A method for preparing a super-wetting coating on the outer surface of a stainless steel pipe

The preparation of super-immersion coating on the outer surface of stainless steel pipes through two-step electrochemical etching and anodizing method solves the problem that it is difficult to uniformly prepare super-immersion coatings in the prior art, and realizes simple and efficient coating preparation, which is suitable for Various application areas.

CN112680775BActive Publication Date: 2024-11-26CHONGQING UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202011322913.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-23
Publication Date
2024-11-26
Estimated Expiration
2040-11-23

AI Technical Summary

Technical Problem

The prior art is difficult to uniformly prepare super-immersion coatings on the outer surface of stainless steel pipes, and the traditional methods are complex and costly, and lack simple and efficient solutions.

Method used

Using two-step method of electrochemical etching and electrochemical anodizing, the super-immersion coating on the outer surface of stainless steel tubes is prepared through dynamic solution replenishment device and coaxial electrochemical treatment, and using electrochemical etching and anodizing electrolyte in stainless steel A uniform superhydrophobic coating is formed on the tube.

Benefits of technology

It realizes the preparation of uniform super-immersion coating on the outer surface of stainless steel pipes, which has the advantages of wide applicability, simple device, convenient operation, green and environmentally friendly and low cost, and is suitable for condensation heat transfer, fluid resistance reduction and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112680775B_ABST
    Figure CN112680775B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of preparation of super-wetting coatings on the surface of metal tubular substrates, and specifically to a method for preparing a super-wetting coating suitable for the outer surface of a stainless steel tube. The present invention adopts coaxial dynamic electrochemical etching and anodizing methods to prepare a uniform micro / nanostructure coating with super-wettability (super-hydrophilic and super-hydrophobic) on the outer surface of a stainless steel tube. The water contact angle of the obtained super-hydrophilic surface is close to 0°, and a super-hydrophobic surface is obtained after modification with a low surface energy material, and the water contact angle is greater than 150°. The method for preparing a super-wetting coating on the outer surface of a stainless steel tube provided by the present invention has the advantages of wide applicability, simple device, convenient operation, green environmental protection and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of super-wetting coatings on the surface of metal tubular substrates, in particular to a method for preparing super-wetting coatings suitable for the outer surface of stainless steel pipes. Background Art

[0002] Since its discovery in 1916, stainless steel has been widely used in petrochemical, medical, light industry, mechanical instrumentation and other fields because of its good corrosion resistance, wear resistance and processability. With the development of society, people's requirements for materials are getting higher and higher. The surface performance of traditional stainless steel can no longer meet people's living and production requirements in some fields. Wettability is one of the important properties of the material surface. When the contact angle of the droplet on the material surface is greater than 150°, the material surface is a super-hydrophobic surface; when the contact angle is less than 10°, the material surface is a super-hydrophilic surface. Stainless steel with super-wetting surface has good application prospects in condensation heat transfer, fluid resistance reduction, anti-icing and other fields. At present, the super-wetting modification treatment of stainless steel surface has been reported at home and abroad, but most scholars' research focuses on the preparation of super-wetting coating on planar substrates. Compared with the planar substrate, the tubular substrate has a certain curvature, and it is difficult to prepare a super-wetting coating on its surface. Therefore, it is urgent to develop a method for preparing stainless steel super-wetting coating with simple operation, simple equipment, safety, high efficiency and low cost. Summary of the invention

[0003] The object of the present invention is to provide a method for preparing a super-wetting coating on the outer surface of a stainless steel pipe, characterized in that it comprises the following steps:

[0004] 1〕Cleaning stainless steel tubes and cathode tubes;

[0005] 2) Drying the stainless steel tube and cathode tube treated in step 1);

[0006] 3〕Put the stainless steel tube into the cathode tube, making sure that the stainless steel tube and the cathode tube are double coaxial;

[0007] 4〕One end of the cathode tube is connected to a dynamic solution supply device;

[0008] 5) The stainless steel tube is connected to the positive electrode of the power supply, and the cathode tube is connected to the negative electrode of the power supply; after power is turned on, the dynamic solution supply device injects etching electrolyte into the cathode tube to perform electrochemical etching;

[0009] 6) After the electrochemical etching is completed, the etching electrolyte is replaced and an anodizing electrolyte is introduced to perform electrochemical anodizing to obtain a stainless steel tube with a super-hydrophobic coating.

[0010] It is worth noting that the purpose of the invention is to provide a two-step method of electrochemical etching and coaxial dynamic anodizing for preparing a uniform super-wetting coating on the outer surface of a stainless steel tube, which solves the problem that the prior art cannot uniformly prepare a super-wetting coating on the outer surface of a stainless steel tube.

[0011] Furthermore, both ends of the stainless steel tube and the cathode tube are open;

[0012] Furthermore, the upper and lower ends of the cathode tube are sealed with concentric plugs; the two concentric plugs are made of elastic material, and the centers thereof have a central through hole for the stainless steel tube to pass through; the two concentric plugs also have through holes for the solution to flow into and out of the stainless steel tube respectively;

[0013] Furthermore, at least one end of the stainless steel tube is sealed.

[0014] Furthermore, the stainless steel tube is made of one of the stainless steel materials such as ferritic stainless steel (such as 409, 430), austenitic stainless steel (such as 316, 316L, 304, 304L), martensitic stainless steel (such as 410, 420), etc.; the cathode tube is made of one of the conductive materials such as metal tube, alloy tube, graphite tube, etc.; the cleaning time is 0.5 to 3 hours.

[0015] Furthermore, in step 1), the stainless steel tube and the cathode tube are cleaned by ultrasonic vibration in a detergent, alcohol, and deionized water respectively, and the cleaning time is 0.5 to 4 hours;

[0016] Further, in step 2), the stainless steel tube and cathode tube in step 1) are blown dry with a nitrogen spray gun; and then the stainless steel tube and cathode tube are dried at a temperature of 50 to 80° C. for a drying time of 0.5 to 4 hours.

[0017] Further, in step 3), the stainless steel tube is vertically inserted into the cathode tube to fix the relative positions of the two;

[0018] Further, in step 4), the cathode tube is fixed vertically, and the lower end of the tube is connected to the dynamic solution replenishing device.

[0019] Further, in step 5), the etching electrolyte is transported by a peristaltic pump; the solvent of the electrochemical etching solution is one or more of the commonly used solvents such as water, ethylene glycol, glycerol, etc.; the solute is one of the halogen compounds such as sodium chloride, potassium chloride, calcium chloride, copper chloride, ferric chloride, sodium bromide, calcium bromide, potassium bromide, copper bromide, ferric bromide, etc., and the solution concentration is 0.05-3 mol / L; the electrochemical etching voltage is 5-60V, and the electrochemical etching time is 0.5-30min. The solvent of the electrochemical etching solution is one or more of the commonly used solvents such as water, ethylene glycol, glycerol, etc.; the solute is one of the halogen compounds such as sodium chloride, potassium chloride, calcium chloride, copper chloride, ferric chloride, sodium bromide, calcium bromide, potassium bromide, copper bromide, ferric bromide, etc., and the solution concentration is 0.05-3 mol / L; the electrochemical etching voltage is 5-60V, and the electrochemical etching time is 0.5-30min

[0020] Further, in step 6), the electrochemical anodizing solution is delivered by a peristaltic pump, the solvent of the electrochemical anodizing solution is one or more of commonly used solvents such as water, ethylene glycol, glycerol, etc.; the solute is one of fluorides such as sodium fluoride, potassium fluoride, calcium fluoride, copper fluoride, iron fluoride, ammonium fluoride, etc.; the solution concentration is 0.05-0.5 mol / L; the voltage of the electrochemical anodizing solution is 10-80 V, and the electrochemical etching time is 5-300 min.

[0021] Further, after the electrochemical anodizing described in step 6 is completed, the stainless steel tube is subjected to the following treatment:

[0022] Further, 7) the stainless steel tube is cleaned and then dried;

[0023] Further, 8) the stainless steel tube is subjected to annealing treatment.

[0024] Further, after the annealing treatment described in step 8) is completed, the stainless steel tube is subjected to the following treatment:

[0025] Further, 9) the stainless steel tube is soaked in a low surface energy modifier and then dried;

[0026] Furthermore, 10) the stainless steel tube is subjected to annealing treatment.

[0027] Further, in step 8), the annealing temperature is 350-550°C, the annealing time is 0.5-3h, and the heating rate is 1-10°C / min;

[0028] Further, in step 9), the low surface energy modifier solute is one of stearic acid, lauric acid, and fluorosilane, the solvent is one of ethanol and n-hexane, the solute volume concentration is 0.5-5%, the immersion time is 0.5-2h, the immersion temperature is 20-70°C, the drying temperature is 50-80°C, and the drying time is 1-3h.

[0029] Furthermore, in the step 10), the annealing temperature is 110-150° C., and the annealing time is 0.5-3 h.

[0030] The present invention adopts a two-step method of electrochemical etching and electrochemical anodizing to prepare a uniform super-wetting coating on the outer surface of a stainless steel pipe. The method of the present invention has the advantages of wide applicability, simple device, convenient operation, green environmental protection and low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a schematic diagram of an electrochemical etching and anodizing device. In the figure, 1, stainless steel tube; 2, concentric plug; 3, cathode tube; 4, waste liquid tank; 5, infusion tube; 6, peristaltic pump; 7, etching electrolyte reservoir; 8, anodizing electrolyte reservoir; 9, DC power supply.

[0032] Figure 2 It is a schematic diagram of the process of preparing the super-wettable outer surface of stainless steel.

[0033] Figure 3 This is a scanning electron micrograph of the outer surface of stainless steel after electrochemical etching.

[0034] Figure 4 This is a scanning electron micrograph of the outer surface of stainless steel after electrochemical anodization.

[0035] Figure 5 This is a static water contact angle test chart of the super-wettable outer surface of stainless steel that has not been modified with low surface energy materials.

[0036] Figure 6 This is a static water contact angle test chart of the super-wettable outer surface of stainless steel modified with low surface energy materials. DETAILED DESCRIPTION

[0037] The present invention is further described below in conjunction with the embodiments, but it should not be understood that the above subject matter of the present invention is limited to the following embodiments. Without departing from the above technical ideas of the present invention, various substitutions and changes are made according to the common technical knowledge and customary means in the art, which should all be included in the protection scope of the present invention.

[0038] Embodiment 1:

[0039] The device used in this embodiment is as shown in the attached Figure 1As shown in the figure, one end of the infusion tube 5 is connected to the liquid outlet of the peristaltic pump 6, and the other end is connected to the lower inlet of the cathode tube 3. Liquid can be supplied to the cathode tube 3 through the peristaltic pump 6. The inlet of the peristaltic pump 6 is connected to the etching electrolyte storage tank 7 and the anodizing electrolyte storage tank 8 through a branch pipeline. The etching electrolyte or the anodizing electrolyte can enter the peristaltic pump 6 by opening and closing the valve, and then be transported to the cathode tube 3 by the peristaltic pump 6. After the etching electrolyte or the anodizing electrolyte is transported to the cathode tube 3, it overflows from the upper end of the cathode tube 3 and / or from the upper end of the stainless steel tube 1. A collection tank for collecting overflowed liquid is provided below the infusion tube 5. A DC power supply 9 provides power for the reaction.

[0040] In this embodiment, the following steps are included:

[0041] 1〕Ultrasonic cleaning of the stainless steel tube and cathode tube (the inner diameter of the cathode tube is larger than the outer diameter of the stainless steel tube) in detergent, alcohol and deionized water respectively;

[0042] 2) Dry the stainless steel tube and cathode tube in step 1) with a nitrogen spray gun;

[0043] 3〕The stainless steel tube is inserted into the dry cathode tube, fixed at the axial position of the cathode tube with a concentric plug 2, and the stainless steel tube is fixed vertically; that is, the stainless steel tube and the cathode tube are kept coaxial as much as possible; one end of the cathode tube is connected to the dynamic solution replenishing device; preferably, the cathode tube is made of a conductive material such as a metal tube, an alloy tube, or a graphite tube;

[0044] 4) Connect the outer surface of the stainless steel tube in step 3) to the positive electrode of the power supply, connect the cathode tube to the negative electrode of the power supply, turn on the peristaltic pump switch to pass the etching electrolyte and control the flow rate. When the etching electrolyte flows out from the upper end of the cathode tube, turn on the power supply to perform electrochemical etching under constant voltage conditions;

[0045] 5〕After the electrochemical etching is completed, pour out the etching electrolyte between the anode and cathode (inside the cathode tube and the infusion tube), reconnect the outer surface of the stainless steel tube to the positive electrode of the power supply, and the cathode tube to the negative electrode of the power supply. Turn on the peristaltic pump switch to pass the anodic oxidation electrolyte and control the flow rate. When the anodic oxidation electrolyte flows out from the upper end of the cathode tube, turn on the power supply to perform electrochemical anodic oxidation under constant voltage conditions;

[0046] 6〕Clean and dry the stainless steel tube;

[0047] The stainless steel tube is cleaned with deionized water and then dried;

[0048] 7〕The stainless steel tube is annealed.

[0049] 8〕 Soak the stainless steel tube in a low surface energy modifier and then dry it;

[0050] 9) Annealing the stainless steel tube.

[0051] Example 2

[0052] The difference from Example 1 is that:

[0053] In step (1), the outer diameter of the stainless steel tube is 0.2 mm, and the material is 316 austenitic stainless steel; the cathode tube is a titanium tube, and the inner diameter is 3 mm.

[0054] In step (5), the etching electrolyte is an aqueous solution of potassium chloride with a concentration of 0.5 mol / L, the etching time is 2 min, and the flow rate of the electrolyte solution is 10 mL / min.

[0055] In step (6), the anodizing electrolyte is an ethylene glycol solution of ammonium fluoride with a concentration of 0.1 mol / L, the anodizing voltage is 50 V and the time is 40 min, and the flow rate of the electrolyte solution is 10 mL / min.

[0056] In step (9), the low surface energy material is a n-hexane solution of stearic acid with a volume concentration of 0.5%, and the immersion time is 1.5 hours.

[0057] Example 3

[0058] The difference from Example 1 is that:

[0059] In step (1), the outer diameter of the stainless steel tube is 0.8 mm, and the material is 304L austenitic stainless steel; the cathode tube is a copper tube with an inner diameter of 5 mm.

[0060] In step (5), the etching electrolyte is a 0.1 mol / L sodium chloride propylene glycol solution, the etching time is 10 min, and the electrolyte solution flow rate is 18 mL / min.

[0061] In step (6), the anodizing electrolyte is an ethylene glycol solution of sodium fluoride with a concentration of 0.1 mol / L, the anodizing voltage is 30 V and the time is 35 min, and the flow rate of the electrolyte solution is 18 mL / min.

[0062] In step (9), the annealing temperature is 450°C, the annealing time is 1.5h, and the heating rate is 2.5°C / min.

[0063] Example 4

[0064] The difference from Example 1 is that:

[0065] In step (1), the outer diameter of the stainless steel tube is 2 mm, and the material is 304 austenitic stainless steel; the cathode tube is an aluminum alloy tube, and the inner diameter is 8 mm.

[0066] In step (5), the etching time is 25 min and the flow rate of the electrolyte solution is 20 mL / min.

[0067] In step (6), the anodic oxidation voltage is 40 V for 45 min, and the flow rate of the electrolyte solution is 20 mL / min.

[0068] Example 5

[0069] The difference from Example 1 is that:

[0070] In step (1), the outer diameter of the stainless steel tube is 5 mm, and the material is 409 ferritic stainless steel; the cathode tube is a titanium tube, and the inner diameter is 10 mm.

[0071] In step (5), the etching time is 25 minutes, the etching electrolyte is an ethylene glycol solution of sodium chloride with a concentration of 0.5 mol / L, and the flow rate of the electrolyte solution is 30 mL / min.

[0072] In step (6), the anodic oxidation voltage is 25 V for 60 min, and the flow rate of the electrolyte solution is 30 mL / min.

[0073] In step (9), the low surface energy material is a n-hexane solution of stearic acid with a volume concentration of 1%, and the immersion time is 0.5 h.

[0074] Example 6

[0075] The difference from Example 1 is that:

[0076] In step (1), the outer diameter of the stainless steel tube is 10 mm, and the material is 430 ferritic stainless steel; the cathode tube is an aluminum tube, and the inner diameter is 15 mm.

[0077] In step (5), the etching time is 30 min and the flow rate of the electrolyte solution is 45 mL / min.

[0078] In step (6), the anodization time is 80 min and the electrolyte solution flow rate is 45 mL / min.

[0079] In step (9), the annealing temperature is 500°C, the annealing time is 2h, and the heating rate is 5°C / min;

[0080] Example 7

[0081] The difference from Example 1 is that:

[0082] In step (1), the outer diameter of the stainless steel tube is 20 mm, and the material is 420 martensitic stainless steel; the cathode tube is a titanium tube with an inner diameter of 35 mm.

[0083] In step (5), the etching time is 50 min and the flow rate of the electrolyte solution is 75 mL / min.

[0084] In step (6), the anodization time is 110 min and the electrolyte solution flow rate is 75 mL / min.

[0085] In step (9), the low surface energy material is an ethanol solution of lauric acid with a volume concentration of 4.5%.

[0086] The results of the embodiment show that the present invention uses a two-step method of coaxial electrochemical etching and dynamic anodization to prepare a super-wetting coating on the outer surface of a stainless steel tube. The water contact angle of the super-hydrophilic stainless steel outer surface obtained is close to 0°, and the water contact angle of the super-hydrophobic outer surface is greater than 150°. The method for preparing a super-wetting coating on the outer surface of a stainless steel tube provided by the present invention has the advantages of wide applicability, simple device, convenient operation, green environmental protection and low cost. It can be widely used in the field of preparing super-wetting coatings on the outer surface of stainless steel tubes.

Claims

1. A method for preparing a super-wetting coating on the outer surface of a stainless steel pipe, characterized in that: The following steps are involved: 1〕Cleaning stainless steel tubes and cathode tubes; the outer diameter of stainless steel tubes is 0.2mm, 0.8mm, 2mm, 5mm, 10mm or 20mm; 2) Drying the stainless steel tube and cathode tube treated in step 1); 3〕Put the stainless steel tube into the cathode tube, and ensure that the stainless steel tube and the cathode tube are double coaxial; 4〕One end of the cathode tube is connected to a dynamic solution supply device; 5〕The stainless steel tube is connected to the positive electrode of the power supply, and the cathode tube is connected to the negative electrode of the power supply; after power is turned on, the dynamic solution supply device injects an etching electrolyte into the cathode tube to perform electrochemical etching; the solvent of the electrochemical etching solution is one or more of water, ethylene glycol, and glycerol; the solute is one of sodium chloride, potassium chloride, calcium chloride, copper chloride, ferric chloride, sodium bromide, calcium bromide, potassium bromide, copper bromide, and ferric bromide, and the solution concentration is 0.05-3 mol / L; the electrochemical etching voltage is 5-60V, and the electrochemical etching time is 0.5-30min; 6) After the electrochemical etching is completed, the etching electrolyte is replaced, and an anodizing electrolyte is introduced to perform electrochemical anodizing to obtain a stainless steel tube with a super-hydrophobic coating; After the electrochemical anodizing described in step 6 is completed, the stainless steel tube is subjected to the following treatment: 7〕Clean and dry the stainless steel tube; 8) Annealing of stainless steel pipe; After the annealing treatment described in step 8 is completed, the stainless steel tube is subjected to the following treatments: 9〕 Soak the stainless steel tube in a low surface energy modifier and then dry it; 10) Annealing the stainless steel tube; In step 6), the electrochemical anodizing solution is delivered by a peristaltic pump, the solvent of the electrochemical anodizing solution is one or more of water, ethylene glycol, and glycerol; the solute is one of sodium fluoride, potassium fluoride, calcium fluoride, copper fluoride, iron fluoride, and ammonium fluoride; the solution concentration is 0.05-0.5 mol / L; the voltage of the electrochemical anodizing solution is 10-80 V, and the electrochemical etching time is 5-300 min; In step 8), the annealing temperature is 350-550°C, the annealing time is 0.5-3h, and the heating rate is 1-10°C / min; In step 9), the low surface energy modifier solute is one of stearic acid, lauric acid, and fluorosilane, the solvent is one of ethanol and n-hexane, the solute volume concentration is 0.5-5%, the immersion time is 0.5-2h, the immersion temperature is 20-70°C, the drying temperature is 50-80°C, and the drying time is 1-3h; In the step 10), the annealing temperature is 110-150° C. and the annealing time is 0.5-3 h.

2. The method for preparing a super-wetting coating on the outer surface of a stainless steel pipe according to claim 1, characterized in that: Both ends of the stainless steel tube and the cathode tube are open; The upper and lower ends of the cathode tube are sealed with concentric plugs; the two concentric plugs are made of elastic material, and have a central through hole in the center for the stainless steel tube to pass through; the two concentric plugs also have through holes for the solution to flow into and out of the stainless steel tube respectively; At least one end of the stainless steel tube is blocked.

3. The method for preparing a super-wetting coating on the outer surface of a stainless steel pipe according to claim 1, characterized in that: The material of the stainless steel tube is one of ferritic stainless steel, austenitic stainless steel, and martensitic stainless steel; the material of the cathode tube is one of metal tube, alloy tube, and graphite tube; the cleaning time is 0.5 to 3 hours.

4. The method for preparing a super-wetting coating on the outer surface of a stainless steel pipe according to claim 1, characterized in that: In step 1), the stainless steel tube and the cathode tube are cleaned by ultrasonic vibration in a detergent, alcohol, and deionized water respectively, and the cleaning time is 0.5 to 4 hours; In step 2), the stainless steel tube and cathode tube in step 1 are blown dry with a nitrogen spray gun; the stainless steel tube and cathode tube are then dried at a temperature of 50 to 80° C. for a drying time of 0.5 to 4 hours.

5. The method for preparing a super-wetting coating on the outer surface of a stainless steel pipe according to claim 1, characterized in that: In step 3), the stainless steel tube is vertically inserted into the cathode tube to fix the relative positions of the two; In step 4), the cathode tube is fixed vertically, and its lower end is connected to a dynamic solution supply device.

6. The method for preparing a super-wetting coating on the outer surface of a stainless steel pipe according to claim 1, characterized in that: In step 5), the etching electrolyte is delivered by a peristaltic pump.

Citation Information

Patent Citations

  • Preparation method of superhydrophobic surface of metal zirconium

    CN101941000A

  • Method for processing super-hydrophobic surface, and evaporator having super-hydrophobic surface

    CN103702928A

  • Preparation method for super-wetting foam titanium for oil water separation

    CN108179454A

  • Preparation method of super-wetting coating on inner surface of U-shaped titanium tube

    CN110552042A

  • Heat exchange tube of efficient liquid nitrogen heat exchanger and heat exchanger

    CN111811315A