A method for coating a photoresist or a protective isolation layer on a deep hole structure on a wafer
By adopting two alternating temperature and pressure control in the spraying technology, the problem of uneven coating of deep-hole wafer photoresist or protective isolation layer is solved, and uniform coating of deep-hole structure is achieved, suitable for TSV and MEMS Process.
Patent Information
- Application Number
- CN201911052497.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-10-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2039-10-31
AI Technical Summary
The existing spraying technology is difficult to achieve uniform coating of photoresist or protective isolation layers on the surface of deep hole wafers, especially at the corners, side walls and bottoms of deep holes, resulting in defects in subsequent processing processes.
Two spraying methods are adopted, by controlling the temperature and pressure, the first spraying is low temperature or low pressure, the second spraying is high temperature or high pressure, and the ultrasonic atomization nozzle or two-fluid nozzle is used for atomization to ensure photoresist or protective isolation. The layer is evenly applied at different locations.
The photoresist or protective isolation layer with deep pore structure on the wafer is uniformly applied to the top, corners, side walls and bottom, avoiding stacking and no coating, and meeting process requirements.
Smart Images

Figure CN112750756B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glue spraying in integrated circuit manufacturing wafer process, and in particular to a method for coating a deep hole structure on a wafer with a photoresist or a protective isolation layer. Background Art
[0002] The TSV process and MEMS process require the coating of photoresist or a protective isolation layer on wafers with rugged surfaces or deep holes. The photoresist or protective isolation layer needs to be coated with uniform thickness at the top, corners, sidewalls, and bottom to avoid accumulation and no coating. In the existing spraying technology, the wafer with deep holes to be processed and sprayed is placed on a rotatable and heated adsorption device. The process only uses one temperature. Since the photoresist or protective isolation layer itself is sensitive to temperature, the fluidity is different at different temperatures; or the process only uses one gas pressure. Due to the different pressures, the photoresist or protective isolation layer is sprayed at different positions in the deep holes, which will lead to problems such as the inability to evenly coat the corners, sidewalls, and bottoms of the deep holes, or even the inability to coat the photoresist and protective isolation layer, resulting in defects in the subsequent processing of the wafer and failure to meet the process requirements. Summary of the invention
[0003] In order to solve the problem that the coating thickness of photoresist or protective isolation layer at various locations of deep hole structures on existing wafers cannot be uniform, the purpose of the present invention is to provide a method for coating photoresist or protective isolation layer on deep hole structures on wafers, which method can achieve uniform coating of photoresist or protective isolation layer on the side walls, corners and bottom of the deep holes on the wafer.
[0004] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0005] A method for coating a deep hole structure on a wafer with a photoresist or a protective isolation layer is to spray the photoresist or the protective isolation layer on the wafer with the deep hole structure, using a two-time spraying method, and controlling the temperature and / or pressure during each spraying process to uniformly coat the photoresist or the protective isolation layer at different positions (top, sidewall, corner and bottom) of the deep hole on the wafer. The method specifically comprises the following steps:
[0006] (1) The wafer to be sprayed is placed on a wafer carrier with a heating device;
[0007] (2) First spraying: low temperature spraying or low pressure spraying is adopted, the temperature range of the low temperature spraying is 20-50°C, and the pressure range of the low pressure spraying is 0-1Bar;
[0008] (3) Second spraying: if the first spraying is low-temperature spraying, the second spraying is high-temperature spraying; if the first spraying is low-pressure spraying, the second spraying is high-pressure spraying; the temperature range of the high-temperature spraying is 70-150°C, and the pressure of the high-pressure spraying is greater than 1 Bar and less than or equal to 10 Bar.
[0009] During the low-temperature spraying process: the temperature of the wafer stage is set to a low-temperature range. Under the low-temperature state, the sprayed photoresist or protective isolation layer has strong fluidity and flows along the side wall of the deep hole to the bottom of the deep hole (T6), the lower corner of the deep hole (T5-1, T5-2) and the lower half of the side wall of the deep hole (T4-1, T4-2).
[0010] During the low-pressure spraying process: the gas pressure is set to a low-pressure range. Under the low-pressure state, the photoresist or protective isolation layer is sprayed with a small force and a short stroke, and adheres to the top (T1-2, T1-1) of the deep hole, the upper corner (T2-1, T2-2) and the upper half of the side wall (T3-1, T3-2).
[0011] After the first low-temperature spraying, the wafer stage is rotated 0-180° and then high-temperature spraying is performed; the wafer stage temperature is set to high temperature. Under high temperature conditions, the sprayed photoresist or protective isolation layer has poor fluidity and is coated on the top of the deep hole (T1-1, T1-2), the upper corner of the deep hole (T2-1, T2-2) and the upper half of the deep hole side wall (T3-1, T3-2).
[0012] After the first low-pressure spraying, the wafer stage is rotated 0-180° and then high-pressure spraying is performed; the gas pressure is set to high pressure. Under high pressure, the photoresist or protective isolation layer is sprayed with great force and large stroke, and adheres to the bottom of the deep hole (T6), the lower corner (T5-1, T5-2) and the lower half of the side wall (T4-1, T4-2).
[0013] The pressure during the low-temperature spraying and high-temperature spraying is 0-10 bar; the temperature during the low-pressure spraying and high-pressure spraying is 30-150°C.
[0014] The depth-to-width ratio of the deep hole structure is 1:1-5:1.
[0015] During the spraying process of the above steps (2) and (3), the photoresist or protective isolation layer to be sprayed is atomized by an ultrasonic atomization nozzle or a two-fluid nozzle, and the atomized droplets are accelerated to spray toward the wafer surface under the action of pressurized gas to form a photoresist film or a protective isolation layer.
[0016] During the spraying process of the above-mentioned step (2) and step (3), the coating results are complementary under the action of two different temperatures or pressures. The photoresist or protective isolation layer reaches the top (T1-1, T1-2) of the deep hole, the upper corner (T2-1, T2-2), the side wall (T3-1, T3-2, T4-1, T4-2), the lower corner (T5-1, T5-2) and the bottom (T6). The coating thickness at each point is uniform and consistent, avoiding accumulation and no coating.
[0017] The advantages and beneficial effects of the present invention are:
[0018] 1. The present invention does not change the original coating equipment, but only improves the process results by adjusting the process method, thus saving the equipment modification cost.
[0019] 2. The present invention is simple to debug. It can solve the existing problems such as uneven deep hole coating and meet the process requirements by simply alternating multiple temperatures or multiple gas pressures.
[0020] 3. The present invention realizes uniform coating of photoresist or protective isolation layer on the sidewall, corner and bottom of the deep hole of the wafer with deep hole. The method of the present invention is applicable to TSV (Through Silicon Via) process, MEMS (Micro Electro Mechanical System) process, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a schematic diagram of different positions T1-T5 of the deep hole structure on the wafer. DETAILED DESCRIPTION
[0022] The present invention is described in detail below with reference to the accompanying drawings and embodiments.
[0023] The present invention provides a method for coating a photoresist or a protective isolation layer on a deep hole structure on a wafer. The schematic diagram of different positions of the deep hole structure on the wafer targeted by the method is as follows: Figure 1 As shown, the positions are respectively the top T1 (including T1-1, T1-2) of the deep hole, the upper corner T2 (including T2-1, T2-2), the side wall T3 and T4 (including T3-1, T3-2, T4-1, T4-2), the lower corner T5 (including T5-1, T5-2) and the bottom (T6). The method adopts a spraying method of alternating multiple process temperatures (low temperature-high temperature, high temperature-low temperature or low temperature-high temperature-low temperature) or alternating multiple gas pressures (low pressure-high pressure, high pressure-low pressure or low pressure-high pressure-low pressure), so that multiple process temperatures or pressures are alternately carried out, and the coating results are complementary, so that the photoresist or protective isolation layer reaches the top (T1) of the deep hole, the upper corner (T2), the side wall (T3, T4), the lower corner (T5,) and the bottom (T6) of the deep hole. The thickness is uniform and consistent, avoiding accumulation and no coating.
[0024] The spraying process is as follows: the wafer to be processed is placed on a wafer carrier equipped with a heating device, and an ultrasonic atomizing nozzle or a two-fluid nozzle is used to ultra-finely atomize the photoresist or protective isolation layer. The atomized liquid particles are accelerated and sprayed onto the wafer surface under the action of pressurized gas.
[0025] In the following embodiments, when the low-temperature spraying-high-temperature spraying process is adopted, the pressure range is 0-10 bar, and when the low-pressure spraying-high-pressure spraying process is adopted, the temperature range is 30-150 degrees.
[0026] After the first spraying, rotate the wafer table 0-180° before spraying for the second time.
[0027] Example 1
[0028] In this embodiment, the deep hole size is 100 μm deep, 30 μm wide, and the angle at the corner is 90°. The coating chemical is a photoresist with a CP value of 420 cp. During the first coating, the stage temperature is set to 40°. After the S-shaped spraying of the photoresist, the stage is rotated 90°. During the second coating, the stage temperature is set to 90°. Spraying is completed.
[0029] After coating, the deep hole wafer was split, and the morphology and film thickness of the sample cross section were detected by SEM. The morphology detection showed that the coating thickness at the top (T1), upper corner (T2), side wall (T3, T4), lower corner (T5,) and bottom (T6) of the deep hole was uniform, avoiding accumulation and no coating. The film thickness at T1, T2, T3, T4, and T5 was 10±1μm, and the non-uniformity was ±5%.
[0030] Example 2
[0031] In this embodiment, the deep hole size is 120 μm deep, 20 μm wide, and the corner angle is 75°. The coating chemical is a photoresist with a CP value of 1000 cp. During the first coating, the gas pressure is set to 0.1 bar. After the S-shaped spraying of the photoresist, the wafer stage is rotated 90°. During the second coating, the gas pressure is set to 3.5 bar. Spraying is completed.
[0032] After coating, the deep hole wafer was split, and the morphology and film thickness of the sample cross section were detected by SEM. The morphology detection showed that the coating thickness at the top (T1), upper corner (T2), side wall (T3, T4), lower corner (T5,) and bottom (T6) of the deep hole was uniform, avoiding accumulation and no coating. The film thickness at T1, T2, T3, T4, and T5 was 5 + 1 μm, and the non-uniformity was ± 10%.
[0033] Example 3
[0034] In this embodiment, the deep hole size is 150 μm deep, 30 μm wide, and the corner angle is 75°. The coating chemical is a photoresist with a CP value of 1000 cp. During the first coating, the stage temperature is set to 30° and the gas pressure is set to 0.3 bar. After the S-shaped spraying of the photoresist, the stage is rotated 90°. During the second coating, the stage temperature is set to 120° and the gas pressure is set to 5.0 bar. Spraying is completed.
[0035] After coating, the deep hole wafer was split, and the morphology and film thickness of the sample cross section were detected by SEM. The morphology detection showed that the coating thickness at the top (T1), upper corner (T2), side wall (T3, T4), lower corner (T5,) and bottom (T6) of the deep hole was uniform, avoiding accumulation and no coating. The film thickness at T1, T2, T3, T4, and T5 was 3 + 1 μm, and the non-uniformity was ± 16.7%.
[0036] The implementation results show that, in the process of spraying photoresist or protective isolation layer on wafers with deep holes, the present invention adopts alternating process temperature (low temperature-high temperature) or alternating gas pressure (low pressure-high pressure) to achieve uniform coating of photoresist or protective isolation layer on the side walls, corners and bottom of the deep holes of the wafer with deep holes.
Claims
1. A method for coating a photoresist on a deep hole structure on a wafer, characterized in that: The method is to spray photoresist on a wafer with a deep hole structure, using a two-time spraying method, and controlling the temperature and / or pressure during each spraying process to uniformly coat the photoresist at different positions of the deep hole on the wafer; The method specifically comprises the following steps: (1) The wafer to be sprayed is placed on a wafer carrier with a heating device; (2) First spraying: low temperature spraying or low pressure spraying is adopted, the temperature range of the low temperature spraying is 20-50°C, and the pressure range of the low pressure spraying is 0-1 Bar; (3) Second spraying: when the first spraying is low-temperature spraying, the second spraying is high-temperature spraying; when the first spraying is low-pressure spraying, the second spraying is high-pressure spraying; the temperature range of the high-temperature spraying is 70-150°C, and the pressure of the high-pressure spraying is greater than 1 Bar and less than or equal to 10 Bar; During the low-temperature spraying process: the temperature of the wafer stage is set to a low-temperature range. Under the low-temperature state, the sprayed photoresist has strong fluidity and flows along the side wall of the deep hole to the bottom of the deep hole, the lower corner of the deep hole and the lower half of the side wall of the deep hole; During the low-pressure spraying process: the gas pressure is set to a low-pressure range. Under the low-pressure state, the photoresist spraying force is small and the stroke is short, and the photoresist adheres to the top of the deep hole, the upper corner and the upper half of the side wall; After the first low-temperature spraying, the wafer stage is rotated 0-180° and then high-temperature spraying is performed; The temperature of the wafer stage is set to high temperature. Under high temperature, the sprayed photoresist has poor fluidity and is coated on the top of the deep hole, the upper corner of the deep hole and the upper half of the side wall of the deep hole; After the first low-pressure spraying, the wafer stage is rotated 0-180° and then high-pressure spraying is performed; the gas pressure is set to high pressure. Under high pressure, the photoresist is sprayed with great force and a large stroke, and adheres to the bottom of the deep hole, the lower corner and the lower half of the side wall.
2. The method for coating a photoresist on a deep hole structure on a wafer according to claim 1, characterized in that: The pressure during the low-temperature spraying and high-temperature spraying is 0-10 bar; the temperature during the low-pressure spraying and high-pressure spraying is 30-150°C.
3. The method for coating a photoresist on a deep hole structure on a wafer according to claim 1, characterized in that: The depth-to-width ratio of the deep hole structure is 1:1-5:
1.
4. The method for coating a photoresist on a deep hole structure on a wafer according to claim 1, characterized in that: During the spraying process of step (2) and step (3), the photoresist to be sprayed is atomized by an ultrasonic atomizing nozzle or a two-fluid nozzle, and the atomized droplets are accelerated to spray toward the wafer surface under the action of pressurized gas to form a photoresist film.
5. The method for coating a deep hole structure on a wafer with a photoresist according to claim 4, characterized in that: During the spraying process of step (2) and step (3), the coating results are complementary under the action of two different temperatures or pressures, and the photoresist reaches the top, upper corner, side wall, lower corner and bottom of the deep hole. The coating thickness at each point is uniform and consistent, avoiding accumulation and no coating.