (HF) scavenger comprises Na 2 SiO 3 、NaAlO 2 、Na 2 O-Al 2 O 3 -SiO 2 or a combination thereof.
[0100] 4. An electrode according to embodiment 1, wherein the electrode active material is a cathode active material.
[0101] 5. An electrode according to embodiment 4, wherein the cathode active material is a transition metal oxide or a transition metal polyanion.
[0102] 6. An electrode according to embodiment 1, wherein the ceramic hydrofluoric acid (HF) scavenger is embedded in the electrode active material.
[0103] 7. An electrode according to embodiment 1, wherein the ceramic hydrofluoric acid (HF) scavenger is in the form of a coating coating at least a portion of the electrode active material.
[0104] 8. An electrode according to embodiment 7, wherein the coating has a thickness of greater than or equal to about 1 micron to less than or equal to about 20 microns.
[0105] 9. The electrode according to embodiment 1, wherein the electrode is an anode, the electrode active material is an anode active material, and the ceramic hydrofluoric acid (HF) scavenger is in the form of a coating coating at least a portion of the anode active material.
[0106] 10. An electrode according to embodiment 1, wherein the electrode is located in a battery that circulates lithium (Li) or sodium (Na) ions and contains a liquid electrolyte that can react with water to form hydrofluoric acid (HF).
[0107] 11. A method of making an electrode for scavenging hydrofluoric acid (HF), the method comprising:
[0108] A ceramic hydrofluoric acid (HF) scavenger powder is mixed into a solution comprising a binder dissolved in a solvent to form a slurry having a viscosity of greater than or equal to about 5000 cps to less than or equal to about 6000 cps. 2 SiO 3 、MA10 2 、M 2 O-Al 2 O 3 -SiO 2or a combination thereof, wherein M is lithium (Li), sodium (Na) or a combination thereof;
[0109] casting a continuous layer of the slurry onto a surface of an electrode;
[0110] The solvent is removed from the slurry to form a coating on the electrode, wherein the coating has a first porosity and scavenges hydrofluoric acid (HF).
[0111] 12. The method according to embodiment 11, wherein the solution comprising the binder dissolved in the solvent comprises 6 wt% polyvinylidene fluoride (PVDF) dissolved in N-methyl-2-pyrrolidone (NMP).
[0112] 13. The method of embodiment 11, wherein the continuous layer of the slurry has a thickness of greater than or equal to about 1 micron to less than or equal to about 20 microns.
[0113] 14. The method of embodiment 11, wherein the slurry comprises the ceramic hydrofluoric acid (HF) scavenger powder at a concentration of greater than or equal to about 70 wt % to less than or equal to about 95 wt %.
[0114] 15. The method according to embodiment 11 further comprises:
[0115] The coated electrode is calendered to create a second porosity in the coating, the second porosity being lower than the first porosity.
[0116] 16. A method of making an electrode for scavenging hydrofluoric acid (HF), the method comprising:
[0117] A powder of a ceramic hydrofluoric acid (HF) scavenger is mixed into a solution comprising a binder dissolved in a solvent to form a slurry having a viscosity of greater than or equal to about 200 cps and less than or equal to about 1000 cps. 2 SiO 3 、MA1O 2 、M 2 O-Al 2 O 3 -SiO 2 or a combination thereof, wherein M is lithium (Li), sodium (Na) or a combination thereof;
[0118] mixing a cathode active material into the slurry until the slurry has a viscosity of greater than or equal to about 4000 cps to less than or equal to about 6000 cps;
[0119] casting a continuous layer of the slurry onto a current collector; and
[0120] removing the solvent from the slurry to produce the electrode scavenged with hydrofluoric acid (HF), the electrode having a first porosity,
[0121] The hydrofluoric acid (HF) scavenging electrode comprises the ceramic hydrofluoric acid (HF) scavenger embedded in the cathode active material.
[0122] 17. The method according to embodiment 16, wherein the solution comprising the binder dissolved in the solvent comprises 6 wt% polyvinylidene fluoride (PVDF) dissolved in N-methyl-2-pyrrolidone (NMP).
[0123] 18. The method of embodiment 16, wherein the solution further comprises carbon black.
[0124] 19. The method of embodiment 16, wherein the slurry comprises the cathode active material at a concentration of greater than or equal to about 70 wt % to less than or equal to about 95 wt %.
[0125] 20. The method according to embodiment 16, further comprising:
[0126] The electrode is calendered to create a second porosity in the electrode, the second porosity being lower than the first porosity.
[0127] The above description of the embodiments has been provided for the purpose of illustration and description. It is not intended to be exhaustive or to limit the present disclosure. Individual elements or features of a particular embodiment are generally not limited to that particular embodiment, but are interchangeable and can be used in selected embodiments when applicable, even if not explicitly shown or described. It can also be changed in many ways. Such changes are not considered to depart from the present disclosure, and all such modifications are intended to be included within the scope of the present disclosure.
Claims
1. An electrode comprising: An electrode active material, wherein the electrode active material is a cathode active material and the cathode active material comprises LiMn2O4; and A ceramic HF scavenger, wherein the ceramic HF scavenger comprises Li2SiO3, LiAlO2, Li2O-Al2O3-SiO2 or a combination thereof; wherein the ceramic HF scavenger is embedded in the electrode active material, The electrode is manufactured by the following method, wherein the method comprises: mixing a powder of a ceramic HF scavenger into a solution comprising a binder dissolved in a solvent to form a slurry having a viscosity greater than or equal to 200 cps and less than or equal to 1000 cps; mixing a cathode active material into the slurry until the slurry has a viscosity of greater than or equal to 4000 cps and less than or equal to 6000 cps; casting a continuous layer of the slurry onto a current collector; and The solvent is removed from the slurry to produce the electrode.
2. The electrode of claim 1, wherein the electrode is in a battery that cycles lithium ions and contains a liquid electrolyte that can react with water to form HF.
3. The electrode of claim 1, wherein the solution comprising the binder dissolved in the solvent comprises 6 wt% polyvinylidene fluoride dissolved in N-methyl-2-pyrrolidone. The electrode according to claim 1 , wherein the solution further comprises carbon black. 5 . The electrode according to claim 1 , wherein the slurry comprises the cathode active material at a concentration of greater than or equal to 70 wt % to less than or equal to 95 wt %.
6. A method of manufacturing an electrode for scavenging HF, the method comprising: mixing a powder of a ceramic HF scavenger including Li2SiO3, LiAlO2, Li2O-Al2O3-SiO2 or a combination thereof into a solution including a binder dissolved in a solvent to form a slurry having a viscosity greater than or equal to 200 cps and less than or equal to 1000 cps; mixing a cathode active material into the slurry until the slurry has a viscosity of greater than or equal to 4000 cps and less than or equal to 6000 cps; casting a continuous layer of the slurry onto a current collector; and removing the solvent from the slurry to produce the HF-scavenging electrode, the electrode having a first porosity, wherein the HF scavenging electrode comprises the ceramic HF scavenger embedded in the cathode active material; and The cathode active material comprises LiMn2O4.
7. The method of claim 6, wherein the solution comprising the binder dissolved in the solvent comprises 6 wt% polyvinylidene fluoride dissolved in N-methyl-2-pyrrolidone.
8. The method of claim 6, wherein the solution further comprises carbon black. 9 . The method of claim 6 , wherein the slurry comprises the cathode active material at a concentration of greater than or equal to 70 wt % to less than or equal to 95 wt %.
10. The method according to claim 6, further comprising: The electrode is calendered to create a second porosity in the electrode, the second porosity being lower than the first porosity.
Citation Information
Patent Citations
Ceramic-coated separators for lithium-containing electrochemical cells and methods of making the same
US20200403204A1
Inorganic binder lithium ion battery
CN108155384A
Protective cathode coatings for lithium-ion batteries
US20170229742A1
Composite porous separator including lithium ion-exchanged zeolite particles
US20180254449A1