Composition for forming a silicon-containing EUV resist underlayer film containing onium sulfonate
By using a hydrolyzable organosilane and a hydrocarbonyl sulfonate ion-containing composition as a resist lower film in semiconductor manufacturing, the problem of insufficient fineness and adhesion of the resist pattern in EUV lithography is solved, and dry etching is improved Speed and pattern transfer effect.
Patent Information
- Application Number
- CN202110148440.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2013-07-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2033-07-29
AI Technical Summary
In the manufacturing of semiconductor devices, it is difficult for the prior art to effectively control the fineness and adhesion of the resist pattern during EUV lithography, and the dry etching speed of the resist underlayer film is insufficient, which affects the pattern transfer effect.
The composition containing hydrolyzable organosilane and hydrocarbyl sulfonate ions is used as the composition for forming the resist underlayer film. By selecting appropriate etching gas and baking conditions, the acidity and dry etching speed of the resist underlayer film are adjusted. Improve the adhesion and pattern transfer performance of resist and photoresist.
It is achieved to improve the fineness and adhesion of the resist pattern during EUV lithography, enhance the dry etching speed, and ensure the quality and accuracy of pattern transfer.
Smart Images

Figure CN112947000B_ABST
Abstract
Description
[0001] This application is filed on July 29, 2013, with application number 201380029266.2 and invention name “Containing sulfonic acid” A divisional application of a patent application for "a composition for forming an EUV resist underlayer film containing silicon salt". Technical Field
[0002] The present invention relates to a composition for forming an underlayer film between a substrate and a resist (e.g., an EUV resist) used in the manufacture of a semiconductor device. Specifically, the present invention relates to a resist underlayer film forming composition for lithography used to form an underlayer film used as an underlayer of a resist in a lithography process for the manufacture of a semiconductor device. In addition, the present invention relates to a method for forming a resist pattern using the underlayer film forming composition. Background Art
[0003] Until now, micro-machining has been performed by photolithography using photoresists in the manufacture of semiconductor devices. The micro-machining is a method of forming a thin film of photoresist on a semiconductor substrate such as a silicon wafer, irradiating it with active light such as ultraviolet rays through a mask pattern depicting a semiconductor device pattern, developing it, and etching the substrate using the obtained photoresist pattern as a protective film, thereby forming micro-concavities and convexities corresponding to the above-mentioned pattern on the surface of the substrate. However, in recent years, with the progress of high integration of semiconductor devices, the active light used has also tended to be shorter in wavelength from KrF excimer laser (248nm) to ArF excimer laser (193nm) and EUV light (13.5nm).
[0004] Therefore, it is more necessary to control the pattern (resist shape) and improve the adhesion with the substrate.
[0005] In addition, as a lower film between the semiconductor substrate and the photoresist, a film known as a hard mask containing metal elements such as silicon is used. In this case, since the resist and the hard mask have large differences in their constituent components, the speed at which they are removed by dry etching depends largely on the type of gas used in the dry etching. Moreover, by appropriately selecting the type of gas, the hard mask can be removed by dry etching without causing a significant reduction in the film thickness of the photoresist. In this way, in the manufacture of semiconductor devices in recent years, in order to achieve various effects, a resist lower film is arranged between the semiconductor substrate and the photoresist (see Patent Documents 1 and 2).
[0006] Furthermore, studies on compositions for resist underlayer films have been conducted so far, but development of new materials for resist underlayer films has been desired in view of the diversity of properties required thereof.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 2008-076889
[0010] Patent Document 2: Japanese Patent Application Laid-Open No. 2010-237667 Summary of the invention
[0011] Problems to be solved by the invention
[0012] The object of the present invention is to provide a resist underlayer film-forming composition for EUV lithography that can be used for manufacturing semiconductor devices by using a rectangular resist pattern to perform fine substrate processing. Specifically, a resist underlayer film-forming composition for lithography that is used to form a resist underlayer film that can be used as a hard mask is provided. In addition, a resist underlayer film-forming composition that has improved exposure sensitivity of EUV resist, does not mix with resist, and has a higher dry etching rate than resist is provided.
[0013] Methods for solving problems
[0014] In the present invention, as a first aspect, there is provided a resist underlayer film-forming composition for EUV lithography, comprising a hydrolyzable organosilane as a silane, a hydrolyzate thereof or a hydrolysis-condensation product thereof, and further comprising a sulfonate ion containing a hydrocarbon group and Ionic salts,
[0015] As a second aspect, in the resist underlayer film-forming composition according to the first aspect, the hydrolyzable organosilane comprises at least one organosilicon compound selected from the group consisting of formula (1) and formula (2), a hydrolyzate thereof, or a hydrolysis-condensation product thereof;
[0016] R 1 a Si(R 2 ) 4-a Formula (1)
[0017] (In formula (1), R 1 Indicates that the sulfonate ion containing hydrocarbon group and ion salt, alkyl, aryl, aralkyl, halogenated alkyl, halogenated aryl, halogenated aralkyl or alkenyl, or an organic group having an epoxy group, an acryloyl group, a methacryloyl group, a mercapto group, an alkoxyaryl group, an acyloxyaryl group, an isocyanurate group, a hydroxyl group, a cyclic amino group or a cyano group and bonded to a silicon atom via a Si-C bond, or a combination thereof, R 2 represents an alkoxy group, an acyloxy group or a halogen group, and a represents an integer of 0 to 3. ),
[0018] 〔R 3 c Si(R 4 )3-c 〕2Y b Formula (2)
[0019] (In formula (2), R 3 represents an alkyl group, R 4 represents an alkoxy group, an acyloxy group or a halogen group, Y represents an alkylene group or an arylene group, b represents an integer of 0 or 1, and c represents an integer of 0 or 1. ),
[0020] According to a third aspect, the resist underlayer film-forming composition according to the first aspect or the second aspect comprises a hydrolysis-condensation product of the compound represented by the above formula (1) as a polymer.
[0021] According to a fourth aspect, the resist underlayer film forming composition according to any one of the first aspect to the third aspect is provided, The ion is a sulfonium ion or an ammonium ion,
[0022] According to a fifth aspect, the resist underlayer film forming composition according to any one of the first aspect to the fourth aspect is provided, The ion is an organic group containing at least one aromatic ring. ion,
[0023] According to a sixth aspect, in the resist underlayer film forming composition according to any one of the first aspect to the fifth aspect, the hydrocarbon group-containing sulfonate ion is a sulfonate ion having a hydrocarbon group which may be partially substituted,
[0024] According to a seventh aspect, the resist underlayer film forming composition according to any one of the first aspect to the sixth aspect further contains an acid.
[0025] According to an eighth aspect, the resist underlayer film forming composition according to any one of the first aspect to the seventh aspect further contains water.
[0026] As a ninth aspect, a composition for forming a resist underlayer film for EUV lithography comprises a hydrolyzable organosilane as a silane, a hydrolyzate thereof, or a hydrolysis-condensation product thereof, wherein the hydrolyzable organosilane is an organosilicon compound represented by formula (2),
[0027] 〔R 3 c Si(R 4 ) 3-c 〕2Y b Formula (2)
[0028] (In formula (2), R 3 represents an alkyl group, R 4 represents an alkoxy group, an acyloxy group or a halogen group, Y represents an alkylene group or an arylene group, b represents an integer of 0 or 1, and c represents an integer of 0 or 1. ),
[0029] As a tenth aspect, the resist underlayer film forming composition according to the ninth aspect further comprises an acid,
[0030] According to an eleventh aspect, the resist underlayer film forming composition according to the ninth aspect or the tenth aspect further comprises water.
[0031] As a twelfth aspect, a resist underlayer film is obtained by applying the resist underlayer film-forming composition according to any one of the first aspect to the eleventh aspect onto a semiconductor substrate and baking the coating.
[0032] As a 13th aspect, a method for manufacturing a semiconductor device comprises the following steps: a step of applying the resist underlayer film forming composition described in any one of the 1st aspect to the 11th aspect on a semiconductor substrate and baking it to form a resist underlayer film; a step of applying an EUV resist composition on the above-mentioned underlayer film to form a resist film; a step of subjecting the above-mentioned resist film to EUV exposure; a step of developing the resist film after exposure to obtain a resist pattern; a step of etching the resist underlayer film using the resist pattern; and a step of processing the semiconductor substrate using the patterned resist film and the resist underlayer film, and
[0033] As a 14th aspect, a method for manufacturing a semiconductor device includes the following steps: a step of forming an organic lower layer film on a semiconductor substrate; a step of coating the composition for forming an anti-etching lower layer film described in any one of the first aspect to the 11th aspect on the organic lower layer film, and baking it to form a resist lower layer film; a step of coating an EUV resist composition on the above-mentioned resist lower layer film to form a resist film; a step of exposing the above-mentioned resist film to EUV; a step of developing the resist film after exposure to obtain a resist pattern; a step of etching the resist lower layer film using the resist pattern; a step of etching the organic lower layer film using the patterned resist lower layer film; and a step of processing the semiconductor substrate using the patterned organic lower layer film.
[0034] Effects of the Invention
[0035] In the present invention, a resist underlayer film is formed on a substrate by a coating method, or a resist underlayer film is formed on an organic underlayer film on the substrate by a coating method, and a resist film (e.g., EUV resist) is formed on the resist underlayer film. Then, a resist pattern is formed by exposure and development, and the resist underlayer film is dry-etched using the resist pattern to transfer the pattern, and the substrate is processed using the pattern, or the organic underlayer film is etched to transfer the pattern, and the substrate is processed using the organic underlayer film.
[0036] In forming fine patterns, the thickness of the resist film tends to be thinned in order to prevent the pattern from collapsing. Due to the thin film of the resist, if the etching rate of the dry etching used to transfer the pattern to the film present in the lower layer is not higher than that of the upper film, the pattern transfer cannot be performed. In the present invention, the resist lower film of the present invention (containing an inorganic silicon compound) is sequentially coated thereon with or without an organic lower film on the substrate, and a resist film (organic resist film) is coated thereon. By selecting the etching gas, the dry etching rate of the film of the organic component and the film of the inorganic component is greatly different. The dry etching rate of the film of the organic component is high when in an oxygen-based gas, and the dry etching rate of the film of the inorganic component is high when in a halogen-containing gas.
[0037] For example, a resist pattern is formed, and the resist underlayer film of the present invention present in the lower layer is dry-etched with a halogen-containing gas, the pattern is transferred to the resist underlayer film, and the substrate is processed using the pattern transferred to the resist underlayer film using the halogen-containing gas. Alternatively, the resist underlayer film to which the pattern is transferred is used to dry-etch the organic underlayer film under it with an oxygen-based gas, the pattern is transferred to the organic underlayer film, and the substrate is processed using the halogen-containing gas using the organic underlayer film to which the pattern is transferred.
[0038] In order to adjust the resist shape, it is important to control the acidity of the silicon-containing resist underlayer film. In the present invention, as a method for adjusting the acidity of the silicon-containing resist underlayer film, it was found that a sulfonic acid is added to the silicon-containing resist underlayer film. Salts are effective. The sulfonic acid salt can reduce the acidity in the area where the acid in the photoresist is excessive, and can improve the adhesion between the silicon-containing resist underlayer film and the photoresist. On the other hand, in the area where the acid in the photoresist is insufficient, the sulfonic acid The salt eliminates the effect of the alkaline component in the photoresist, thereby improving the resolution of the photoresist. Salts provide a silicon-containing resist underlayer film having a so-called buffering function for controlling acidity, and can adjust the resist shape.
[0039] Furthermore, by containing the compound of formula (2) used in the present invention, the cured film can be densified and the hard mask property can be improved. DETAILED DESCRIPTION
[0040] The present invention is a hydrolyzable organosilane as a silane, a hydrolyzate thereof or a hydrolysis-condensation product thereof, and a sulfonate ion containing a hydrocarbon group and A resist underlayer film-forming composition for EUV lithography comprising a salt of an ion.
[0041] The resist underlayer film-forming composition of the present invention may contain a hydrolyzable organosilane, a hydrolyzate thereof, or a hydrolysis-condensation product thereof as a silane, and may further contain a sulfonate ion containing a hydrocarbon group and The present invention further includes salts of ions and acids, water, alcohols, curing catalysts, acid generators, other organic polymers, light absorbing compounds, surfactants, and the like as arbitrary components.
[0042] The solid content in the resist underlayer film forming composition of the present invention is, for example, 0.1 to 50 mass %, or 0.1 to 30 mass %, or 0.1 to 25 mass %. The solid content here refers to the components obtained by removing the solvent component from all the components of the resist underlayer film forming composition.
[0043] The proportion of silane (hydrolyzable silane, its hydrolyzate and its hydrolysis-condensate) in the solid content is 20% by mass or more, for example, 50 to 99.9% by mass, or 60 to 99.9% by mass, or 70 to 99.0% by mass.
[0044] Moreover, the sulfonate ions containing hydrocarbon groups The content of the ionic salt in the solid content is, for example, 0.1 to 10% by mass, or 0.1 to 5% by mass.
[0045] The hydrolyzable organosilane includes at least one organosilicon compound selected from the group consisting of formula (1) and formula (2), and a hydrolyzate or a hydrolysis-condensation product thereof.
[0046] In formula (1), R 1 Indicates that the sulfonate ion containing hydrocarbon group and ion salt, alkyl, aryl, aralkyl, halogenated alkyl, halogenated aryl, halogenated aralkyl or alkenyl, or an organic group having an epoxy group, an acryloyl group, a methacryloyl group, a mercapto group, an alkoxyaryl group, an acyloxyaryl group, an isocyanurate group, a hydroxyl group, a cyclic amino group or a cyano group and bonded to a silicon atom via a Si-C bond, or a combination thereof, R 2 represents an alkoxy group, an acyloxy group or a halogen group, and a represents an integer of 0 to 3.
[0047] The alkyl group is a linear or branched alkyl group having 1 to 10 carbon atoms, and examples thereof include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, 1-methyl-n-butyl, 2-methyl-n-butyl, 3-methyl-n-butyl, 1,1-dimethyl-n-propyl, 1,2-dimethyl-n-propyl, 2,2-dimethyl-n-propyl, 1-ethyl-n-propyl, n-hexyl, 1-methyl-n-pentyl, 2-methyl-n-pentyl, 3-methyl-n-butyl, The invention relates to 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1-dimethyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl and 1-ethyl-2-methyl-n-propyl, etc. In addition, a cyclic alkyl group can be used. Examples of the cyclic alkyl group having 1 to 10 carbon atoms include cyclopropyl, cyclobutyl, 1-methyl-cyclopropyl, 2-methyl-cyclopropyl, cyclopentyl, 1-methyl-cyclobutyl, 2-methyl-cyclobutyl, 3-methyl-cyclobutyl, 1,2-dimethyl-cyclopropyl, 2,3-dimethyl-cyclopropyl, 1-ethyl-cyclopropyl, 2-ethyl-cyclopropyl, cyclohexyl, 1-methyl-cyclopentyl, 2-methyl-cyclopentyl, 3-methyl-cyclopentyl, 1-ethyl-cyclobutyl, 2-ethyl-cyclobutyl, 3-ethyl-cyclobutyl, 1,2-dimethyl-cyclobutyl cyclopropyl, 1-ethyl-2-methyl-cyclopropyl, 2-ethyl-1-methyl-cyclopropyl, 2-ethyl-2-methyl-cyclopropyl and 2-ethyl-3-methyl-cyclopropyl, etc.
[0048] Examples of the aryl group include aryl groups having 6 to 20 carbon atoms, such as phenyl, o-methylphenyl, m-methylphenyl, p-methylphenyl, o-chlorophenyl, m-chlorophenyl, p-chlorophenyl, o-fluorophenyl, p-mercaptophenyl, o-methoxyphenyl, p-methoxyphenyl, p-aminophenyl, p-cyanophenyl, α-naphthyl, β-naphthyl, o-biphenyl, m-biphenyl, p-biphenyl, 1-anthryl, 2-anthryl, 9-anthryl, 1-phenanthryl, 2-phenanthryl, 3-phenanthryl, 4-phenanthryl and 9-phenanthryl.
[0049] Examples of the alkenyl group include alkenyl groups having 2 to 10 carbon atoms, such as vinyl, 1-propenyl, 2-propenyl, 1-methyl-1-vinyl, 1-butenyl, 2-butenyl, 3-butenyl, 2-methyl-1-propenyl, 2-methyl-2-propenyl, 1-ethylvinyl, 1-methyl-1-propenyl, 1-methyl-2-propenyl, 1-pentenyl, 2-pentenyl, 3-pentenyl, 4-pentenyl, 1-n-propylvinyl, 1-methyl-1-butenyl, 1-methyl-2-butenyl, 1-methyl-3-butenyl, 2-ethyl-2-propenyl, 2-methyl-1-butenyl, 2-methyl-2-butenyl, 2-methyl 1-butylene, 2-methyl-1-pentenyl, 2-methyl-2-pentenyl, 2-methyl-3-pentenyl, 1-methyl-4-pentenyl, 1-butylene, 2-methyl-1-pentenyl, 2-methyl-2-pentenyl, 2-methyl-3-pentenyl, 1-methyl-2-pentenyl, 1-methyl-3-pentenyl, 1-methyl-4-pentenyl, 1-butylene, 2-methyl-1-pentenyl, 2-methyl-2-pentenyl, 2-methyl-3-pentenyl, 1-methyl-3-pentenyl, 1-methyl-4-pentenyl, 1-butylene, 2-methyl-1-pentenyl, 2-methyl-2-pentenyl, 2-methyl-3-pentenyl, 1-methyl-3-pentenyl, 1-methyl-4-pentenyl, 1-butylene, 2-methyl-1-pentenyl, 2-methyl-2-pentenyl, 2-methyl-3-pentenyl, 1-methyl-3-pentenyl, 1-methyl-4-pentenyl, 1-butylene 4-Methyl-3-pentenyl, 4-methyl-4-pentenyl, 1,1-dimethyl-2-butenyl, 1,1-dimethyl-3-butenyl, 1,2-dimethyl-1-butenyl, 1,2-dimethyl-2-butenyl, 1,2-dimethyl-3-butenyl, 1-methyl-2-ethyl-2-propenyl, 1-sec-butylvinyl, 1, 3-Dimethyl-1-butenyl, 1,3-dimethyl-2-butenyl, 1,3-dimethyl-3-butenyl, 1-isobutyl vinyl, 2,2-dimethyl-3-butenyl, 2,3-dimethyl-1-butenyl, 2,3-dimethyl-2-butenyl, 2,3-dimethyl-3-butenyl, 2-isopropyl-2-propenyl, 3,3-dimethyl-1-butenyl, 1-ethyl-1-butenyl, 1-ethyl-2-butenyl, 1-ethyl-3-butenyl, 1-n-propyl-1-propenyl, 1-n-propyl-2-propenyl, 2-ethyl-1-butenyl, 2-ethyl-2-butenyl, 2-ethyl-3-butenyl, 1,1,2-Trimethyl-2-propenyl, 1-tert-butylvinyl, 1-methyl-1-ethyl-2-propenyl, 1-ethyl-2-methyl-1-propenyl, 1-ethyl-2-methyl-2-propenyl, 1-isopropyl-1-propenyl, 1-isopropyl-2-propenyl, 1-methyl-2-cyclopentenyl, 1-methyl-3-cyclopentenyl, 2-methyl-1-cyclopentenyl, 2-methyl-2-cyclopentenyl cyclopentenyl, 2-methyl-3-cyclopentenyl, 2-methyl-4-cyclopentenyl, 2-methyl-5-cyclopentenyl, 2-methylene-cyclopentyl, 3-methyl-1-cyclopentenyl, 3-methyl-2-cyclopentenyl, 3-methyl-3-cyclopentenyl, 3-methyl-4-cyclopentenyl, 3-methyl-5-cyclopentenyl, 3-methylene-cyclopentyl, 1-cyclohexenyl, 2-cyclohexenyl and 3-cyclohexenyl, etc.
[0050] The aralkyl group is an alkyl group substituted with an aryl group, and examples thereof include an alkyl group having 1 to 10 carbon atoms substituted with a phenyl group. Specific examples thereof include a benzyl group, an ethylphenyl group, a propylphenyl group, and a butylphenyl group.
[0051] Examples of the halogenated alkyl group, halogenated aryl group and halogenated aralkyl group include organic groups in which these groups are substituted with a halogen atom such as fluorine, chlorine, bromine or iodine.
[0052] Examples of the organic group having an epoxy group include a glycidoxymethyl group, a glycidoxyethyl group, a glycidoxypropyl group, a glycidoxybutyl group, and an epoxycyclohexyl group.
[0053] Examples of the organic group having an acryloyl group include an acryloylmethyl group, an acryloylethyl group, and an acryloylpropyl group.
[0054] Examples of the organic group having a methacryloyl group include a methacryloylmethyl group, a methacryloylethyl group, and a methacryloylpropyl group.
[0055] Examples of the organic group having a mercapto group include ethylmercapto, butylmercapto, hexylmercapto, and octylmercapto.
[0056] The organic group having an alkoxyaryl group is an aryl group substituted with an alkoxy group or an organic group having these aryl groups. Examples of these alkoxy groups and aryl groups include the above-mentioned and the following groups.
[0057] The organic group having an acyloxyaryl group is an aryl group substituted with an acyloxy group or an organic group having these aryl groups. Examples of these acyloxy groups and aryl groups include the above-mentioned and the following groups.
[0058] Examples of the organic group having an isocyanurate group include an isocyanurate group and an alkylene cyanurate group, and examples of the alkylene group include groups corresponding to the above-mentioned alkyl groups. The isocyanurate group may be substituted with an alkenyl group such as an allyl group, an epoxy-containing group such as a glycidyl group, an alkyl group, or the like.
[0059] Examples of the organic group having a hydroxyl group include a hydroxyl group, a hydroxyalkyl group, and a hydroxyalkylene group. Examples of the alkyl group include the above-mentioned groups, and examples of the alkylene group include groups corresponding to the alkyl group.
[0060] As an organic group having a cyclic amino group, a cyclic amino group or a cyclic aminoalkylene group can be mentioned. As a cyclic amino group, an imidazolyl group, a 4,5-dihydroimidazolyl group, etc. can be mentioned. The cyclic aminoalkylene group can be exemplified by a group corresponding to the above-mentioned alkyl group. For example, a propylimidazolyl group, a propyl-4,5-dihydroimidazolyl group, etc. can be mentioned. These can be used as cyclic amine compounds.
[0061] Examples of the organic group having a cyano group include a cyanoethyl group and a cyanopropyl group.
[0062] Examples of the alkoxy group include alkoxy groups having a linear, branched, or cyclic alkyl moiety having 1 to 20 carbon atoms, such as a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, an n-pentoxy group, a 1-methyl-n-butoxy group, a 2-methyl-n-butoxy group, a 3-methyl-n-butoxy group, a 1,1-dimethyl-n-propoxy group, a 1,2-dimethyl-n-propoxy group, a 2,2-dimethyl-n-propoxy group, a 1-ethyl-n-propoxy group, an n-hexyloxy group, a 1-methyl-n-pentoxy group, a 2-methyl-n-pentoxy group, a 3-methyl-n-pentoxy group, Examples of the cyclic alkoxy group include cyclopropyloxy, cyclobutyloxy, cyclohexyl ... -methyl-cyclopropyloxy, 2-methyl-cyclopropyloxy, cyclopentyloxy, 1-methyl-cyclobutyloxy, 2-methyl-cyclobutyloxy, 3-methyl-cyclobutyloxy, 1,2-dimethyl-cyclopropyloxy, 2,3-dimethyl-cyclopropyloxy, 1-ethyl-cyclopropyloxy, 2-ethyl-cyclopropyloxy, cyclohexyloxy, 1-methyl-cyclopentyloxy, 2-methyl-cyclopentyloxy, 3-methyl-cyclopentyloxy, 1-ethyl-cyclobutyloxy, 2-ethyl-cyclobutyloxy, 3-ethyl-cyclobutyloxy, 1,2-dimethyl-cyclobutyloxy, 1,3-dimethyl-cyclobutyloxy, 2,2-dimethyl-cyclopropyloxy, Methyl-cyclobutyloxy, 2,3-dimethyl-cyclobutyloxy, 2,4-dimethyl-cyclobutyloxy, 3,3-dimethyl-cyclobutyloxy, 1-n-propyl-cyclopropyloxy, 2-n-propyl-cyclopropyloxy, 1-isopropyl-cyclopropyloxy, 2-isopropyl-cyclopropyloxy, 1,2,2-trimethyl-cyclopropyloxy, 1,2,3-trimethyl-cyclopropyloxy, 2,2,3-trimethyl-cyclopropyloxy, 1-ethyl-2-methyl-cyclopropyloxy, 2-ethyl-1-methyl-cyclopropyloxy, 2-ethyl-2-methyl-cyclopropyloxy and 2-ethyl-3-methyl-cyclopropyloxy, etc.
[0063] Examples of the acyloxy group include acyloxy groups having 2 to 20 carbon atoms, such as methylcarbonyloxy, ethylcarbonyloxy, n-propylcarbonyloxy, isopropylcarbonyloxy, n-butylcarbonyloxy, isobutylcarbonyloxy, sec-butylcarbonyloxy, tert-butylcarbonyloxy, n-pentylcarbonyloxy, 1-methyl-n-butylcarbonyloxy, 2-methyl-n-butylcarbonyloxy, 3-methyl-n-butylcarbonyloxy, 1,1-dimethyl-n-propylcarbonyloxy, 1,2-dimethyl-n-propylcarbonyloxy, 2,2-dimethyl-n-propylcarbonyloxy, 1-ethyl-n-propylcarbonyloxy, n-hexylcarbonyloxy, 1-methyl-n-pentylcarbonyloxy, 2-methyl-n-pentylcarbonyloxy, 3-methyl- n-Pentylcarbonyloxy, 4-methyl-n-pentylcarbonyloxy, 1,1-dimethyl-n-butylcarbonyloxy, 1,2-dimethyl-n-butylcarbonyloxy, 1,3-dimethyl-n-butylcarbonyloxy, 2,2-dimethyl-n-butylcarbonyloxy, 2,3-dimethyl-n-butylcarbonyloxy, 3,3-dimethyl-n-butylcarbonyloxy, 1-ethyl-n-butylcarbonyloxy, 2-ethyl-n-butylcarbonyloxy, 1,1,2-trimethyl-n-propylcarbonyloxy, 1,2,2-trimethyl-n-propylcarbonyloxy, 1-ethyl-1-methyl-n-propylcarbonyloxy, 1-ethyl-2-methyl-n-propylcarbonyloxy, phenylcarbonyloxy and tosylcarbonyloxy, etc.
[0064] Examples of the halogen group include fluorine, chlorine, bromine, and iodine.
[0065] The hydrolyzable organosilane represented by formula (1) includes, for example, tetramethoxysilane, tetrachlorosilane, tetraacetoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetraisopropoxysilane, tetra-n-butoxysilane, tetraacetoxysilane, methyltrimethoxysilane, methyltriethoxysilane, methyltrichlorosilane, methyltriacetoxysilane, methyltripropoxysilane, methyltriacetoxysilane, methyltributoxysilane, methyltripropoxysilane, methyltripentoxysilane, methyltriphenoxysilane, methyltripenyloxysilane, methyltriphenethoxysilane, cyclopentyloxysilane, methyltriphenyloxysilane, methyltriphenylethoxysilane, methyltriphen ... α-Glycidoxymethyl trimethoxysilane, glycidoxymethyl triethoxysilane, α-glycidoxyethyl trimethoxysilane, α-glycidoxyethyl triethoxysilane, β-glycidoxyethyl trimethoxysilane, β-glycidoxyethyl triethoxysilane, α-glycidoxypropyl trimethoxysilane, α-glycidoxypropyl triethoxysilane, β-glycidoxypropyl trimethoxysilane, β-glycidoxypropyl triethoxysilane, γ-glycidoxypropyl trimethoxysilane, γ-glycidoxypropyl triethoxysilane, γ- Glycidoxypropyl tripropoxysilane, γ-glycidoxypropyl tributoxysilane, γ-glycidoxypropyl triphenoxysilane, α-glycidoxybutyl trimethoxysilane, α-glycidoxybutyl triethoxysilane, β-glycidoxybutyl triethoxysilane, γ-glycidoxybutyl trimethoxysilane, γ-glycidoxybutyl triethoxysilane, δ-glycidoxybutyl trimethoxysilane, δ-glycidoxybutyl triethoxysilane, (3,4-epoxycyclohexyl)methyl trimethoxysilane, (3,4-epoxycyclohexyl) Methyltriethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltriethoxysilane, β-(3,4-epoxycyclohexyl)ethyltriproxylsilane, β-(3,4-epoxycyclohexyl)ethyltributoxysilane, β-(3,4-epoxycyclohexyl)ethyltriphenoxysilane, γ-(3,4-epoxycyclohexyl)propyltrimethoxysilane, γ-(3,4-epoxycyclohexyl)propyltriethoxysilane, δ-(3,4-epoxycyclohexyl)butyltrimethoxysilane, δ-(3,4-epoxycyclohexyl)ethyltriproxylsilane,4-Epoxycyclohexyl)butyltriethoxysilane, glycidoxymethylmethyldimethoxysilane, glycidoxymethylmethyldiethoxysilane, α-glycidoxyethylmethyldimethoxysilane, α-glycidoxyethylmethyldiethoxysilane, β-glycidoxyethylmethyldimethoxysilane, β-glycidoxyethylethyldimethoxysilane, α-glycidoxypropylmethyldimethoxysilane, α-glycidoxypropylmethyldiethoxysilane, β-glycidoxypropylmethyldimethoxysilane, β-glycidoxypropylethyldimethoxysilane, γ-glycidoxypropylmethyldimethoxy Silane, γ-glycidoxypropylmethyldiethoxysilane, γ-glycidoxypropylmethyldipropoxysilane, γ-glycidoxypropylmethyldibutoxysilane, γ-glycidoxypropylmethyldiphenoxysilane, γ-glycidoxypropylethyldimethoxysilane, γ-glycidoxypropylethyldiethoxysilane, γ-glycidoxypropylvinyldimethoxysilane, γ-glycidoxypropylvinyldiethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, vinyltrimethoxysilane, vinyltrichlorosilane, vinyltriacetoxysilane, vinyltriethoxysilane, vinyl Triacetoxysilane, phenyltrimethoxysilane, phenyltrichlorosilane, phenyltriacetoxysilane, phenyltriethoxysilane, phenyltriacetoxysilane, γ-chloropropyltrimethoxysilane, γ-chloropropyltriethoxysilane, γ-chloropropyltriacetoxysilane, 3,3,3-trifluoropropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, β-cyanoethyltriethoxysilane, chloromethyltrimethoxysilane, chloromethyltriethoxysilane, dimethyldimethoxysilane, phenylmethyldimethoxysilane, dimethyldimethoxysilane Ethoxysilane, phenylmethyldiethoxysilane, γ-chloropropylmethyldimethoxysilane, γ-chloropropylmethyldiethoxysilane, dimethyldiacetoxysilane, γ-methacryloxypropylmethyldimethoxysilane, γ-methacryloxypropylmethyldiethoxysilane, γ-mercaptopropylmethyldimethoxysilane, γ-mercaptomethyldiethoxysilane, methylvinyldimethoxysilane, methylvinyldiethoxysilane, phenylsulfonylaminopropyltriethoxysilane, methylsulfonylaminopropyltriethoxysilane, phenylsulfonylaminopropyltrimethoxysilane, methylsulfonylaminopropyltrimethoxysilane, etc.
[0066] In particular, a combination of a tetraalkoxysilane such as tetramethoxysilane and tetraethoxysilane and a phenyltrialkoxysilane such as phenyltrimethoxysilane and phenyltriethoxysilane is preferred, and an alkyltrialkoxysilane such as methyltrimethoxysilane and methyltriethoxysilane is further preferred in combination with these combinations.
[0067] The hydrolyzable organosilane of (1) above may also be exemplified by the following structures. 2 Represents R in formula (1) 2 Same definition.
[0068]
[0069]
[0070]
[0071]
[0072]
[0073] R of the hydrolyzable organosilane of formula (2) 3 represents an alkyl group, R 4 represents an alkoxy group, an acyloxy group or a halogen group, Y represents an alkylene group or an arylene group, b represents an integer of 0 or 1, and c represents an integer of 0 or 1.
[0074] As the alkyl group, alkoxy group, acyloxy group or halide group, the groups exemplified in formula (1) can be used. In addition, as the alkylene group and arylene group, the divalent organic groups corresponding to the above-mentioned alkyl group and aryl group can be exemplified.
[0075] Examples of the hydrolyzable organosilanes of formula (2) include methylenebistrimethoxysilane, methylenebistrichlorosilane, methylenebistriacetoxysilane, ethylenebistriethoxysilane, ethylenebistrichlorosilane, ethylenebistriacetoxysilane, propylenebistriethoxysilane, butylenebistrimethoxysilane, phenylenebistrimethoxysilane, phenylenebistriethoxysilane, phenylenebismethyldiethoxysilane, phenylenebismethyldimethoxysilane, naphthylenebistrimethoxysilane, bistrimethoxydisilane, bistriethoxydisilane, bisethyldiethoxydisilane, bismethyldimethoxydisilane, and the like.
[0076] In the present invention, a hydrolysis-condensation product of the hydrolyzable organosilane of the formula (1) or a hydrolysis-condensation product of the hydrolyzable organosilane of the formula (1) and the hydrolyzable organosilane of the formula (2) can be used.
[0077] In the present invention, it is preferred to use a hydrolyzable organosilane represented by formula (1).
[0078] The hydrolysis-condensation products of the hydrolyzable organosilane used in the present invention are exemplified below.
[0079]
[0080]
[0081]
[0082]
[0083] These are preferably used as hydrolysis condensates (polymers of polyorganosiloxane), and preferably hydrolysis condensates (polymers of polyorganosiloxane) of a hydrolyzable organosilane represented by formula (1) are used.
[0084] The hydrolysis condensate (polyorganosiloxane) of the hydrolyzable organosilane of formula (1) or the hydrolysis condensate (polyorganosiloxane) of the hydrolyzable organosilane of formula (1) and the hydrolyzable organosilane of formula (2) can obtain a condensate having a weight average molecular weight of 1000 to 1000000 or 1000 to 100000. These molecular weights are molecular weights obtained by GPC analysis in terms of polystyrene.
[0085] Here, the measurement conditions of GPC can be carried out using the following conditions: for example, a GPC apparatus (trade name HLC-8220GPC, manufactured by Tosoh Corporation), a GPC column (trade name Shodex KF803L, KF802, KF801, manufactured by Showa Denko K.K.), a column temperature of 40°C, an eluent (elution solvent) of tetrahydrofuran, a flow rate (flow velocity) of 1.0 ml / min, and a standard sample of polystyrene (manufactured by Showa Denko K.K.).
[0086] In the hydrolysis of the alkoxysilyl group, the acyloxysilyl group or the halosilyl group, 0.5 to 100 mol, preferably 1 to 10 mol of water is used per 1 mol of the hydrolyzable group.
[0087] The hydrolysis catalyst can be used in an amount of 0.001 to 10 mol, preferably 0.001 to 1 mol, per 1 mol of the hydrolyzable group.
[0088] The reaction temperature during the hydrolysis and condensation is usually 20 to 80°C.
[0089] The hydrolysis may be complete or partial, that is, hydrolyzate and monomers may remain in the hydrolysis-condensation product.
[0090] Furthermore, a catalyst may be used in the hydrolysis and condensation.
[0091] Examples of the hydrolysis catalyst include metal chelates, organic acids, inorganic acids, organic bases, and inorganic bases.
[0092] Examples of the metal chelate as the hydrolysis catalyst include triethoxy mono(acetylacetonate)titanium, tri-n-propoxy mono(acetylacetonate)titanium, tri-isopropoxy mono(acetylacetonate)titanium, tri-n-butoxy mono(acetylacetonate)titanium, tri-sec-butoxy mono(acetylacetonate)titanium, tri-tert-butoxy mono(acetylacetonate)titanium, diethoxy bis(acetylacetonate)titanium, di-n-propoxy bis(acetylacetonate)titanium, di-isopropoxy bis(acetylacetonate)titanium, di-n-butoxy bis(acetylacetonate)titanium, di-sec-butoxybis(acetylacetonate)titanium, di-tert-butoxybis(acetylacetonate)titanium, monoethoxytris(acetylacetonate)titanium, mono-n-propoxytris(acetylacetonate)titanium, monoisopropoxytris(acetylacetonate)titanium, mono-n-butoxytris(acetylacetonate)titanium, mono-sec-butoxytris(acetylacetonate)titanium, mono-tert-butoxytris(acetylacetonate)titanium, tetrakis(acetylacetonate)titanium, triethoxymono(ethyl acetoacetate)titanium, tri-n-propoxy ethyl acetoacetate titanium, tri-isopropoxy mono(ethyl acetoacetate titanium), tri-n-butoxy mono(ethyl acetoacetate titanium), tri-sec-butoxy mono(ethyl acetoacetate titanium), tri-tert-butoxy mono(ethyl acetoacetate titanium), diethoxy bis(ethyl acetoacetate titanium), di-n-propoxy bis(ethyl acetoacetate titanium), di-isopropoxy bis(ethyl acetoacetate titanium), di-n-butoxy bis(ethyl acetoacetate titanium), di-sec-butoxy bis(ethyl acetoacetate titanium, di-tert-butoxy bis( Titanium chelates such as ethyl acetoacetate, monoethoxy tris(ethyl acetoacetate) titanium, mono-n-propoxy tris(ethyl acetoacetate) titanium, mono-isopropoxy tris(ethyl acetoacetate) titanium, mono-n-butoxy tris(ethyl acetoacetate) titanium, mono-sec-butoxy tris(ethyl acetoacetate) titanium, mono-tert-butoxy tris(ethyl acetoacetate) titanium, tetrakis(ethyl acetoacetate) titanium, mono(acetylacetonate) tris(ethyl acetoacetate) titanium, bis(acetylacetonate) bis(ethyl acetoacetate) titanium, and tris(acetylacetonate) mono(ethyl acetoacetate) titanium;triethoxy zirconium mono(acetylacetonate), tri-n-propoxy zirconium mono(acetylacetonate), tri-isopropoxy zirconium mono(acetylacetonate), tri-n-butoxy zirconium mono(acetylacetonate), tri-sec-butoxy zirconium mono(acetylacetonate), tri-tert-butoxy zirconium mono(acetylacetonate), diethoxy zirconium bis(acetylacetonate), di-n-propoxy zirconium bis(acetylacetonate), di-isopropoxy zirconium bis(acetylacetonate), di-n-butoxy zirconium bis(acetylacetonate), di-sec-butoxy Zirconium (acetylacetonate), di-tert-butoxy bis(acetylacetonate), monoethoxy tris(acetylacetonate), mono-n-propoxy tris(acetylacetonate), monoisopropoxy tris(acetylacetonate), mono-n-butoxy tris(acetylacetonate), mono-sec-butoxy tris(acetylacetonate), mono-tert-butoxy tris(acetylacetonate), zirconium tetrakis(acetylacetonate), triethoxy mono(ethyl acetoacetate), tri-n-propoxy mono(ethyl acetoacetate), tri-isopropoxy mono(acetylacetonate) ethyl acetoacetate) zirconium, tri-n-butoxy mono(ethyl acetoacetate) zirconium, tri-sec-butoxy mono(ethyl acetoacetate) zirconium, tri-tert-butoxy mono(ethyl acetoacetate) zirconium, diethoxy bis(ethyl acetoacetate) zirconium, di-n-propoxy bis(ethyl acetoacetate) zirconium, di-isopropoxy bis(ethyl acetoacetate) zirconium, di-n-butoxy bis(ethyl acetoacetate) zirconium, di-sec-butoxy bis(ethyl acetoacetate) zirconium, di-tert-butoxy bis(ethyl acetoacetate) zirconium, monoethoxy tris(ethyl acetoacetate) zirconium, mono ... Zirconium chelates such as propoxy tris(ethyl acetoacetate), monoisopropoxy tris(ethyl acetoacetate), mono-n-butoxy tris(ethyl acetoacetate), mono-sec-butoxy tris(ethyl acetoacetate), mono-tert-butoxy tris(ethyl acetoacetate), tetrakis(ethyl acetoacetate), mono(acetylacetonate) tris(ethyl acetoacetate), bis(acetylacetonate) bis(ethyl acetoacetate), and tris(acetylacetonate) mono(ethyl acetoacetate) zirconium; aluminum chelates such as tris(acetylacetonate) aluminum and tris(ethyl acetoacetate) aluminum; etc.;
[0093] Examples of the organic acid used as the hydrolysis catalyst include acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, heptanoic acid, octanoic acid, nonanoic acid, capric acid, oxalic acid, maleic acid, methylmalonic acid, adipic acid, sebacic acid, gallic acid, butyric acid, mellitic acid, arachidonic acid, shikimic acid, 2-ethylhexanoic acid, oleic acid, stearic acid, linoleic acid, linolenic acid, salicylic acid, benzoic acid, p-aminobenzoic acid, p-toluenesulfonic acid, benzenesulfonic acid, monochloroacetic acid, dichloroacetic acid, trichloroacetic acid, trifluoroacetic acid, formic acid, malonic acid, sulfonic acid, phthalic acid, fumaric acid, citric acid, and tartaric acid.
[0094] Examples of the inorganic acid as the hydrolysis catalyst include hydrochloric acid, nitric acid, sulfuric acid, hydrofluoric acid, phosphoric acid and the like.
[0095] As the organic base of the hydrolysis catalyst, for example, pyridine, pyrrole, piperazine, pyrrolidine, piperidine, picolin, trimethylamine, triethylamine, monoethanolamine, diethanolamine, dimethylmonoethanolamine, monomethyldiethanolamine, triethanolamine, diazabicyclooctane, diazabicyclononane, diazabicycloundecene, tetramethylammonium hydroxide, etc. can be mentioned. As the inorganic base, for example, ammonia, sodium hydroxide, potassium hydroxide, barium hydroxide, calcium hydroxide, etc. can be mentioned. Among these catalysts, metal chelates, organic acids, and inorganic acids are preferred, and they can be used alone or in combination of two or more.
[0096] Examples of the organic solvent used in the hydrolysis include aliphatic hydrocarbon solvents such as n-pentane, isopentane, n-hexane, isohexane, n-heptane, isoheptane, 2,2,4-trimethylpentane, n-octane, isooctane, cyclohexane, and methylcyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, trimethylbenzene, methylethylbenzene, n-propylbenzene, isopropylbenzene, diethylbenzene, isobutylbenzene, triethylbenzene, diisopropylbenzene, n-pentylnaphthalene, and trimethylbenzene; and methanol. , ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, n-pentanol, isopentanol, 2-methylbutanol, sec-pentanol, tert-pentanol, 3-methoxybutanol, n-hexanol, 2-methylpentanol, sec-hexanol, 2-ethylbutanol, sec-heptanol, heptanol-3, n-octanol, 2-ethylhexanol, sec-octanol, n-nonanol, 2,6-dimethylheptanol-4, n-decanol, sec-undecanol, trimethylnonanol, sec-tetradecanol, sec-heptadecanol, phenol, cyclohexane Monohydric alcohol solvents such as ethanol, methyl cyclohexanol, 3,3,5-trimethylcyclohexanol, benzyl alcohol, phenyl methyl carbinol, diacetone alcohol, cresol, etc.; polyhydric alcohol solvents such as ethylene glycol, propylene glycol, 1,3-butanediol, pentanediol-2,4, 2-methylpentanediol-2,4, hexanediol-2,5, heptanediol-2,4, 2-ethylhexanediol-1,3, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, glycerol, etc.; acetone, methyl ethyl ketone, methyl-n-propyl Ketone solvents such as ketone, methyl-n-butyl ketone, diethyl ketone, methyl isobutyl ketone, methyl-n-amyl ketone, ethyl-n-butyl ketone, methyl-n-hexyl ketone, diisobutyl ketone, trimethyl nonanone, cyclohexanone, methylcyclohexanone, 2,4-pentanedione, acetone acetone, diacetone alcohol, acetophenone, and fenchone; ether, isopropyl ether, n-butyl ether, n-hexyl ether, 2-ethylhexyl ether, ethylene oxide, 1,2-propylene oxide, dioxolane, 4-methyldioxolane, dimethicone Alkane, dimethyl Alkane, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol diethyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol mono-n-hexyl ether, ethylene glycol monophenyl ether, ethylene glycol mono-2-ethylbutyl ether, ethylene glycol dibutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol diethyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol di-n-butyl ether, diethylene glycol mono-n-hexyl ether, ethoxytriethylene glycol, tetraethylene glycol di-n-butyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol Ether solvents such as monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monobutyl ether, tripropylene glycol monomethyl ether, tetrahydrofuran, 2-methyltetrahydrofuran, etc.; diethyl carbonate, methyl acetate, ethyl acetate, γ-butyrolactone, γ-valerolactone, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, sec-butyl acetate, n-pentyl acetate, sec-pentyl acetate, 3-methoxybutyl acetate, methylpentyl acetate, 2-ethylbutyl acetate, 2-ethylhexyl acetate, benzyl acetate, cyclohexyl acetate, methyl acetate Cyclohexyl acetate, n-nonyl acetate, methyl acetoacetate, ethyl acetoacetate, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-butyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, ethylene glycol diacetate, methoxytriglycol acetate, ethyl propionate, n-butyl propionate, isopentyl propionate, diethyl oxalate , di-n-butyl oxalate, methyl lactate, ethyl lactate, n-butyl lactate, n-pentyl lactate, diethyl malonate, dimethyl phthalate, diethyl phthalate and other ester solvents; N-methylformamide, N,N-dimethylformamide, N,N-diethylformamide, acetamide, N-methylacetamide, N,N-dimethylacetamide, N-methylpropionamide, N-methylpyrrolidone and other nitrogen-containing solvents; methyl sulfide, ethyl sulfide, thiophene, tetrahydrothiophene, dimethyl sulfoxide, cyclopentane sulfone, 1,3-propane sultone and other sulfur-containing solvents, etc. These solvents can be used alone or in combination of two or more.
[0097] In view of the storage stability of the solution, ketone solvents such as acetone, methyl ethyl ketone, methyl-n-propyl ketone, methyl-n-butyl ketone, diethyl ketone, methyl-isobutyl ketone, methyl-n-amyl ketone, ethyl-n-butyl ketone, methyl-n-hexyl ketone, diisobutyl ketone, trimethylnonanone, cyclohexanone, methylcyclohexanone, 2,4-pentanedione, acetonylacetone, diacetone alcohol, acetophenone, and fenchone (1,1,3-trimethyl-2-norbornene) are particularly preferred.
[0098] The hydrolyzable organosilane is hydrolyzed and condensed in a solvent using a catalyst, and the resulting hydrolysis-condensation product (polymer) can be simultaneously removed by vacuum distillation or the like as a byproduct of alcohol, the hydrolysis catalyst used, and water. In addition, the acid and base catalyst used in the hydrolysis can be removed by neutralization or ion exchange. Moreover, for the resist underlayer film-forming composition for lithography of the present invention, an acid (e.g., an organic acid), water, an alcohol, or a combination thereof can be added to the resist underlayer film-forming composition containing the hydrolysis-condensation product thereof for stabilization.
[0099] As the above-mentioned organic acid, for example, oxalic acid, malonic acid, methylmalonic acid, succinic acid, maleic acid, malic acid, tartaric acid, phthalic acid, citric acid, glutaric acid, citric acid, lactic acid, salicylic acid, etc. can be mentioned. Among them, oxalic acid, maleic acid, etc. are preferred. The organic acid added is 0.5 to 5.0 parts by mass relative to 100 parts by mass of the condensate (polyorganosiloxane). In addition, pure water, ultrapure water, ion exchange water, etc. can be used as the water added, and the amount thereof added can be 1 to 20 parts by mass relative to 100 parts by mass of the resist underlayer film forming composition.
[0100] The alcohol to be added is preferably an alcohol that is easily dispersed by heating after coating, and examples thereof include methanol, ethanol, propanol, isopropanol, butanol, etc. The amount of the alcohol to be added may be 1 to 20 parts by mass based on 100 parts by mass of the resist underlayer film-forming composition.
[0101] The present invention also includes sulfonate ions containing hydrocarbon groups and Ionic salt. The ions can be sulfonium ions, ammonium ions, iodine ions ion, Ions, oxygen ion.
[0102] Should The ion may be an organic group containing at least one aromatic ring. Ions. Preferred The ions are exemplified below.
[0103]
[0104]
[0105]
[0106] In addition, the sulfonate ion containing a hydrocarbon group may be a sulfonate ion having a partially substituted hydrocarbon group. The hydrocarbon group contains a portion of a carbon-hydrogen bond, and a portion of the carbon-hydrogen bond can be replaced by a halogen atom such as fluorine, but it is not preferred that the portion is completely replaced by a halogen atom such as fluorine. Examples of the hydrocarbon group include alkyl and aryl groups having 1 to 20 carbon atoms, and examples include straight-chain alkyl groups such as methyl, ethyl, propyl, and dodecyl, cyclic alkyl groups such as cyclohexyl, phenyl, and combinations of straight-chain and cyclic groups. In formula (1), R 1 Sulfonate ions containing hydrocarbon groups In the case of an ionic salt, the above hydrocarbon group is a corresponding divalent organic group.
[0107] Preferred sulfonate ions containing a hydrocarbon group or sulfonate ions having a hydrocarbon group which may be partially substituted are exemplified below.
[0108]
[0109]
[0110] (In the above formula, n represents 1 to 1000.)
[0111] Furthermore, bisphenol S or a bisphenol S derivative may be added as an additive. The amount of bisphenol S or a bisphenol S derivative is 0.01 to 20 parts by mass, or 0.01 to 10 parts by mass, or 0.01 to 5 parts by mass based on 100 parts by mass of the polyorganosiloxane.
[0112] Preferred bisphenol S or bisphenol S derivatives are exemplified below.
[0113]
[0114] The resist underlayer film-forming composition of the present invention may contain a curing catalyst. The curing catalyst functions as a curing catalyst when a coating film containing a polyorganosiloxane formed from a hydrolysis-condensation product is heated and cured.
[0115] As the curing catalyst, ammonium salts, phosphines, Salt, sulfonium salt.
[0116] Examples of ammonium salts include quaternary ammonium salts having a structure represented by formula (D-1), quaternary ammonium salts having a structure represented by formula (D-2), quaternary ammonium salts having a structure represented by formula (D-3), quaternary ammonium salts having a structure represented by formula (D-4), quaternary ammonium salts having a structure represented by formula (D-5), and tertiary ammonium salts having a structure represented by formula (D-6).
[0117]
[0118] (wherein, m represents an integer of 2 to 11, n represents an integer of 2 to 3, R21 represents an alkyl group or an aryl group, and Y- represents an anion. )
[0119] R 22 R 23 R 24 R 5 N + Y - Formula (D-2)
[0120] (Among them, R 22 , R 23 , R 24 and R 5 represents an alkyl group or an aryl group, N represents a nitrogen atom, and Y - represents an anion, and R 22 , R 23 , R 24 and R 5 Each is bonded to the nitrogen atom through a CN bond)
[0121]
[0122] (Among them, R 6 and R 7 represents an alkyl or aryl group, and Y- represents an anion)
[0123]
[0124] (Among them, R 8 represents an alkyl or aryl group, Y - represents anion)
[0125]
[0126] (Among them, R 9 and R 10 represents an alkyl group or an aryl group, Y - represents anion)
[0127]
[0128] (wherein, m represents an integer of 2 to 11, n represents an integer of 2 to 3, H represents a hydrogen atom, and Y - represents anion)
[0129] In addition, as Salts include quaternary Salt.
[0130] R 11 R 12 R 13 R 14 P + Y -Formula (D-7)
[0131] (Among them, R 11 , R 12 , R 13 and R 14 represents an alkyl group or an aryl group, P represents a phosphorus atom, and Y - represents an anion, and R 11 , R 12 , R 13 and R 14 Each is bonded to the phosphorus atom through a CP bond)
[0132] In addition, examples of the sulfonium salt include tertiary sulfonium salts represented by formula (D-8).
[0133] R 15 R 16 R 17 S + Y - Formula (D-8)
[0134] (Among them, R 15 , R 16 and R 17 represents an alkyl group or an aryl group, S represents a sulfur atom, and Y - represents an anion, and R 15 , R 16 and R 17 Each is bonded to the sulfur atom via a CS bond)
[0135] The compound of the formula (D-1) is a quaternary ammonium salt derived from an amine, wherein m represents an integer of 2 to 11, and n represents an integer of 2 to 3. 21 represents an alkyl group or aryl group having 1 to 18 carbon atoms, preferably 2 to 10 carbon atoms, and examples thereof include straight-chain alkyl groups such as ethyl, propyl, and butyl, benzyl, cyclohexyl, cyclohexylmethyl, and dicyclopentadienyl. - ) can be exemplified by chloride ion (Cl - ), bromide ion (Br - ), iodide ion (I - ) and other halide ions, carboxylates (-COO - ), oxygen radical (-O - ), nitrate ion (NO3 - ) and other acid radicals.
[0136] The compound of the above formula (D-2) is R 22 R 23 R 24 R 5 N + Y - The quaternary ammonium salt R 22 , R23 , R 24 and R 5 It is an alkyl or aryl group having 1 to 18 carbon atoms, or a silane compound bonded to a silicon atom via a Si-C bond. - ) can be chlorine ion (Cl - ), bromide ion (Br - ), iodide ion (I - ) and other halide ions, carboxylates (-COO - ), oxygen radical (-O - ), nitrate ion (NO3 - ) and other acid radicals. The quaternary ammonium salt can be obtained as a commercial product, and examples thereof include tetramethylammonium acetate, tetrabutylammonium acetate, triethylbenzylammonium chloride, triethylbenzylammonium bromide, trioctylmethylammonium chloride, tributylbenzylammonium chloride, trimethylbenzylammonium chloride, etc. These can be added as ammonium compounds.
[0137] The compound of formula (D-3) is a quaternary ammonium salt derived from 1-substituted imidazole, preferably R 6 and R 7 The number of carbon atoms is 1 to 18, R 6 and R 7 The total number of carbon atoms is 7 or more. 6 R represents a methyl group, an ethyl group, a propyl group, a phenyl group, a benzyl group, a silane compound bonded to a silicon atom via a Si-C bond, or a combination thereof. 7 Examples include benzyl, octyl, and octadecyl. - ) can be exemplified by chloride ion (Cl - ), bromide ion (Br - ), iodide ion (I - ) and other halide ions, carboxylates (-COO - ), oxygen radical (-O - ), nitrate ion (NO3 - ) and other acid radicals. The compound can also be obtained as a commercial product, but can be prepared by reacting an imidazole compound such as 1-methylimidazole, 1-benzylimidazole, etc. with an alkyl halide such as benzyl bromide, methyl bromide, or an aryl halide. In addition, the compound of formula (D-3) can be used as a 4,5-dihydroimidazole compound hydrogenated at the 4 and 5 positions. They can be added as cyclic ammonium compounds.
[0138] The compound of formula (D-4) is a quaternary ammonium salt derived from pyridine, R 8 It is an alkyl group or aryl group having 1 to 18 carbon atoms, preferably 4 to 18 carbon atoms, and examples thereof include butyl group, octyl group, benzyl group, and lauryl group. - ) can be exemplified by chloride ion (Cl - ), bromide ion (Br -), iodide ion (I - ) and other halide ions, carboxylates (-COO - ), oxygen radical (-O - ), nitrate ion (NO3 ― ) and other acid radicals. The compound can also be obtained as a commercial product, and can be produced, for example, by reacting pyridine with an alkyl halide such as lauryl chloride, benzyl chloride, benzyl bromide, methyl bromide, octane bromide, or an aryl halide. The compound can be exemplified by, for example, N-laurylpyridinium chloride N-Benzylpyridinium bromide wait.
[0139] The compound of the above formula (D-5) is a quaternary ammonium salt derived from a substituted pyridine represented by picolinate, etc. 9 It is an alkyl group or aryl group having 1 to 18 carbon atoms, preferably 4 to 18 carbon atoms, and examples thereof include methyl, octyl, lauryl, and benzyl. 10 is an alkyl group or an aryl group having 1 to 18 carbon atoms. For example, in the case of a quaternary ammonium group derived from picolinate, R 10 Methyl. Anion (Y - ) can be exemplified by chloride ion (Cl - ), bromide ion (Br - ), iodide ion (I - ) and other halide ions, carboxylates (-COO - ), oxygen radical (-O - ), nitrate ion (NO3 ― ) and other acid radicals. The compound can also be obtained as a commercial product, for example, by reacting a substituted pyridine such as picolinate with an alkyl halide such as methyl bromide, octyl bromide, lauryl chloride, benzyl chloride, benzyl bromide, or an aryl halide. The compound can be exemplified by, for example, N-benzylpicolinate chloride N-Benzylpicoline bromide N-Laurylpicolinyl chloride wait.
[0140] The compound of the above formula (D-6) is a tertiary ammonium salt derived from an amine, wherein m represents an integer of 2 to 11, and n represents an integer of 2 to 3. - ) can be exemplified by chloride ion (Cl - ), bromide ion (Br - ), iodide ion (I - ) and other halide ions, carboxylates (-COO - ), oxygen radical (-O - ), nitrate ion (NO3 ― ) and other acid radicals. It can be produced by the reaction of amines with weak acids such as carboxylic acids and phenols. As carboxylic acids, formic acid and acetic acid can be cited. When formic acid is used, the anion (Y - ) is (HCOO- ), in the case of acetic acid, the anion (Y - ) is (CH3COO - ). In addition, when phenol is used, the anion (Y - ) is (C6H5O - ).
[0141] The compound of the above formula (D-7) is a compound having R 11 R 12 R 13 R 14 P + Y - The structure of the season Salt. 11 , R 12 , R 13 and R 14 is an alkyl or aryl group having 1 to 18 carbon atoms, or a silane compound bonded to a silicon atom via a Si-C bond, preferably R 11 ~R 14 Three of the four substituents are phenyl or substituted phenyl, such as phenyl and tolyl, and the remaining one is an alkyl group having 1 to 18 carbon atoms, an aryl group, or a silane compound bonded to a silicon atom via a Si-C bond. - ) can be exemplified by chloride ion (Cl - ), bromide ion (Br - ), iodide ion (I - ) and other halide ions, carboxylates (-COO - ), oxygen radical (-O - ), nitrate ion (NO3 ― ) and other acid radicals.
[0142] This compound is commercially available, and examples thereof include tetra-n-butyl halogenide Tetra-n-propyl halide Tetraalkyl halides Triethylbenzyl halide Trialkylbenzyl halides Triphenylmethyl halides Triphenylethyl halide Triphenyl halogenated monoalkyl , triphenylbenzyl halides Tetraphenyl halides Trimethylphenyl halides or trimethylbenzene monoalkyl halides (The halogen atom is a chlorine atom or a bromine atom.) A halogenated triphenylmethyl Triphenylethyl halide Triphenyl halogenated monoalkyl Triphenylbenzyl halides Isohalogenated triphenyl monoaryl Halogenated trimethylphenyl monophenyl Isohalogenated trimethylphenyl monoaryl Trimethylol Halide Isohalogenated trimethylbenzyl monoalkyl (The halogen atom is a chlorine atom or a bromine atom).
[0143] In addition, examples of the phosphines include primary phosphines such as methyl phosphine, ethyl phosphine, propyl phosphine, isopropyl phosphine, isobutyl phosphine and phenyl phosphine, secondary phosphines such as dimethyl phosphine, diethyl phosphine, diisopropyl phosphine, diisopentyl phosphine and diphenyl phosphine, and tertiary phosphines such as trimethyl phosphine, triethyl phosphine, triphenyl phosphine, methyldiphenyl phosphine and dimethylphenyl phosphine.
[0144] The compound of the above formula (D-8) is a compound having R 15 R 16 R 17 S + Y - The structure of tertiary sulfonium salt. 15 , R 16 and R 17 is an alkyl or aryl group having 1 to 18 carbon atoms, or a silane compound bonded to a silicon atom via a Si-C bond, preferably R 15 ~R 17 Three of the four substituents are phenyl or substituted phenyl, such as phenyl and tolyl, and the remaining one is an alkyl or aryl group having 1 to 18 carbon atoms which may be substituted. - ) can be exemplified by chloride ion (Cl - ), bromide ion (Br - ), iodide ion (I - ) and other halide ions, carboxylates (-COO - ), oxygen radical (-O - ), nitrate ion (NO3 ― The compound can be obtained as a commercial product, and examples thereof include tetraalkyl halides such as tri-n-butylsulfonium halide and tri-n-propylsulfonium halide. trialkylbenzylsulfonium halides such as diethylbenzylsulfonium halides, diphenylmonoalkylsulfonium halides such as diphenylmethylsulfonium halides and diphenylethylsulfonium halides, triphenylsulfonium halides (the halogen atom is a chlorine atom or a bromine atom), tetraalkylcarboxylates such as tri-n-butylsulfonium carboxylate and tri-n-propylsulfonium carboxylate , trialkylbenzylsulfonium carboxylates such as diethylbenzylsulfonium carboxylate, diphenylmonoalkylsulfonium carboxylates such as diphenylmethylsulfonium carboxylate and diphenylethylsulfonium carboxylate, triphenylsulfonium carboxylate, etc. Particularly preferred are triphenylsulfonium halides and triphenylsulfonium carboxylates.
[0145] The curing catalyst is contained in an amount of 0.01 to 10 parts by mass, or 0.01 to 5 parts by mass, or 0.01 to 3 parts by mass based on 100 parts by mass of the polyorganosiloxane.
[0146] The composition for forming an underlayer film for lithography of the present invention may contain an organic polymer compound, a photoacid generator, a surfactant, and the like, in addition to the above-mentioned components, as necessary.
[0147] By using an organic polymer compound, the dry etching rate (amount of reduction in film thickness per unit time), extinction coefficient, refractive index, etc. of the resist underlayer film formed from the composition for forming an underlayer film for lithography of the present invention can be adjusted.
[0148] As the organic polymer compound, there is no particular limitation, and various organic polymers can be used. Condensation polymers and addition polymers can also be used. Addition polymers and condensation polymers such as polyester, polystyrene, polyimide, acrylic polymer, methacrylic polymer, polyvinyl ether, phenol novolac, naphthol novolac, polyether, polyamide, polycarbonate can be used. It is preferred to use organic polymers with aromatic ring structures such as benzene rings, naphthalene rings, anthracene rings, triazine rings, quinoline rings and quinoxaline rings that act as light absorption sites.
[0149] Examples of such organic polymer compounds include addition polymers containing addition polymerizable monomers such as benzyl acrylate, benzyl methacrylate, phenyl acrylate, naphthyl acrylate, anthracene methacrylate, anthracene methyl methacrylate, styrene, hydroxystyrene, benzyl vinyl ether and N-phenylmaleimide as structural units; and condensation polymers such as phenol novolac and naphthol novolac.
[0150] When an addition polymer is used as the organic polymer compound, the polymer compound may be a homopolymer or a copolymer. When producing the addition polymer, an addition polymerizable monomer may be used. Examples of such addition polymerizable monomers include acrylic acid, methacrylic acid, acrylate compounds, methacrylate compounds, acrylamide compounds, methacrylamide compounds, vinyl compounds, styrene compounds, maleimide compounds, maleic anhydride, and acrylonitrile.
[0151] When an organic polymer compound is used, the ratio thereof is 1 to 200 parts by mass, or 5 to 100 parts by mass, or 10 to 50 parts by mass, or 20 to 30 parts by mass based on 100 parts by mass of the condensate (polyorganosiloxane).
[0152] In the present invention, a crosslinking compound may be contained. As these crosslinking agents, crosslinking compounds having at least two substituents forming crosslinks are preferably used. For example, melamine compounds and substituted urea compounds having substituents forming crosslinks such as methylol and methoxymethyl may be mentioned. Specifically, compounds such as methoxymethylated glycoluril or methoxymethylated melamine, for example, tetramethoxymethyl glycoluril, tetrabutoxymethyl glycoluril or hexamethoxymethyl melamine. In addition, compounds such as tetramethoxymethyl urea and tetrabutoxymethyl urea may also be mentioned. When these crosslinking agents are included, the content in the solid content is, for example, less than 50% by mass, 0.01 to 50% by mass, or 10 to 40% by mass.
[0153] The resist underlayer film-forming composition of the present invention may contain an acid compound. Examples of the acid compound include p-toluenesulfonic acid, trifluoromethanesulfonic acid, and pyridinium p-toluenesulfonate. Examples of the acid compound include sulfonic acid compounds such as succinic acid, salicylic acid, sulfosalicylic acid, citric acid, benzoic acid, and hydroxybenzoic acid. In addition, examples of the acid compound include acid generators that generate acid by heat or light, such as 2,4,4,6-tetrabromocyclohexadienonone, benzoin toluenesulfonate, 2-nitrobenzyl toluenesulfonate, p-trifluoromethylbenzenesulfonic acid-2,4-dinitrobenzyl ester, and phenyl-bis(trichloromethyl)-s-triazine. Examples of the acid compound include diphenyl iodide. Hexafluorophosphate and other iodine Salt-based acid generator. As the acid compound, iodine is preferred Salt-based acid generators are acid generators.
[0154] The photoacid generator may be used alone or in combination of two or more.
[0155] When a photoacid generator is used, the ratio thereof is 0.01 to 15 parts by mass, or 0.1 to 10 parts by mass, or 0.5 to 5 parts by mass based on 100 parts by mass of the condensate (polyorganosiloxane).
[0156] When the resist underlayer film-forming composition for lithography of the present invention is applied to a substrate, a surfactant is effective in suppressing the generation of pinholes, streaks, and the like.
[0157] Examples of the surfactant contained in the resist underlayer film-forming composition of the present invention include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether, polyoxyethylene alkyl aryl ethers such as polyoxyethylene octylphenol ether and polyoxyethylene nonylphenol ether, polyoxyethylene-polyoxypropylene block copolymers, sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate, and sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate. Nonionic surfactants such as polyoxyethylene sorbitan fatty acid esters such as polyoxyethylene sorbitan tristearate, trade names EFTOP EF301, EF303, EF352 (manufactured by Tokem Projects Co., Ltd.), trade names Megaphak F171, F173, R-08, R-30 (manufactured by Dainippon Inki Chemical Industries, Ltd.), Fluora Fluorine-based surfactants such as fluorosilicone FC430, FC431 (manufactured by Sumitomo Slide (Co., Ltd.), trade name Asahigard AG710, Surflon S-382, SC101, SC102, SC103, SC104, SC105, SC106 (manufactured by Asahi Glass Co., Ltd.), and organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.). These surfactants can be used alone or in combination of two or more. When a surfactant is used, the ratio thereof is 0.0001 to 5 parts by mass, or 0.001 to 1 part by mass, or 0.01 to 0.5 parts by mass relative to 100 parts by mass of the condensate (polyorganosiloxane).
[0158] In addition, the resist underlayer film-forming composition of the present invention may contain a rheology control agent and an adhesion auxiliary agent. The rheology control agent is effective in improving the fluidity of the underlayer film-forming composition. The adhesion auxiliary agent is effective in improving the adhesion between the semiconductor substrate or the resist and the underlayer film.
[0159] The solvent used in the resist underlayer film-forming composition of the present invention can be used without particular limitation as long as it is a solvent that can dissolve the above-mentioned solid components. Examples of such solvents include methyl cellosolve acetate, ethyl cellosolve acetate, propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, methyl isobutyl carbinol, propylene glycol monobutyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, propylene glycol monobutyl ether acetate, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxylate, ethyl hydroxylate, methyl 2-hydroxy-3-methylbutyrate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate , ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monopropyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, diethylene glycol dibutyl ether, propylene glycol monomethyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, propylene glycol dipropyl ether, propylene glycol dibutyl ether, ethyl lactate, propyl lactate, isopropyl lactate, butyl lactate, isopropyl lactate Butyl ester, methyl formate, ethyl formate, propyl formate, isopropyl formate, butyl formate, isobutyl formate, pentyl formate, isoamyl formate, methyl acetate, ethyl acetate, pentyl acetate, isoamyl acetate, hexyl acetate, methyl propionate, ethyl propionate, propyl propionate, isopropyl propionate, butyl propionate, isobutyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, isopropyl butyrate, butyl butyrate, isobutyl butyrate, ethyl hydroxyacetate, ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxy-2-methylpropionate, methyl 2-hydroxy-3-methylbutyrate, ethyl methoxyacetate, ethyl ethoxyacetate, 3- Methyl methoxypropionate, ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-methoxybutyl acetate, 3-methoxypropyl acetate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutyl propionate, 3-methyl-3-methoxybutyl butyrate, methyl acetoacetate, toluene, xylene, methyl ethyl ketone, methyl propyl ketone, methyl butyl ketone, 2-heptanone, 3-heptanone, 4-heptanone, cyclohexanone, N,N-dimethylformamide, N-methylacetamide, N,N-dimethylacetamide, N-methylpyrrolidone, 4-methyl-2-pentanol and γ-butyrolactone. These solvents can be used alone or in combination of two or more.
[0160] In addition, in the present invention, a composition for forming a resist underlayer film for EUV lithography can be prepared, which contains a hydrolyzable organosilane as a silane, a hydrolyzate thereof, or a hydrolysis-condensation product thereof, wherein the hydrolyzable organosilane is the silane represented by the above formula (2). Examples of the hydrolyzable organosilane used herein include bistriethoxysilylethane, bistriethoxysilylmethane, bistriethoxysilane, bistriethoxysilyloctane, and the like.
[0161] The resist underlayer film-forming composition for EUV lithography containing a hydrolyzable organosilane as silane, a hydrolyzate thereof, or a hydrolysis-condensation product thereof, wherein the hydrolyzable organosilane is a silane represented by the above formula (2), can be implemented in combination with the respective constitutions described in the present specification.
[0162] The resist underlayer film forming composition of the present invention is applied to a semiconductor substrate (e.g., a silicon / silicon dioxide coated substrate, a silicon nitride substrate, a glass substrate, and an ITO substrate, etc.) by an appropriate coating method such as a spin coater or a coater, and then baked to form a resist underlayer film.
[0163] The baking conditions are appropriately selected from a baking temperature of 80° C. to 250° C. and a baking time of 0.3 to 60 minutes. Preferably, the baking temperature is 130° C. to 250° C. and the baking time is 0.5 to 5 minutes. Here, the film thickness of the formed resist lower layer film is, for example, 0.005 to 3.0 μm, preferably, for example, 0.01 to 1.0 μm, or 0.01 to 0.5 μm, or 0.01 to 0.05 μm.
[0164] Next, a high-energy-ray resist layer such as an EUV resist is formed on the resist underlayer film. The high-energy-ray resist layer can be formed by a known method, that is, by applying a high-energy-ray resist composition solution on the underlayer film and baking it.
[0165] As the EUV resist, for example, a resist composition using a resin such as PMMA (polymethyl methacrylate), polyhydroxystyrene, or a phenol resin can be used.
[0166] Next, exposure is performed through a specified mask. EUV light (13.5 nm), electron beams, X-rays, etc. can be used for exposure. After exposure, post-exposure baking (PEB) can be performed as needed. The post-exposure baking temperature is appropriately selected from 70°C to 150°C and the heating time is 0.3 to 10 minutes.
[0167] Next, the image is developed by a developer. Examples of the developer include aqueous solutions of alkali metal hydroxides such as potassium hydroxide and sodium hydroxide, aqueous solutions of quaternary ammonium hydroxides such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, and choline, and alkaline aqueous solutions of amines such as ethanolamine, propylamine, and ethylenediamine. In addition, a surfactant may be added to these developers. The conditions for development are appropriately selected from a temperature of 5 to 50° C. and a time of 10 to 300 seconds.
[0168] In addition, in the present invention, an organic solvent can be used as a developer. After exposure, development is performed by a developer (solvent). Thus, when a positive photoresist is used, for example, the photoresist of the unexposed portion is removed to form a photoresist pattern.
[0169] Examples of the developer include methyl acetate, butyl acetate, ethyl acetate, isopropyl acetate, amyl acetate, isoamyl acetate, methoxyethyl acetate, ethoxyethyl acetate, propylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monopropyl ether acetate, ethylene glycol monobutyl ether acetate, ethylene glycol monophenyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monopropyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monophenyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, 2-methoxybutyl acetate, 3-methoxybutyl acetate, 4-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, 3-ethyl-3-methoxybutyl acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, 2-ethoxybutyl acetate, 4-ethoxybutyl acetate. butyl acetate, 4-propoxybutyl acetate, 2-methoxypentyl acetate, 3-methoxypentyl acetate, 4-methoxypentyl acetate, 2-methyl-3-methoxypentyl acetate, 3-methyl-3-methoxypentyl acetate, 3-methyl-4-methoxypentyl acetate, 4-methyl-4-methoxypentyl acetate, propylene glycol diacetate, methyl formate, ethyl formate, butyl formate, propyl formate, ethyl lactate, lactate The developer may be butyl ester, propyl lactate, ethyl carbonate, propyl carbonate, butyl carbonate, methyl pyruvate, ethyl pyruvate, propyl pyruvate, butyl pyruvate, methyl acetoacetate, ethyl acetoacetate, methyl propionate, ethyl propionate, propyl propionate, isopropyl propionate, methyl 2-hydroxypropionate, ethyl 2-hydroxypropionate, methyl-3-methoxypropionate, ethyl-3-methoxypropionate, ethyl-3-ethoxypropionate, propyl-3-methoxypropionate, etc. In addition, a surfactant may be added to the developer. The conditions for development may be appropriately selected from a temperature of 5 to 50° C. and a time of 10 to 600 seconds.
[0170] Then, the photoresist pattern thus formed is used as a protective film to remove the resist underlayer film and process the semiconductor substrate. The removal of the resist underlayer film is carried out using a gas such as tetrafluoromethane, perfluorocyclobutane (C4F8), perfluoropropane (C3F8), trifluoromethane, carbon monoxide, argon, oxygen, nitrogen, sulfur hexafluoride, difluoromethane, nitrogen trifluoride, and chlorine trifluoride.
[0171] Before forming the resist underlayer film of the present invention on the semiconductor substrate, a planarization film, a gap filling material layer, and an organic underlayer film may be formed. When a semiconductor substrate having a large step difference or a hole is used, it is preferred to form a planarization film and a gap filling material layer.
[0172] In addition, as the lower film of the EUV resist, in addition to the function as a hard mask, it can also be used for the following purposes. As a lower anti-reflective film of the EUV resist that is not mixed with the EUV resist and can prevent the unpreferable exposure light such as the above-mentioned UV, DUV (ArF light, KrF light) from reflecting from the substrate or interface during EUV exposure (wavelength 13.5nm), the above-mentioned resist lower film forming composition can be used. Reflection can be effectively prevented in the lower layer of the EUV resist. When used as an EUV resist lower film, the process can be carried out in the same way as the photoresist lower film.
[0173] Example
[0174] Synthesis example 1
[0175] 24.48 g (70 mol%) of tetramethoxysilane, 9.39 g (30 mol%) of methyltrimethoxysilane, and 50.81 g of acetone were added to a 300 ml flask, and 15.31 g of 0.01 mol / l hydrochloric acid was added dropwise to the mixed solution while stirring the mixed solution with an electromagnetic stirrer. After the addition, the flask was transferred to an oil bath adjusted to 85°C, and the mixture was reacted under heating and reflux for 240 minutes. Then, the reaction solution was cooled to room temperature, 68.00 g of propylene glycol monomethyl ether acetate was added to the reaction solution, and methanol, acetone, water, and hydrochloric acid as reaction by-products were removed by reduced pressure distillation, and concentrated to obtain a hydrolysis condensation product (polymer) propylene glycol monomethyl ether acetate solution. Propylene glycol monoethyl ether was added, and the solvent ratio of propylene glycol monomethyl ether acetate / propylene glycol monoethyl ether 20 / 80 was adjusted to 20% by weight based on the solid residue at 140°C. The obtained polymer corresponds to the formula (2-1), and the weight average molecular weight obtained by GPC was Mw 2000 in terms of polystyrene.
[0176] Synthesis example 2
[0177] 24.06 g (70 mol%) of tetramethoxysilane, 7.69 g (25 mol%) of methyltrimethoxysilane, 2.24 g (5 mol%) of phenyltrimethoxysilane, and 50.97 g of acetone were added to a 300 ml flask, and 15.04 g of 0.01 mol / l hydrochloric acid was added dropwise to the mixed solution while stirring the mixed solution with an electromagnetic stirrer. After the addition, the flask was transferred to an oil bath adjusted to 85°C, and the mixture was reacted under heating and reflux for 240 minutes. Then, the reaction solution was cooled to room temperature, 68.00 g of propylene glycol monomethyl ether acetate was added to the reaction solution, and methanol, acetone, water, and hydrochloric acid as reaction by-products were removed by vacuum distillation, and the mixture was concentrated to obtain a hydrolysis condensation product (polymer) propylene glycol monomethyl ether acetate solution. Propylene glycol monoethyl ether was added to adjust the solvent ratio of propylene glycol monomethyl ether acetate / propylene glycol monoethyl ether to 20 / 80, which was 20% by weight in terms of solid residue at 140° C. The obtained polymer corresponded to formula (2-2) and had a weight average molecular weight of Mw 2000 in terms of polystyrene as determined by GPC.
[0178] Synthesis example 3
[0179] 23.85 g (70 mol%) of tetramethoxysilane, 7.62 g (25 mol%) of methyltrimethoxysilane, 2.56 g (5 mol%) of 4-(methoxyphenyl)trimethoxysilane, and 51.05 g of acetone were added to a 300 ml flask, and 14.92 g of 0.01 mol / l hydrochloric acid was added dropwise to the mixed solution while stirring the mixed solution with an electromagnetic stirrer. After the addition, the flask was transferred to an oil bath adjusted to 85°C, and the mixture was reacted under heating and reflux for 240 minutes. Then, the reaction solution was cooled to room temperature, 68.00 g of propylene glycol monomethyl ether acetate was added to the reaction solution, and methanol, acetone, water, and hydrochloric acid as reaction by-products were removed by reduced pressure distillation, and the mixture was concentrated to obtain a hydrolysis condensation product (polymer) propylene glycol monomethyl ether acetate solution. Propylene glycol monoethyl ether was added to adjust the solvent ratio of propylene glycol monomethyl ether acetate / propylene glycol monoethyl ether to 20 / 80, which was 20% by weight in terms of solid residue at 140° C. The obtained polymer corresponded to formula (2-3) and had a weight average molecular weight of Mw 2000 in terms of polystyrene as determined by GPC.
[0180] Synthesis example 4
[0181] 22.68 g (70 mol%) of tetramethoxysilane, 7.25 g (25 mol%) of methyltrimethoxysilane, 4.40 g (5 mol%) of 3-(triethoxysilyl)propyldiallyl isocyanurate, and 51.50 g of acetone were added to a 300 ml flask, and 14.18 g of 0.01 mol / l hydrochloric acid was added dropwise to the mixed solution while stirring the mixed solution with an electromagnetic stirrer. After the addition, the flask was transferred to an oil bath adjusted to 85°C, and the mixture was reacted under heating and reflux for 240 minutes. Then, the reaction solution was cooled to room temperature, 68.00 g of propylene glycol monomethyl ether acetate was added to the reaction solution, and methanol, acetone, water, and hydrochloric acid as reaction by-products were removed by reduced pressure distillation, and the mixture was concentrated to obtain a hydrolysis condensation product (polymer) propylene glycol monomethyl ether acetate solution. Propylene glycol monoethyl ether was added to adjust the solvent ratio of propylene glycol monomethyl ether acetate / propylene glycol monoethyl ether to 20 / 80, which was 20% by weight in terms of solid residue at 140° C. The obtained polymer corresponded to formula (2-4) and had a weight average molecular weight of Mw 2000 in terms of polystyrene as determined by GPC.
[0182] Synthesis example 5
[0183] 21.62 g (70 mol%) of tetramethoxysilane, 4.15 g (15 mol%) of methyltrimethoxysilane, 4.20 g (5 mol%) of 3-(triethoxysilyl)propyldiallyl isocyanurate, 4.63 g (10 mol%) of 4-(methoxyphenyl)trimethoxysilane, and 51.89 g of acetone were added to a 300 ml flask, and 13.52 g of 0.01 mol / l hydrochloric acid was added dropwise to the mixed solution while stirring the mixed solution with an electromagnetic stirrer. After the addition, the flask was transferred to an oil bath adjusted to 85° C., and the mixture was reacted under heating and reflux for 240 minutes. Then, the reaction solution was cooled to room temperature, 68.00 g of propylene glycol monomethyl ether acetate was added to the reaction solution, and methanol, acetone, water, and hydrochloric acid as reaction by-products were removed by reduced pressure distillation, and the mixture was concentrated to obtain a hydrolysis condensation product (polymer) propylene glycol monomethyl ether acetate solution. Propylene glycol monoethyl ether was added to adjust the solvent ratio of propylene glycol monomethyl ether acetate / propylene glycol monoethyl ether to 20 / 80, which was 20% by weight in terms of solid residue at 140° C. The obtained polymer corresponded to formula (2-5) and had a weight average molecular weight of Mw 2000 in terms of polystyrene as determined by GPC.
[0184] Synthesis example 6
[0185] 23.19 g (70 mol%) of tetramethoxysilane, 7.41 g (25 mol%) of methyltrimethoxysilane, 3.59 g (5 mol%) of pentafluorophenyltriethoxysilane, and 51.30 g of acetone were added to a 300 ml flask, and 14.50 g of 0.01 mol / l hydrochloric acid was added dropwise to the mixed solution while stirring the mixed solution with an electromagnetic stirrer. After the addition, the flask was transferred to an oil bath adjusted to 85°C, and the mixture was reacted under heating and reflux for 240 minutes. Then, the reaction solution was cooled to room temperature, 68.00 g of propylene glycol monomethyl ether acetate was added to the reaction solution, and methanol, acetone, water, and hydrochloric acid as reaction by-products were removed by vacuum distillation, and the mixture was concentrated to obtain a hydrolysis condensation product (polymer) propylene glycol monomethyl ether acetate solution. Propylene glycol monoethyl ether was added to adjust the solvent ratio of propylene glycol monomethyl ether acetate / propylene glycol monoethyl ether to 20 / 80, which was 20% by weight in terms of solid residue at 140° C. The obtained polymer corresponded to formula (2-6) and had a weight average molecular weight of Mw 2000 in terms of polystyrene as determined by GPC.
[0186] Synthesis Example 7
[0187] 23.55 g (70 mol%) of tetramethoxysilane, 7.53 g (25 mol%) of methyltrimethoxysilane, 3.04 g (5 mol%) of p-chlorophenyltriethoxysilane, and 51.16 g of acetone were added to a 300 ml flask, and 14.73 g of 0.01 mol / l hydrochloric acid was added dropwise to the mixed solution while stirring the mixed solution with an electromagnetic stirrer. After the addition, the flask was transferred to an oil bath adjusted to 85°C, and the mixture was reacted under heating and reflux for 240 minutes. Then, the reaction solution was cooled to room temperature, 68.00 g of propylene glycol monomethyl ether acetate was added to the reaction solution, and methanol, acetone, water, and hydrochloric acid as reaction by-products were removed by reduced pressure distillation, and the mixture was concentrated to obtain a hydrolysis condensation product (polymer) propylene glycol monomethyl ether acetate solution. Propylene glycol monoethyl ether was added to adjust the solvent ratio of propylene glycol monomethyl ether acetate / propylene glycol monoethyl ether to 20 / 80, which was 20% by weight in terms of solid residue at 140° C. The obtained polymer corresponded to formula (2-7) and had a weight average molecular weight of Mw 2000 in terms of polystyrene as determined by GPC.
[0188] Synthesis example 8
[0189] 23.04 g (70 mol%) of tetramethoxysilane, 7.36 g (25 mol%) of methyltrimethoxysilane, 3.83 g (5 mol%) of bistriethoxysilylethane, and 51.35 g of acetone were added to a 300 ml flask, and 14.41 g of 0.01 mol / l hydrochloric acid was added dropwise to the mixed solution while stirring the mixed solution with an electromagnetic stirrer. After the addition, the flask was transferred to an oil bath adjusted to 85°C, and the mixture was reacted under heating and reflux for 240 minutes. Then, the reaction solution was cooled to room temperature, 68.00 g of propylene glycol monomethyl ether acetate was added to the reaction solution, and methanol, acetone, water, and hydrochloric acid as reaction by-products were removed by reduced pressure distillation, and the mixture was concentrated to obtain a hydrolysis condensation product (polymer) propylene glycol monomethyl ether acetate solution. Propylene glycol monoethyl ether was added to adjust the solvent ratio of propylene glycol monomethyl ether acetate / propylene glycol monoethyl ether to 20 / 80, which was 20% by weight in terms of solid residue at 140° C. The obtained polymer corresponded to formula (2-8) and had a weight average molecular weight of Mw 2000 in terms of polystyrene as determined by GPC.
[0190] Synthesis example 9
[0191] 24.17 g (70 mol%) of tetramethoxysilane, 8.96 g (29 mol%) of methyltrimethoxysilane, 0.82 g (1 mol%) of N-3-(triethoxysilyl)propylbenzenesulfonamide, and 50.93 g of acetone were added to a 300 ml flask, and 15.12 g of 0.01 mol / l hydrochloric acid was added dropwise to the mixed solution while stirring the mixed solution with an electromagnetic stirrer. After the addition, the flask was transferred to an oil bath adjusted to 85°C, and the mixture was reacted under heating and reflux for 240 minutes. Then, the reaction solution was cooled to room temperature, 68.00 g of propylene glycol monomethyl ether acetate was added to the reaction solution, and methanol, acetone, water, and hydrochloric acid as reaction by-products were removed by reduced pressure distillation, and the mixture was concentrated to obtain a hydrolysis condensation product (polymer) propylene glycol monomethyl ether acetate solution. Propylene glycol monoethyl ether was added to adjust the solvent ratio of propylene glycol monomethyl ether acetate / propylene glycol monoethyl ether to 20 / 80, which was 20% by weight in terms of solid residue at 140° C. The obtained polymer corresponded to formula (2-9) and had a weight average molecular weight of Mw 2000 in terms of polystyrene as determined by GPC.
[0192] Synthesis example 10
[0193] 27.61 g (80 mol%) of tetramethoxysilane, 6.18 g (20 mol%) of methyltrimethoxysilane, and 50.69 g of acetone were added to a 300 ml flask, and 15.52 g of 0.01 mol / l hydrochloric acid was added dropwise to the mixed solution while stirring the mixed solution with an electromagnetic stirrer. After the addition, the flask was transferred to an oil bath adjusted to 85°C, and the mixture was reacted under heating reflux for 240 minutes. Then, the reaction solution was cooled to room temperature, 68.00 g of propylene glycol monomethyl ether acetate was added to the reaction solution, and methanol, acetone, water, and hydrochloric acid as reaction by-products were removed by reduced pressure distillation, and concentrated to obtain a hydrolysis condensation product (polymer) propylene glycol monomethyl ether acetate solution. Propylene glycol monoethyl ether was added, and the solvent ratio of propylene glycol monomethyl ether acetate / propylene glycol monoethyl ether 20 / 80 was adjusted to 20% by weight based on the solid residue at 140°C. The obtained polymer corresponds to the formula (2-1), and the weight average molecular weight obtained by GPC was Mw 2000 in terms of polystyrene.
[0194] Synthesis Example 11
[0195] 24.20 g (70 mol%) of tetramethoxysilane, 8.97 g (29 mol%) of methyltrimethoxysilane, N-(3-triethoxysilylpropyl)ethyl-4,5-dihydroimidazole chloride 0.77g, 50.92g of acetone are added to a 300ml flask, and 15.14g of 0.01mol / l hydrochloric acid is added dropwise to the mixed solution while stirring the mixed solution with an electromagnetic stirrer. After addition, the flask is transferred to an oil bath adjusted to 85°C and reacted for 240 minutes under heating reflux. Then, the reaction solution is cooled to room temperature, 68.00g of propylene glycol monomethyl ether acetate is added to the reaction solution, and methanol, acetone, water, and hydrochloric acid as reaction by-products are removed by reduced pressure distillation, and concentrated to obtain a hydrolysis condensation product (polymer) propylene glycol monomethyl ether acetate solution. Propylene glycol monoethyl ether is added, and the solvent ratio of propylene glycol monomethyl ether acetate / propylene glycol monoethyl ether 20 / 80 is adjusted to 20% by weight based on the solid residue at 140°C. The polymer obtained is equivalent to formula (2-10), and the weight average molecular weight obtained by GPC is Mw2000 based on polystyrene.
[0196] Synthesis example 12
[0197] 24.25 g (70 mol%) of tetramethoxysilane, 8.99 g (29 mol%) of methyltrimethoxysilane, 0.69 g of 3-(triethoxysilyl)propylsuccinic anhydride, and 50.90 g of acetone were added to a 300 ml flask, and 15.17 g of 0.01 mol / l hydrochloric acid was added dropwise to the mixed solution while stirring the mixed solution with an electromagnetic stirrer. After the addition, the flask was transferred to an oil bath adjusted to 85°C, and the mixture was reacted under heating and reflux for 240 minutes. Then, the reaction solution was cooled to room temperature, 68.00 g of propylene glycol monomethyl ether acetate was added to the reaction solution, and methanol, acetone, water, and hydrochloric acid as reaction by-products were removed by reduced pressure distillation, and the mixture was concentrated to obtain a hydrolysis condensation product (polymer) propylene glycol monomethyl ether acetate solution. Propylene glycol monoethyl ether was added to adjust the solvent ratio of propylene glycol monomethyl ether acetate / propylene glycol monoethyl ether to 20 / 80, which was 20% by weight in terms of solid residue at 140° C. The obtained polymer corresponded to formula (2-11) and had a weight average molecular weight of Mw 2000 in terms of polystyrene as determined by GPC.
[0198] Synthesis example 13
[0199] 23.87 g (70 mol%) of tetramethoxysilane, 8.85 g (29 mol%) of methyltrimethoxysilane, 1.31 g of 3-(triethoxysilyl)propylsuccinic acid monotriphenylsulfonium salt, and 51.04 g of acetone were added to a 300 ml flask, and 14.93 g of 0.01 mol / l hydrochloric acid was added dropwise to the mixed solution while stirring the mixed solution with an electromagnetic stirrer. After the addition, the flask was transferred to an oil bath adjusted to 85°C, and the mixture was reacted under heating and reflux for 240 minutes. Then, the reaction solution was cooled to room temperature, 68.00 g of propylene glycol monomethyl ether acetate was added to the reaction solution, and methanol, acetone, water, and hydrochloric acid as reaction by-products were removed by reduced pressure distillation, and the mixture was concentrated to obtain a hydrolysis condensation product (polymer) propylene glycol monomethyl ether acetate solution. Propylene glycol monoethyl ether was added to adjust the solvent ratio of propylene glycol monomethyl ether acetate / propylene glycol monoethyl ether to 20 / 80, which was 20% by weight in terms of solid residue at 140° C. The obtained polymer corresponded to formula (2-12) and had a weight average molecular weight of Mw 2000 in terms of polystyrene as determined by GPC.
[0200] Synthesis Example 14
[0201] 24.03 g (70 mol%) of tetramethoxysilane, 8.91 g (29 mol%) of methyltrimethoxysilane, 1.05 g of triphenylsulfonium 3-(trihydroxysilyl)propanesulfonate, and 50.98 g of acetone were added to a 300 ml flask, and 15.03 g of 0.01 mol / l hydrochloric acid was added dropwise to the mixed solution while stirring the mixed solution with an electromagnetic stirrer. After the addition, the flask was transferred to an oil bath adjusted to 85°C, and the mixture was reacted under heating and reflux for 240 minutes. Then, the reaction solution was cooled to room temperature, 68.00 g of propylene glycol monomethyl ether acetate was added to the reaction solution, and methanol, acetone, water, and hydrochloric acid as reaction by-products were removed by reduced pressure distillation, and the mixture was concentrated to obtain a hydrolysis condensation product (polymer) propylene glycol monomethyl ether acetate solution. Propylene glycol monoethyl ether was added to adjust the solvent ratio of propylene glycol monomethyl ether acetate / propylene glycol monoethyl ether to 20 / 80, which was 20% by weight in terms of solid residue at 140° C. The obtained polymer corresponded to formula (2-13) and had a weight average molecular weight of Mw 2000 in terms of polystyrene as determined by GPC.
[0202] (Adjustment of Si-containing resist underlayer film)
[0203] The silicon-containing polymer obtained in the above synthesis example, an acid, a curing catalyst, a sulfonate ion containing a hydrocarbon group and Ionic salts, solvents, and water were mixed in the ratios shown in Table 1 and filtered through a 0.1 μm fluororesin filter to prepare solutions of resist underlayer film forming compositions. The polymer addition ratios in Table 1 do not indicate the addition amount of the polymer solution but indicate the addition amount of the polymer itself.
[0204] As a sulfonate ion containing a hydrocarbon group As salts of ions, triphenylsulfonium camphorsulfonate (TPSCS), triphenylsulfonium p-toluenesulfonate (TPSPTS), triphenylsulfonium methanesulfonate (TPSMS), triphenylsulfonium trifluoromethanesulfonate (TPSTf), benzyltriethylammonium camphorsulfonate (BTEACS), benzyltriethylammonium p-toluenesulfonate (BTEAPTS), benzyltriethylammonium methanesulfonate (BTEAMS), benzyltriethylammonium trifluoromethanesulfonate (BTEATf), trihydroxyphenylsulfonium camphorsulfonate THPSCS, and triphenylsulfonium adamantanecarbonyloxy-1,1-difluoroethane-1-sulfonate TPSAdS were used.
[0205] In Table 1, maleic acid is abbreviated as MA, benzyltriethylammonium chloride is abbreviated as BTEAC, triphenylsulfonium chloride is abbreviated as TPSCl, monotriphenylsulfonium maleate is abbreviated as TPSMA, triphenylsulfonium nitrate is abbreviated as TPSNO3, sodium camphorsulfonic acid salt is abbreviated as NaCS, propylene glycol monomethyl ether acetate is abbreviated as PGMEA, propylene glycol monoethyl ether is abbreviated as PGEE, and propylene glycol monomethyl ether is abbreviated as PGME. Ultrapure water was used for water. Each addition amount is expressed in parts by mass.
[0206] 〔Table 1〕
[0207] Table 1
[0208]
[0209] Table 1 (continued)
[0210]
[0211] (Adjustment of organic resist lower layer film)
[0212] In a 100 mL four-necked flask under nitrogen, carbazole (6.69 g, 0.040 mol, manufactured by Tokyo Chemical Industry Co., Ltd.), 9-fluorenone (7.28 g, 0.040 mol, manufactured by Tokyo Chemical Industry Co., Ltd.), p-toluenesulfonic acid monohydrate (0.76 g, 0.0040 mol, manufactured by Tokyo Chemical Industry Co., Ltd.), 1,4-dihydro-1,4-dione (0.76 g, 0.0040 mol, manufactured by Tokyo Chemical Industry Co., Ltd.) were added. 6.69 g of oxane (manufactured by Kanto Chemical Co., Ltd.) was added, stirred, heated to 100°C, dissolved, and polymerization was initiated. After 24 hours, the mixture was cooled to 60°C, and then chloroform (34 g, manufactured by Kanto Chemical Co., Ltd.) was added for dilution, and reprecipitated in methanol (168 g, manufactured by Kanto Chemical Co., Ltd.). The obtained precipitate was filtered and dried at 80°C for 24 hours using a reduced pressure dryer to obtain 9.37 g of the target polymer (Formula (3-1), hereinafter abbreviated as PCzFL).
[0213]
[0214] PCzFL 1 The results of H-NMR measurement are as follows.
[0215] 1 H-NMR (400MHz, DMSO-d6): δ7.03-7.55 (br, 12H), δ7.61-8.10 (br, 4H), δ11.18 (br, 1H)
[0216] The weight average molecular weight Mw of PCzFL measured by GPC in terms of polystyrene was 2,800, and the polydispersity Mw / Mn was 1.77.
[0217] To 20 g of the obtained resin, 3.0 g of tetramethoxymethyl glycoluril (Mitsui Science Co., Ltd., trade name: Pawdalen 1174) as a crosslinking agent and pyridinium p-toluenesulfonate as a catalyst were added. 0.30 g of salt and 0.06 g of Megaphage R-30 (manufactured by Dainippon Inki Chemical Co., Ltd., trade name) as a surfactant were mixed and dissolved in 88 g of propylene glycol monomethyl ether acetate to prepare a solution. Then, the mixture was filtered using a polyethylene microfilter with a pore size of 0.10 μm, and then filtered using a polyethylene microfilter with a pore size of 0.05 μm to prepare a solution of a composition for forming an organic resist underlayer film used in a photolithography process using a multilayer film.
[0218] (Optical constants measurement)
[0219] The compositions for forming resist underlayer films containing Si prepared in Examples 1 to 23 and Comparative Examples 1 to 5 were coated on silicon wafers using a spin coater. The films were heated at 200° C. for 1 minute on a hot plate to form resist underlayer films containing Si (film thickness 0.05 μm). Then, the refractive index (n value) and optical absorption coefficient (k value, also called attenuation coefficient) of these resist underlayer films were measured at a wavelength of 193 nm using a spectroscopic ellipsometer (manufactured by JA Woollam, VUV-VASEVU-302).
[0220] (Determination of dry etching rate)
[0221] The etcher and etching gas used for the measurement of the dry etching rate were as follows.
[0222] ES401 (manufactured by Japan's Sasuke Technology Co., Ltd.): CF4
[0223] RIE-10NR (manufactured by SAMU): O2
[0224] A solution of a resist underlayer film forming composition containing Si prepared by Examples 1 to 23 and Comparative Examples 1 to 5 was applied to a silicon wafer using a spin coater. The solution was heated at 240°C on a hot plate for 1 minute to form resist underlayer films containing Si (film thickness 0.08 μm (for measuring the etching rate using CF4 gas) and 0.05 μm (for measuring the etching rate using O2 gas). In addition, a coating film (film thickness 0.20 μm) was formed on a silicon wafer using a spin coater. O2 gas was used as an etching gas to measure the dry etching rate, and a comparison of the dry etching rates of the resist underlayer films containing Si in Examples 1 to 19 and Comparative Examples 1 to 5 was performed.
[0225] (Resist Pattern Formation Evaluation)
[0226] The composition for forming an organic lower layer film (layer A) containing PCzFL obtained above was applied to a silicon wafer and baked on a hot plate at 240°C for 60 seconds to obtain an organic lower layer film (layer A) with a film thickness of 200 nm. The composition for forming an anti-etching lower layer film (layer B) containing Si obtained in Examples 1 to 6 and Comparative Examples 1 to 4 was applied thereon and baked on a hot plate at 240°C for 45 seconds to obtain an anti-etching lower layer film (layer B) containing Si. The film thickness of the anti-etching lower layer film (layer B) containing Si was 45 nm.
[0227] A commercially available photoresist solution (JSR (co., Ltd., trade name AR2772) was applied thereon using a spin coater, and baked on a hot plate at 110°C for 60 seconds to form a photoresist film (C layer) with a thickness of 120 nm. The pattern formation of the resist was performed using an ArF exposure machine S-307E (wavelength 193nm, NA, σ: 0.85, 0.93 / 0.85 (Dipole) immersion liquid: water) manufactured by NIKON. After development, the target was exposed through a mask set to form a line width of the photoresist and a so-called line and space (dense line) with a width of 0.065μm between the lines.
[0228] Then, it was baked on a hot plate at 110°C for 60 seconds, cooled, and developed with a 2.38 mass % tetramethylammonium hydroxide aqueous solution (developer) using a 60 second single pulse process. The lower shape of the resist pattern after photolithography was set as a straight line when the line was rectangular, and the fat at the bottom of the line was set as lateral etching (footing).
[0229] Table 2 shows the refractive index n at a wavelength of 193 nm, the optical absorption coefficient k at a wavelength of 193 nm, the etching rate (etching speed: nm / minute) when using fluorine-based gas (CF4 gas), and the resistance to oxygen-based gas (O2 gas). The resistance to oxygen-based gas (O2 gas) is expressed as the etching rate ratio of (resist lower layer film of the present invention) / (organic lower layer film).
[0230] 〔Table 2〕
[0231] Table 2
[0232]
[0233] Table 3 shows the 65 nm line and space after lithography evaluation, and the optimal exposure at this time is reduced by 3 mJ / cm 2 And the observation results of the lower shape of the pattern when the exposure focus was reduced by 0.7 μm.
[0234] 〔Table 3〕
[0235] Table 3
[0236]
[0237] In Table 3, straight line means a rectangular and good pattern shape, lateral etching means that there is expansion in the lower part of the pattern, which is not preferable, and undercut means that there is etching in the lower part of the pattern, which is not preferable.
[0238] [Formation of resist pattern using EUV exposure]
[0239] The composition for forming the organic underlayer film (layer A) was coated on a silicon wafer and baked on a hot plate at 215°C for 60 seconds to obtain an organic underlayer film (layer A) with a thickness of 90 nm. The resist underlayer film forming composition solution prepared by Examples 1 to 15, Examples 20 to 23, and Comparative Examples 1, 4, and 5 of the present invention was spin-coated thereon and heated at 215°C for 1 minute to form a resist underlayer film (B) layer (25 nm). On the hard mask, an EUV resist solution (methacrylate resin resist) was spin-coated and heated to form an EUV resist layer (C) layer, and an EUV exposure device (MicroExposureTool, MET for short) was used to expose the film under the conditions of NA = 0.30, σ = 0.36 / 0.68 Quadropole. After exposure, PEB was performed, cooled to room temperature on a cooling plate, and developed and rinsed to form a resist pattern. The evaluation was conducted on whether or not 26 nm lines and spaces could be formed and the pattern shape observed from the pattern cross section.
[0240] In Table 4, (Good) indicates a state in which the shape between the undercuts is etched laterally and there is no significant residue in the gap, (Collapse) indicates an unpreferable state in which the resist pattern peels off and collapses, and (Bridge) indicates an unpreferable state in which the upper or lower parts of the resist pattern contact each other.
[0241] 〔Table 4〕
[0242] Table 4
[0243] #imgpt92#
[0244] Industrial Availability
[0245] The thin film forming composition of the present invention can be used for a resist underlayer film forming composition such as a photoresist, a resist underlayer film forming composition such as an EUV resist, a EUV resist upper layer film forming composition, a reverse material forming composition, and the like.
Claims
1. Hydrolyzable organosilane, its hydrolyzate or its hydrolysis condensate, and sulfonate ion and Use of ionic salts for preparing compositions for forming resist underlayer films for EUV lithography, The resist underlayer film-forming composition for EUV lithography comprises the hydrolyzable organosilane, its hydrolyzate or its hydrolysis-condensation product, the sulfonate ion and The present invention is composed of a salt of an ion, a solvent, and, as required, an acid, water, an alcohol, a curing catalyst, an acid generator, a light absorbing compound, and a surfactant as optional components. The sulfonate ion is selected from the following formula: Said The ion is a sulfonium ion or an ammonium ion containing at least one organic group having an aromatic ring, The hydrolyzable organosilane is composed of at least one organosilicon compound selected from formula (1) and formula (2), R 1 a Si(R 2 ) 4-a formula(1) In formula (1), R 1 represents an alkyl group, an aryl group, an aralkyl group, a halogenated alkyl group, a halogenated aryl group, a halogenated aralkyl group or an alkenyl group, or is a glycidoxymethyl group, a glycidoxyethyl group, a glycidoxypropyl group, a glycidoxybutyl group, an epoxycyclohexyl group, an acryloylmethyl group, an acryloylethyl group, an acryloylpropyl group, a methacryloylmethyl group, a methacryloylethyl group, a methacryloylpropyl group, an ethylmercapto group, a butylmercapto group, a hexylmercapto group, an octylmercapto group, an aryl group substituted with an alkoxy group, an aryl group substituted with an acyloxy group, a cyanurate alkylene group, a hydroxyalkyl group, a hydroxyalkylene group, a cyclic amino group, a cyclic aminoalkylene group, a cyanoethyl group, a cyanopropyl group or a combination thereof, and R 1 Combined with silicon atoms through Si-C bonds, R 2 represents an alkoxy group, an acyloxy group or a halogen group, a represents an integer of 0 to 3, 〔R 3 c Si(R 4 ) 3-c 〕2Y b Formula (2) In formula (2), R 3 represents an alkyl group, R 4 represents an alkoxy group, an acyloxy group or a halogen group, Y represents an alkylene group or an arylene group, b represents an integer of 0 or 1, and c represents an integer of 0 or 1. 2 . The use according to claim 1 , wherein the resist underlayer film-forming composition for EUV lithography comprises a hydrolysis-condensation product of the compound represented by the formula (1) in the form of a polymer.
3. Hydrolyzable organosilane, its hydrolyzate or its hydrolysis condensate, and sulfonate ion and Use of ionic salts for manufacturing resist underlayer films for EUV lithography, The hydrolyzable organosilane, its hydrolyzate or its hydrolysis-condensation product, the sulfonate ion and A resist underlayer film forming composition for EUV lithography, which comprises a salt of an ionic species, a solvent, and, as required, an acid, water, an alcohol, a curing catalyst, an acid generator, a light absorbing compound, and a surfactant as optional components, is applied on a semiconductor substrate and baked to obtain a resist underlayer film for EUV lithography. The sulfonate ion is selected from the following formula: Said The ion is a sulfonium ion or an ammonium ion containing at least one organic group having an aromatic ring, The hydrolyzable organosilane is composed of at least one organosilicon compound selected from formula (1) and formula (2), R 1 a Si(R 2 ) 4-a formula(1) In formula (1), R 1 represents an alkyl group, an aryl group, an aralkyl group, a halogenated alkyl group, a halogenated aryl group, a halogenated aralkyl group or an alkenyl group, or is a glycidoxymethyl group, a glycidoxyethyl group, a glycidoxypropyl group, a glycidoxybutyl group, an epoxycyclohexyl group, an acryloylmethyl group, an acryloylethyl group, an acryloylpropyl group, a methacryloylmethyl group, a methacryloylethyl group, a methacryloylpropyl group, an ethylmercapto group, a butylmercapto group, a hexylmercapto group, an octylmercapto group, an aryl group substituted with an alkoxy group, an aryl group substituted with an acyloxy group, a cyanurate alkylene group, a hydroxyalkyl group, a hydroxyalkylene group, a cyclic amino group, a cyclic aminoalkylene group, a cyanoethyl group, a cyanopropyl group or a combination thereof, and R 1 Combined with silicon atoms through Si-C bonds, R 2 represents an alkoxy group, an acyloxy group or a halogen group, a represents an integer of 0 to 3, 〔R 3 c Si(R 4 ) 3-c 〕2Y b Formula (2) In formula (2), R 3 represents an alkyl group, R 4 represents an alkoxy group, an acyloxy group or a halogen group, Y represents an alkylene group or an arylene group, b represents an integer of 0 or 1, and c represents an integer of 0 or 1.
4. A method for manufacturing a semiconductor device, comprising the following steps: a step of coating a composition for forming a resist underlayer film for EUV lithography prepared by the use according to claim 1 or 2 on a semiconductor substrate and baking the composition to form a resist underlayer film; a step of coating the EUV resist composition on the underlayer film to form a resist film; a step of subjecting the resist film to EUV exposure; a step of developing the resist film after exposure to obtain a resist pattern; a step of etching the resist underlayer film using the resist pattern; and a step of processing the semiconductor substrate using the patterned resist film and the resist underlayer film.
5. A method for manufacturing a semiconductor device, comprising the following steps: a step of forming an organic lower layer film on a semiconductor substrate; a step of coating the composition for forming a resist underlayer film for EUV lithography produced by the use according to claim 1 or 2 on the organic lower layer film, and baking the coating to form a resist underlayer film; a step of coating the EUV resist composition on the resist underlayer film to form a resist film; a step of subjecting the resist film to EUV exposure; a step of developing the resist film after exposure to obtain a resist pattern; a step of etching the resist underlayer film using the resist pattern; a step of etching the organic underlayer film using the patterned resist underlayer film; and a step of processing a semiconductor substrate using the patterned organic underlayer film.
Citation Information
Patent Citations
Silicon-containing film-forming composition, silicon-containing film, and pattern forming method
JP2010237667A
Silicon-containing composition having sulfonamide group for forming resist underlayer film