Ammonia and Ammonium Hydroxide Stabilizers for Paraformaldehyde

By using ammonia and/or ammonium hydroxide stabilizers to react with paraformaldehyde chain ends to inhibit chain growth and alcohol end-capping, the problems of reduced solubility and increased viscosity during storage and transportation of paraformaldehyde are solved, achieving long shelf life and Easy to operate.

CN112714773BActive Publication Date: 2024-10-22CELANESE INTERNATIONAL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980060701.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-09-28
Filing Date
2019-09-05
Publication Date
2024-10-22
Estimated Expiration
2039-09-05

AI Technical Summary

Technical Problem

During storage and transportation, the solubility of paraformaldehyde decreases due to changes in molecular weight and chain growth, resulting in the formation of insoluble matter, resulting in a short shelf life. Existing stabilizers increase viscosity and are difficult to operate.

Method used

Use ammonia and/or ammonium hydroxide as stabilizers to form crystals by reacting with paraformaldehyde chain ends, inhibiting chain growth and alcohol end-capping, extending shelf life and avoiding viscosity increase.

Benefits of technology

A non-sticky paraformaldehyde product is achieved, which extends the shelf life, maintains the original performance during transportation and operation, and avoids an increase in the concentration of insoluble matter.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0002979482610000011
    Figure HDA0002979482610000011
Patent Text Reader

Abstract

A method of forming a stabilized paraformaldehyde may include: heating a formaldehyde solution comprising 30 wt % or more formaldehyde to a temperature of about 70° C. to about 130° C.; aging the formaldehyde solution for a sufficient time to polymerize the formaldehyde and form the paraformaldehyde; curing the paraformaldehyde; and contacting the formaldehyde solution before and / or during heating, the formaldehyde solution during aging, the paraformaldehyde, and / or the cured paraformaldehyde with an ammonia and / or ammonium hydroxide stabilizer.
Need to check novelty before this filing date? Find Prior Art

Description

Background of the Invention

[0002] The present invention is directed to improving the shelf life, handling and transportation of paraformaldehyde.

[0003] Paraformaldehyde is a solid form of 80% or more formaldehyde. Typically, the formaldehyde concentration is 90% to 96%. Paraformaldehyde is considered to be a polyoxymethylene glycol, HO-(CH2O) n -H, wherein n = 8-100. Generally, paraformaldehyde is produced by concentrating a hot aqueous formaldehyde solution under reduced pressure. After cooling, the resulting solution is solidified into pellets for storage and / or transportation.

[0004] After paraformaldehyde is first produced, it exhibits excellent solubility in water and organic solvents such as butanol. Paraformaldehyde is easily dissolved in water or alcohol by hydrolysis or depolymerization to produce methylene glycol or formal. However, the solubility of paraformaldehyde in water and solvents decreases over time or when stored at temperatures generally above about 35°C. This change in solubility is presumably due to changes in molecular weight (or value of n) and the termination of the paraformaldehyde chain by methanol. As the molecular weight increases, the solubility and reactivity of paraformaldehyde decrease.

[0005] The presence of methanol in the reaction mixture also forms insolubles. Insolubles are generally paraformaldehydes that have been capped with alcohols to form ethers. These high molecular weight ethers are insoluble in any solution (unless the solution contains a strong acid). Paraformaldehyde includes insolubles that are typically in a concentration of about 10ppm to 20ppm. As the time that the paraformaldehyde is stored passes, a small amount of alcohol in the pellets reacts with the paraformaldehyde to form more insolubles. For example, the concentration of insolubles after storage at ambient temperature can exceed 100ppm, and in some cases, if there is a high concentration of methanol, it is 350ppm or higher. The industry standard for an acceptable amount of insolubles is less than 100ppm. Therefore, the shelf life of paraformaldehyde is very short.

[0006] To alleviate this problem, various stabilizers and inhibitors have been proposed. For example, amines such as hexaethylamine and triethylamine have been used. It is believed that stabilizers slow down chain growth and slow down the end-capping of the paraformaldehyde, so that insoluble matter formation is reduced over time. However, stabilizers also increase the stickiness of the pellets, which makes them very difficult to manufacture and handle. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] The following drawings are included to illustrate certain aspects of the embodiments and should not be considered exclusive embodiments. The disclosed subject matter is capable of considerable modification, alteration, combination, and equivalents in form and function as will occur to those skilled in the art and having the benefit of this disclosure.

[0009] Figure 1 A diagram showing the apparatus simulating a quench vessel. DETAILED DESCRIPTION OF THE INVENTION

[0011] The present disclosure relates to improving the shelf life, handling, and transportation of paraformaldehyde using ammonia and / or ammonium hydroxide as stabilizers.

[0012] As used herein, the term "pellet" refers to a pellet or solid pellet. Depending on the manner in which the paraformaldehyde is cured and dried, the finished paraformaldehyde may also be in the form of flakes, agglomerates, granules, and the like. The finished paraformaldehyde is described herein as "cured paraformaldehyde" and may be in any suitable cured form, including but not limited to pellets, flakes, agglomerates, granules, and the like.

[0013] At low concentrations, the hydrocarbon amines can stabilize the cured paraformaldehyde without making the cured paraformaldehyde tacky. However, the concentration of the hydrocarbon amines is low enough that the shelf life of the cured paraformaldehyde is not significantly extended. At higher concentrations, the hydrocarbon amines make the cured paraformaldehyde tacky to the point where it cannot be transported by normal means such as compressed air.

[0014] It has been found that using ammonia and / or ammonium hydroxide as a stabilizer for paraformaldehyde produces a cured paraformaldehyde that is not tacky and has a long shelf life because the stabilizer can be used in high concentrations. Urea can be used as a source of ammonia by mixing urea with water and heating.

[0015] Without being limited by theory, it is believed that the ammonia and / or ammonium hydroxide reacts with the ends of the paraformaldehyde chains to form crystalline oximes and also neutralizes any acid catalyst, both of which effectively inhibit chain growth and alcohol termination of the cured paraformaldehyde.

[0016] In general, the production of solidified paraformaldehyde includes heating a formaldehyde solution containing 30% by weight or more formaldehyde (e.g., about 30% to 90% by weight formaldehyde) to a temperature of about 70°C to about 130°C, preferably about 80°C to about 100°C. The formaldehyde solution is maintained at this temperature for about 0.1 hour to about 3 hours, preferably about 20 minutes to about 40 minutes, and more preferably about 20 minutes to about 30 minutes. This is generally referred to as aging. During aging, the formaldehyde polymerizes to form paraformaldehyde. Once the aging step is completed, the paraformaldehyde product is solidified. Specifically, in order to form pellets, the paraformaldehyde is passed through a nozzle in a pelletizing tower to form pellets that fall into a gas countercurrent. This solidifies the paraformaldehyde. Polymerization can still occur during the curing of the paraformaldehyde. Optionally, the solidified paraformaldehyde is transferred to a quenching vessel, typically using compressed air, for further cooling. The cured paraformaldehyde can be dried at a temperature of about ambient temperature to about 150° C., preferably about 50° C. to about 100° C., for a time of about 15 minutes to about 20 hours, preferably about 1 hour to about 2 hours. Polymerization can still occur during the drying of the cured paraformaldehyde. The cured paraformaldehyde is then stored or shipped to the customer. Handling and transporting the cured paraformaldehyde within the plant or to and from storage is typically performed using compressed air. The use of ammonia and / or ammonium hydroxide stabilizers does not make the cured paraformaldehyde as sticky as other amine stabilizers, so the handling and transportation of the cured paraformaldehyde is essentially the same as untreated cured paraformaldehyde. Ammonia and / or ammonium hydroxide stabilizers can be incorporated in any part of the manufacture or storage of the paraformaldehyde.

[0017] An exemplary embodiment of the present disclosure includes: heating a formaldehyde solution containing 30 wt% or more formaldehyde and about 50 ppm to about 1000 ppm, preferably 100 ppm to 500 ppm, more preferably 150 ppm to 250 ppm ammonia and / or ammonium hydroxide stabilizer to a temperature of about 70°C to about 130°C; aging the formaldehyde solution for a sufficient time to polymerize the formaldehyde and form paraformaldehyde; and curing the paraformaldehyde (e.g., transferring the paraformaldehyde through a nozzle in a prilling tower to form pellets that fall into a countercurrent of gas for further polymerization and curing). The method may also include drying the cured paraformaldehyde.

[0018] Another exemplary embodiment of the present disclosure includes: heating a formaldehyde solution containing 30% by weight or more formaldehyde to a temperature of about 70°C to about 130°C; aging the formaldehyde solution for a sufficient time to polymerize the formaldehyde and form paraformaldehyde in the presence of about 50 ppm to about 1000 ppm, preferably 100 ppm to 500 ppm, more preferably 150 ppm to 250 ppm ammonia and / or ammonium hydroxide stabilizer; and curing the paraformaldehyde (e.g., transferring the paraformaldehyde through a nozzle in a prilling tower to form pellets that fall into a countercurrent of gas for further polymerization and curing). The method may also include drying the cured paraformaldehyde.

[0019] Yet another exemplary embodiment of the present disclosure includes: heating a formaldehyde solution containing 30% by weight or more formaldehyde to a temperature of about 70°C to about 130°C; aging the formaldehyde solution for a sufficient time to polymerize the formaldehyde and form paraformaldehyde; and curing the paraformaldehyde in a prilling tower (e.g., transferring the paraformaldehyde via a nozzle to form pellets that fall into a countercurrent of the gas) in the presence of a gas containing about 10 ppm to about 1000 ppm, preferably 25 ppm to 500 ppm, more preferably 50 ppm to 150 ppm ammonia and / or ammonium hydroxide stabilizer, to further polymerize and cure. The method may also include drying the cured paraformaldehyde.

[0020] Another exemplary embodiment of the present disclosure includes: heating a formaldehyde solution comprising 30 wt % or more formaldehyde to a temperature of about 70° C. to about 130° C.; aging the formaldehyde solution for a sufficient time to polymerize the formaldehyde and form paraformaldehyde; curing the paraformaldehyde (e.g., transferring the paraformaldehyde through a nozzle in a prilling tower to form pellets that fall into a countercurrent of gas for further polymerization and curing); drying the cured paraformaldehyde; and during and / or after drying, exposing the cured paraformaldehyde to a gas comprising about 10 ppm to about 1000 ppm, preferably 25 ppm to 500 ppm, more preferably 50 ppm to 150 ppm ammonia and / or ammonium hydroxide stabilizer.

[0021] Another exemplary embodiment of the present disclosure includes: heating a formaldehyde solution comprising 30 wt % or more formaldehyde to a temperature of about 70° C. to about 130° C.; aging the formaldehyde solution for a sufficient time to polymerize the formaldehyde and form paraformaldehyde; solidifying the paraformaldehyde (e.g., transferring the paraformaldehyde through a nozzle in a prilling tower to form pellets that fall into a countercurrent of gas for further polymerization and solidification); drying the solidified paraformaldehyde; transporting the solidified paraformaldehyde to a storage facility; and during transportation or in the storage facility, exposing the solidified paraformaldehyde to a gas comprising about 10 ppm to about 1000 ppm, preferably 25 ppm to 500 ppm, more preferably 50 ppm to 150 ppm ammonia and / or ammonium hydroxide stabilizer.

[0022] Combinations of the foregoing methods may be used. For example, ammonia and / or ammonium hydroxide stabilizers may be used in one or more of the heating, aging, curing, drying, or storage steps. When two or more steps include exposure to ammonia and / or ammonium hydroxide stabilizers, lower concentrations of ammonia and / or ammonium hydroxide stabilizers may be used in each step.

[0023] In each of the foregoing embodiments, urea may be used as the source of ammonia and / or ammonium hydroxide stabilizer.

[0024] In each of the foregoing embodiments, the formaldehyde solution may comprise 30 wt % or more formaldehyde (eg, about 30 to 90 wt % formaldehyde), preferably about 35 to 75 wt % formaldehyde, and more preferably about 36 to 50 wt % formaldehyde.

[0025] In each of the foregoing embodiments, the formaldehyde solution may be heated to a temperature of about 70°C to about 130°C, preferably about 80°C to about 100°C.

[0026] In each of the foregoing embodiments, the formaldehyde solution may be maintained (aged) at a temperature of about 70°C to about 130°C, preferably about 80°C to about 100°C, for about 0.1 hour to about 3 hours, preferably about 20 minutes to about 40 minutes, and more preferably about 20 minutes to about 30 minutes.

[0027] In each of the foregoing embodiments, the cured paraformaldehyde may be dried at a temperature from about ambient temperature to about 150°C, preferably from about 50°C to about 100°C, for a time from about 15 minutes to about 20 hours, preferably from about 1 hour to about 2 hours.

[0028] Exposing the solidified paraformaldehyde to ammonia and / or ammonium hydroxide stabilizer at any time between and including forming and storing can include exposing the solidified paraformaldehyde to a gas containing from about 10 ppm to about 1000 ppm, preferably from 25 ppm to 500 ppm, more preferably from 50 ppm to 150 ppm ammonia and / or ammonium hydroxide stabilizer. The ammonia and / or ammonium hydroxide stabilizer can be diluted in a carrier gas. Examples of carrier gases include, but are not limited to, air, oxygen, nitrogen, carbon dioxide, argon, and the like, and any combination thereof.

[0029] In each of the foregoing embodiments, the formaldehyde solution may further include an acid or alkaline catalyst. Examples of catalysts include, but are not limited to, formic acid, boric acid, sodium tetraborate, oxalic acid, and any combination thereof.

[0030] In each of the foregoing embodiments, the formaldehyde solution, the paraformaldehyde, and the cured paraformaldehyde may lack an organic amine. As used herein, the term "organic amine" includes low molecular weight compounds (less than 500 g / mol, preferably less than 300 g / mol) composed of carbon, hydrogen, nitrogen, and optionally oxygen. Examples of organic amines include, but are not limited to, methylamine, ethylamine, n-propylamine, n-butylamine, isobutylamine, tert-butylamine, dimethylamine, diethylamine, di-n-propylamine, diisopropylamine, dibutylamine, triethylamine, and triethanolamine, hexamethylenetetramine, 2-ethylhexylamine, 2-aminopropylene glycol, hexylamine, ethanolamine, mixed C 20 Amines, Mixed C 10 Amine, cyclohexylamine, 1,2-dimethoxypropaneamine, triethylamine, ethanolamine, 1-amino-1,3-propanediol, 1-aminopentane, 2-methyloxypropylamine, and any combination thereof.

[0031] In each of the foregoing embodiments, the method may further include storing the cured paraformaldehyde at ambient temperature to 50° C. for more than 30 days (e.g., 30 days to one year or longer) without increasing the insoluble concentration in the cured paraformaldehyde to above about 150 ppm, preferably about 120 ppm, more preferably about 100 ppm.

[0032] Another embodiment of the present disclosure is a paraformaldehyde composition comprising from about 1 ppm to 100 ppm, preferably from about 5 ppm to about 50 ppm, more preferably from about 10 ppm to about 25 ppm of ammonia and / or ammonium hydroxide stabilizer, and from about 80 wt % to about 99.9 wt %, preferably from about 90 wt % to about 99.9 wt %, more preferably from about 95 wt % to about 99.9 wt % of paraformaldehyde.

[0033] The paraformaldehyde composition may further comprise insoluble matter in an amount of from about 1 ppm to about 200 ppm, preferably from about 5 ppm to about 100 ppm, and more preferably from about 10 ppm to about 50 ppm.

[0034] In each of the aforementioned paraformaldehyde composition embodiments, the paraformaldehyde composition may further include an acid or alkaline catalyst. Examples of catalysts include, but are not limited to, formic acid, boric acid, sodium tetraborate, oxalic acid, and any combination thereof.

[0035] The source of ammonia and / or ammonium hydroxide stabilizer is urea. In each of the aforementioned paraformaldehyde composition embodiments, the paraformaldehyde composition may lack organic amines. Examples of organic amines include, but are not limited to, methylamine, ethylamine, n-propylamine, n-butylamine, isobutylamine, tert-butylamine, dimethylamine, diethylamine, di-n-propylamine, diisopropylamine, dibutylamine, triethylamine, and triethanolamine, hexamethylenetetramine, 2-ethylhexylamine, 2-aminopropylene glycol, hexylamine, ethanolamine, mixed C 20 Amines, Mixed C 10 Amine, cyclohexylamine, 1,2-dimethoxypropaneamine, triethylamine, ethanolamine, 1-amino-1,3-propanediol, 1-aminopentane, 2-methyloxypropylamine, and any combination thereof.

[0036] For each of the foregoing paraformaldehyde composition embodiments, the cured paraformaldehyde can be in the form of pellets, flakes, briquettes, granules, and the like.

[0037] An exemplary embodiment of the present invention is a method comprising: heating a formaldehyde solution comprising 30 wt % or more formaldehyde to a temperature of about 70° C. to about 130° C.; aging the formaldehyde solution for a sufficient time to polymerize the formaldehyde and form paraformaldehyde; curing the paraformaldehyde; and contacting the formaldehyde solution before and / or during heating, the formaldehyde solution during aging, the paraformaldehyde, and / or the cured paraformaldehyde with an ammonia and / or ammonium hydroxide stabilizer. Optionally, the method may include one or more of the following: Element 1: wherein the formaldehyde solution during heating further comprises about 50 ppm to about 1000 ppm of ammonia and / or ammonium hydroxide stabilizer; Element 2: wherein the formaldehyde solution during aging further comprises about 50 ppm to about 1000 ppm of ammonia and / or ammonium hydroxide stabilizer; Element 3: wherein curing the paraformaldehyde involves contacting the paraformaldehyde with a gas comprising about 10 ppm to about 1000 ppm of ammonia and / or ammonium hydroxide stabilizer; Element 4: the method further comprises drying the cured paraformaldehyde; Element 5: Element 4 and the method further comprises, during and / or after drying, exposing the cured paraformaldehyde to a gas comprising about 10 ppm to about 1000 ppm of ammonia and / or ammonium hydroxide stabilizer; Element 6: Element 4 or 5 and the method further comprises exposing the cured paraformaldehyde to a gas comprising about 10 ppm to about 1000 ppm of ammonia and / or ammonium hydroxide stabilizer; transporting the polyformaldehyde to a storage facility; Element 7: Element 6 and the method further includes exposing the solidified polyformaldehyde to a gas containing about 10 ppm to about 1000 ppm ammonia and / or ammonium hydroxide stabilizer during transportation or in the storage facility; Element 8: Element 6 or 7 and the method further includes storing the solidified polyformaldehyde at ambient temperature to about 50°C for more than 30 days and maintaining the insoluble concentration in the solidified polyformaldehyde below about 150 ppm; Element 9: wherein aging of the formaldehyde solution lasts for about 0.1 hour to about 3 hours; Element 10: wherein an organic amine is not included in the method; Element 11: the method further includes transporting the solidified polyformaldehyde to a storage facility; Element 12: wherein the formaldehyde solution is aged at 70°C to 130°C; and Element 13: wherein the source of the ammonia and / or ammonium hydroxide stabilizer is urea. Examples of combinations include, but are not limited to: elements 1, 4 and 11 combined; elements 2, 4 and 11 combined; elements 3, 4 and 11 combined; elements 4, 5 and 11 combined; elements 4, 6 and 7 (and optionally 8) combined; elements 1, 4, 6 and 8 combined; elements 2, 4, 6 and 8 combined; elements 3, 4, 6 and 8 combined; two or more of elements 1, 2, 3, 4 and 5 combined, optionally further combined with elements 6 and 7; and elements 9, 12 and / or 13 combined with any of the foregoing.

[0038] Another exemplary embodiment of the present invention is a method comprising exposing a cured paraformaldehyde to a gas comprising from about 10 ppm to about 1000 ppm ammonia and / or ammonium hydroxide stabilizer. Optionally, the cured paraformaldehyde lacks an organic amine, and / or the source of the ammonia and / or ammonium hydroxide stabilizer is urea.

[0039] Another exemplary embodiment of the present invention is a cured paraformaldehyde comprising: about 1 ppm to 100 ppm of ammonia and / or ammonium hydroxide stabilizer, and about 80 wt % to about 99.9 wt % of the paraformaldehyde. Optionally, the cured paraformaldehyde may include one or more of the following: Element 14: wherein the cured paraformaldehyde lacks organic amines; Element 15: the cured paraformaldehyde also contains less than 150 ppm of insolubles; and Element 16: wherein the cured paraformaldehyde is in the form of pellets, flakes, agglomerates or granules.

[0040] Unless otherwise indicated, all numbers used in this specification and the associated claims expressing amounts of ingredients, properties such as molecular weight, reaction conditions, and the like should be understood as being modified in all instances by the term "about". Therefore, unless otherwise indicated, the numerical parameters set forth in the following specification and the appended claims are approximations that may vary depending on the desired properties sought to be obtained by embodiments of the present invention. At the very least, and not as an attempt to limit the application of the doctrine of equivalents to the scope of the claims, each numerical parameter should at least be interpreted in light of the number of reported significant digits and by applying ordinary rounding techniques.

[0041] One or more illustrative embodiments of the invention embodiments disclosed herein are presented herein. For clarity, not all features of material implementation methods are described or shown in this application. It is to be understood that in the development of the material embodiments of the embodiments of the present invention, numerous implementation method specific decisions must be made to reach the developer's goal, such as meeting system-related, enterprise-related, government-related and other constraints, which vary from time to time depending on the implementation method. Although the developer's efforts may be time-consuming, such efforts will be a routine task of those of ordinary skill in the art and have the benefit of the present disclosure.

[0042] Although compositions and methods are described herein in terms of "comprising / including various components or steps," the compositions and methods may also "consist essentially of" or "consist of" the various components and steps.

[0043] To aid in a better understanding of the embodiments of the present invention, the following examples of preferred or representative embodiments are given. The following examples should in no way be read as limiting or defining the scope of the present invention. Example

[0044] Example 1. Use according to Figure 1 The apparatus 100 is used to simulate a quench vessel. The apparatus 100 includes a drying tube 102 (2.5 inch radius, 11 inch height) having a porous plate 104 1.75 inches from the bottom, a gas inlet 106 located between the bottom of the drying tube 102 and the porous plate 104, and a vent 108 at the top of the drying tube 102. In addition, a thermocouple 110 extends through the top of the drying tube 102 to above the porous plate to measure the temperature in the drying tube 102. The gas inlet 106 is fluidly coupled to an ammonia and / or ammonium hydroxide stabilizer source 112 (e.g., a tank of ammonia, a tank of ammonia diluted in air, a solution of urea in water, a solution of ammonium hydroxide, and the like). As used herein, when two components are described as being fluidly coupled, there is hardware connecting the two components so that fluid can be transferred from one component to another. The hardware can be more than one component, including lines, tubing, pipes, pumps, connectors, heat exchangers, valves, and the like.

[0045] Between the ammonia and / or ammonium hydroxide stabilizer source 112 is a heat exchanger 114, which is used to heat the ammonia and / or ammonium hydroxide stabilizer prior to introduction into the drying tube 102. Optionally, a gas (e.g., process air) may entrain the ammonia and / or ammonium hydroxide stabilizer via line 116 to dilute the ammonia and / or ammonium hydroxide stabilizer to a desired concentration.

[0046] In this example, 350 grams of paraformaldehyde pellets were added to the drying tube 102, which resulted in the top level of the pellets being 2.5 inches from the top of the drying tube 102. A tank of 100 ppm ammonia in air was used as the ammonia and / or ammonium hydroxide stabilizer source 112. The heat exchanger 114 was set at 200°F (93.3°C). 100 ppm ammonia in air was passed through the apparatus 100 at 30 standard cubic feet per minute, which resulted in the pellets becoming a fluidized bed in the drying tube 102. The pellets maintained a fluidized bed, indicating that the ammonia and / or ammonium hydroxide stabilizer did not make the pellets too sticky for shipping.

[0047] The same experiment was performed using ethylhexylamine as the stabilizer. The pellets became too viscous to fluidize in the drying tube 102.

[0048] Example 2. In a full-scale plant, paraformaldehyde pellets were exposed to different concentrations of ammonium hydroxide in a prilling tower. More specifically, a solution of 19% ammonium hydroxide in water was heated to about 90°C. The resulting vapor was passed through a prilling tower. Optionally, the vapor was diluted with process air. The pellets were then aged at 50°C for 4 days, which simulates 6 months of aging under normal storage conditions (about 23°C to 38°C). The amount of insolubles after aging is provided in Table 1, where the control is the pellets that were not exposed to ammonium hydroxide.

[0049] Table 1

[0050] Ammonium hydroxide concentration Insoluble matter concentration after aging Reduction percentage of insoluble matter 0ppm 129ppm -- 10ppm 65ppm 60% 20ppm 60ppm 53% 46ppm 50ppm 61% 77ppm 45ppm 65% 86ppm 15ppm 88% 116ppm 45ppm 65% 131ppm 15ppm 88% 155ppm 40ppm 69%

[0051] In each case, the pellets were not tacky and were easily transported using standard methods and equipment.

[0052] These examples illustrate the use of ammonia and / or ammonium hydroxide stabilizers to maintain low concentrations of insolubles in solidified paraformaldehyde during storage and the ability to be handled and shipped by conventional means.

[0053] Therefore, the present invention is well suited to achieve the purposes and advantages mentioned and contained therein. The specific embodiments disclosed above are illustrative only, because the present invention can be modified and practiced in different but equivalent ways that are understood by those skilled in the art to have the benefits of teaching herein. In addition, it is not intended to impose restrictions on the details of construction or design shown herein, except as described in the claims below. It is therefore obvious that the specific illustrative embodiments disclosed above can be changed, combined or improved, and all such variations are considered within the scope and spirit of the present invention. The present invention disclosed illustratively herein can be suitably practiced in the absence of any elements not explicitly disclosed herein and / or any optional elements disclosed herein. Although compositions and methods are described in accordance with "including, containing or containing various components or steps", compositions and methods can also be "essentially composed of various components and steps" or "composed of various components and steps". All numbers and ranges disclosed above may have certain changes. Whenever a numerical range with a lower limit and an upper limit is disclosed, any number and any included range belonging to the range are explicitly disclosed. Specifically, each range of values ​​disclosed herein (in the form of "about a to about b", or equivalently "about a to b", or equivalently "about ab") should be understood to set forth each number and range encompassed within the broader range of values. In addition, unless otherwise expressly and clearly defined by the patentee, the terms in the claims have their ordinary and plain meanings. In addition, the indefinite articles "a" or "an" used in the claims are defined herein to mean one or more than one / one or more than one of the elements they introduce.

Claims

1. A method comprising: heating a formaldehyde solution containing 30 wt % or more formaldehyde and 50-1000 ppm ammonia and / or ammonium hydroxide stabilizer to a temperature of 70-130° C.; aging the formaldehyde solution for a period of time sufficient to allow the formaldehyde to polymerize and form paraformaldehyde; and Allow the paraformaldehyde to cure.

2. The method of claim 1, further comprising: The cured paraformaldehyde was allowed to dry.

3. The method of claim 2, further comprising: The cured paraformaldehyde during and / or after drying is exposed to a gas containing 10-1000 ppm of ammonia and / or ammonium hydroxide stabilizer.

4. The method according to claim 2 or 3, further comprising: Transport the cured paraformaldehyde to a storage facility.

5. The method of claim 4, further comprising: The cured paraformaldehyde during transport or in a storage facility is exposed to a gas containing 10-1000 ppm of ammonia and / or ammonium hydroxide stabilizer.

6. The method of claim 4, further comprising: The cured paraformaldehyde is stored at ambient temperature to 50° C. for more than 30 days and the insoluble concentration in the cured paraformaldehyde is maintained below 150 ppm.

7. The method of any one of claims 1 to 3, wherein the formaldehyde solution is aged for 0.1 to 3 hours.

8. The method of any one of claims 1 to 3, wherein the formaldehyde solution is aged at 70-130°C.

9. The method of any one of claims 1 to 3, wherein organic amines are not included in the method.

10. The method according to any one of claims 1 to 3, further comprising: Transport the cured paraformaldehyde to a storage facility.

11. The method of any one of claims 1 to 3, wherein the source of ammonia and / or ammonium hydroxide stabilizer is urea.

12. A method comprising: heating a formaldehyde solution containing 30 wt % or more of formaldehyde to a temperature of 70-130° C.; aging the formaldehyde solution in the presence of 50-1000 ppm of ammonia and / or ammonium hydroxide stabilizer for a sufficient time to polymerize the formaldehyde and form paraformaldehyde; and Allow the paraformaldehyde to cure.

13. The method of claim 12, further comprising: Allowing the cured paraformaldehyde to dry; and The cured paraformaldehyde during and / or after drying is exposed to a gas containing 10-1000 ppm of ammonia and / or ammonium hydroxide stabilizer.